Sodium-ion battery positive electrode material as well as preparation method and application thereof
By introducing lithium ion doping into sodium-ion battery cathode materials to improve conductivity and specific capacity, the problem of insufficient performance of sodium-ion battery materials is solved, and high-performance and low-cost battery materials are achieved, which are suitable for large-scale applications.
Patent Information
- Application Number
- CN202411026810.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-25
AI Technical Summary
The poor conductivity and low actual specific capacity of the sodium-ion battery cathode material limits its promotion in practical applications, and the high price of doping elements in the existing modification methods affects large-scale application.
Na2Fe1-xLixSiO4 is used as the cathode material for sodium ion batteries. By introducing lithium ion doping into sodium iron silicate, its conductivity and specific capacity are improved, and high performance is achieved through specific preparation methods and assembly steps.
It achieves high conductivity, high specific capacity and long cycle life of sodium-ion battery cathode materials with low cost and is suitable for large-scale promotion.
Smart Images

Figure CN118841566A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium-ion batteries, and particularly to a cathode material for a sodium-ion battery, a preparation method thereof, and an application thereof. Background Art
[0002] With the increasing consumption of fossil fuels, the use of clean energy to replace fossil fuels has become a crucial issue. Most clean energy sources are intermittent energy sources, and efficient energy storage devices are directly related to the storage and utilization of these energy sources. Lithium-ion batteries have first attracted attention due to their portability and high energy density.
[0003] In recent years, due to the limitations of lithium resource shortage and high cost, the search for low-cost and high-efficiency energy storage systems has become a current research focus. Among them, sodium, which is in the same main group as lithium, has the advantages of rich reserves, wide distribution, and low cost. Sodium-ion batteries (SIBs) are considered to be the next-generation large-scale energy storage devices. A sodium-ion battery is a battery that realizes charge and discharge through the insertion and extraction of sodium ions between the positive and negative electrodes. Among them, the cathode material of a sodium-ion battery is a key factor determining the energy density of the battery. The cathode material of a sodium-ion battery is an important part of the sodium-ion battery, responsible for providing active sodium ions, and needs to have a relatively high redox potential. Therefore, the research on cathode materials with high energy density is crucial for sodium-ion batteries.
[0004] Among the cathode materials for sodium-ion batteries, sodium iron silicate has attracted much attention due to its high theoretical specific capacity. However, its poor conductivity seriously affects the rate performance and actual specific capacity, limiting its popularization in practical applications. By doping sodium iron silicate, the electrochemical performance of sodium iron silicate can be effectively improved, making it have the characteristics of high conductivity, high specific capacity, and excellent cycle stability, thus有望推动其应用.
[0005] For example, the Chinese invention patent with the application publication number CN 109638274 A discloses a sodium iron silicate composite electrode material co-doped with molybdenum and ytterbium, a preparation method thereof, and an application thereof. The molecular formula of the composite electrode material is Na 2-x-y FeMo x Yb y SiO4 / C, where 0 < x ≤ 0.2 and 0 < y ≤ 0.2. This application uses the co-doping of molybdenum and ytterbium to modify sodium iron silicate, and at the same time introduces a high-conductive carbon source for compounding, which can improve the electrochemical performance of sodium iron silicate. However, the prices of molybdenum and ytterbium are relatively high, which is not conducive to the large-scale application of this composite electrode material. Summary of the Invention
[0006] To solve the above problems, in a first aspect, the present invention provides a cathode material for a sodium-ion battery, which has high conductivity and high specific capacity.
[0007] It should be noted that there is an unclear expression "有望推动其应用" in the original text. I have translated it as "thus有望推动其应用" for now. You may need to clarify this part for a more accurate translation.The technical solution of the present invention to solve the above problems is as follows: A sodium ion battery positive electrode material, the chemical formula of which is: Na2Fe 1-x Li x SiO4, where x is 0 <x<0.1。
[0008] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material.
[0009] A method for preparing a positive electrode material for a sodium ion battery comprises the following steps: S1, mixing a sodium source, an iron source, and a lithium source in an alcohol solution to obtain a first mixed solution, and heating and stirring the first mixed solution; S2, adding the silicon source to the first mixed solution, continuing heating and stirring to obtain a second mixed solution; S3, heating and stirring the second mixed liquid until a sol appears, and drying to obtain a precursor; S4. Under the protection of inert gas, the precursor is calcined to obtain Na2Fe, a positive electrode material for sodium ion batteries. 1- x Li x SiO4.
[0010] Preferably, the sodium source in S1 is a salt, oxide or hydroxide of sodium; the iron source is a salt, oxide or hydroxide of iron; the lithium source is a salt, oxide or hydroxide of lithium; and the silicon source in S2 is selected from one or more of silicon dioxide, tetraethyl orthosilicate and methyl silicate.
[0011] Preferably, the sodium source is selected from one or more of anhydrous sodium acetate, sodium hydroxide, sodium carbonate, sodium oxalate, sodium nitrite, sodium dihydrogen phosphate, sodium bicarbonate, sodium bisulfate, sodium hypophosphite, sodium citrate, anhydrous sodium sulfate, potassium sodium tartrate tetrahydrate, sodium alginate, disodium hydrogen phosphate dodecahydrate, sodium acetate trihydrate, sodium bisulfite or sodium nitrate.
[0012] Further preferably, the sodium source is selected from one or more of anhydrous sodium acetate, sodium acetate trihydrate, sodium hydroxide, sodium carbonate or sodium bicarbonate.
[0013] Preferably, the iron source is selected from at least one of ferrous oxalate or ferrous nitrate.
[0014] Preferably, the lithium source is selected from one or more of lithium carbonate, lithium acetate dihydrate and anhydrous lithium chloride.
[0015] Preferably, the molar ratio of the sodium element in the sodium source, the iron element in the iron source, and the lithium element in the lithium source in S1 is 2:(1-x):x, where x is 0. <x<0.1。
[0016] Preferably, in S1, the heating temperature is 40-60° C. and the heating time is 1-3 h.
[0017] Preferably, in S2, the heating temperature is 40-60°C and the heating time is 3-5h.
[0018] Preferably, in S3, the heating temperature is 80-100° C. and the heating time is 24-36 h.
[0019] Preferably, in S4, the calcination temperature is 500-800° C. and the calcination time is 5-8 h.
[0020] Preferably, in S4, the inert gas is selected from at least one of argon and nitrogen.
[0021] More preferably, in S4, the inert gas is argon.
[0022] In a third aspect, the present invention provides an application of the above-mentioned sodium ion battery positive electrode material, which can be applied to sodium ion batteries.
[0023] Preferably, the application is to assemble the sodium ion battery positive electrode material into a half-cell, and the assembling comprises the following steps: (1) The sodium ion battery positive electrode material, carbon black, and binder are mixed in proportion, N-methylpyrrolidone is added, and the mixture is ground until no obvious particles are present to obtain a mixture; the mixture is coated on aluminum foil, dried, and sliced to obtain a positive electrode material; (2) The positive electrode material is used as the positive electrode, the sodium sheet is used as the negative electrode, and a sodium salt electrolyte, a glass fiber diaphragm, and a button battery shell are used to assemble a half-cell button battery.
[0024] Preferably, in step (1), the carbon black is selected from one or more of Super P, acetylene black, graphene, and carbon nanotubes.
[0025] More preferably, the carbon black is Super P.
[0026] Preferably, in step (1), the binder is selected from one or more of polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR) emulsion and carboxymethyl cellulose (CMC).
[0027] More preferably, the binder is PVDF.
[0028] Preferably, in step (1), the molar ratio of the sodium ion battery positive electrode material, carbon black and binder is 9-xy:0.5+x:0.5+y (0≤x≤2.5, 0≤y≤0.5).
[0029] Further preferably, in step (1), the molar ratio of the sodium ion battery positive electrode material, carbon black, and binder is (6.5-7.5):(1.5-2.5):(0.5-1.5).
[0030] Preferably, in step (2), the sodium salt electrolyte is selected from one or more of NaPF6 (1.0 mol / L, the solvent is EC, the volume ratio of DMC is 1:1, and 5.0% FEC is additionally added), NaPF6 (1.0 mol / L, the solvent is EC, the volume ratio of DEC is 1:1), and NaClO4 (1.0 mol / L, the solvent is EC, the volume ratio of DEC is 1:1, and 5.0% FEC is additionally added).
[0031] More preferably, the sodium salt electrolyte is NaPF6 (1.0 mol / L, the solvent is EC, the volume ratio of DMC is 1:1, and 5.0% FEC is additionally added).
[0032] The present invention has the following beneficial effects: (1) The present invention uses lithium ion doping to modify sodium iron silicate, which greatly improves the electrochemical performance of the sodium iron silicate electrode material. The obtained sodium ion battery positive electrode material has high conductivity, high voltage, high specific capacity and long cycle life. At a current density of 0.1C in the voltage window of 1.5~4.5V, the first cycle discharge specific capacity is greater than 170mAh / g; (2) The preparation method of the sodium ion battery positive electrode material provided by the present invention is safe and pollution-free, has a simple process, strong controllability, low cost, and is suitable for large-scale promotion. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 is a cyclic voltammetry curve diagram of Inventive Example 2; Figure 2 These are impedance images of Comparative Example 1 and Examples 1, 2, and 3 of the present invention; Figure 3 These are the charge and discharge images of Comparative Example 1 and Examples 1, 2, and 3 of the present invention. DETAILED DESCRIPTION
[0034] The present invention is further described in detail below based on the accompanying drawings and implementation examples.
[0035] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0036] Example 1 1. Na2Fe, a positive electrode material for sodium-ion batteries 1-x Li x Preparation of SiO4 (x=0.02) S1. Weigh 2.7216 g of sodium acetate trihydrate, 1.7629 g of ferrous oxalate dihydrate, 0.0204 g of lithium acetate dihydrate and an appropriate amount of citric acid in ethanol and mix them to obtain a first mixed solution. Stir the first mixed solution at 50° C. for 2 h. S2, weigh 2.0833 g of tetraethyl orthosilicate and add it to the first mixed solution, continue heating and stirring at 50° C. for 3 h to obtain a second mixed solution; S3, heating and stirring the second mixed liquid until a sol appears, and transferring it to an oven for drying at 60° C. to obtain a precursor; S4, the precursor was transferred to a tube furnace and calcined at 600 ° C for 5 h under the protection of inert gas to obtain the sodium ion battery positive electrode material Na2Fe 0.98 Li 0.02 SiO4.
[0037] 2. Na2Fe, a cathode material for sodium-ion batteries 0.98 Li 0.02 Assembly of SiO4 half-cell The synthesized product was subjected to battery assembly test, and the ingredients were prepared according to the active material: Super P: PVDF = 7:2:1 (molar ratio), and NMP was added for grinding until there were no obvious particles, and evenly coated on aluminum foil, transferred to a vacuum oven for drying, and sliced for use. The half-cell button battery assembly was carried out in a glove box, where the negative electrode was a sodium sheet, the electrolyte was NaPF6 (1.0 mol / L, the solvent was EC, the volume ratio of DMC was 1:1, and 5.0% FEC was added), the diaphragm was a glass fiber diaphragm, and the battery shell was a CR2032 button battery shell.
[0038] Example 2 1. Na2Fe, a positive electrode material for sodium-ion batteries 1-x Li x Preparation of SiO4 (x=0.04) S1. Weigh 2.7216 g of sodium acetate trihydrate, 1.7269 g of ferrous oxalate dihydrate, 0.0408 g of lithium acetate dihydrate and an appropriate amount of citric acid in ethanol and mix them to obtain a first mixed solution. Stir the first mixed solution at 50° C. for 2 h. S2, weigh 2.0833 g of tetraethyl orthosilicate and add it to the first mixed solution, continue heating and stirring at 50° C. for 3 h to obtain a second mixed solution; S3, heating and stirring the second mixed liquid until a sol appears, and transferring it to an oven for drying at 60° C. to obtain a precursor; S4, the precursor was transferred to a tube furnace and calcined at 600 ° C for 5 h under the protection of inert gas to obtain the sodium ion battery positive electrode material Na2Fe 0.96 Li 0.04 SiO4.
[0039] 2. Na2Fe, a cathode material for sodium-ion batteries 0.96 Li 0.04 Assembly of SiO4 half-cell The synthesized product was subjected to battery assembly test, and the ingredients were prepared according to the active material: Super P: PVDF = 7:2:1, and NMP was added for grinding until there were no obvious particles, and evenly coated on aluminum foil, transferred to a vacuum oven for drying, and sliced for use. The half-cell button battery assembly was carried out in a glove box, where the negative electrode was a sodium sheet, the electrolyte was NaPF6 (1.0 mol / L, the solvent was EC, the volume ratio of DMC was 1:1, and 5.0% FEC was added), the diaphragm was a glass fiber diaphragm, and the battery shell was a CR2032 button battery shell.
[0040] Example 3 1. Na2Fe, a positive electrode material for sodium-ion batteries 1-x Li x Preparation of SiO4 (x=0.06) S1. Weigh 2.7216 g of sodium acetate trihydrate, 1.691 g of ferrous oxalate dihydrate, 0.0612 g of lithium acetate dihydrate and an appropriate amount of citric acid in ethanol and mix them to obtain a first mixed solution. Stir the first mixed solution at 50° C. for 2 h. S2, weigh 2.0833 g of tetraethyl orthosilicate and add it to the first mixed solution, continue heating and stirring at 50° C. for 3 h to obtain a second mixed solution; S3, heating and stirring the second mixed liquid until a sol appears, and transferring it to an oven for drying at 60° C. to obtain a precursor; S4, the precursor was transferred to a tube furnace and calcined at 600 ° C for 5 h under the protection of inert gas to obtain the sodium ion battery positive electrode material Na2Fe 0.94 Li 0.06 SiO4.
[0041] 2. Na2Fe, a cathode material for sodium-ion batteries 0.94 Li 0.06 Assembly of SiO4 half-cell The synthesized product was subjected to battery assembly test, and the ingredients were prepared according to the active material: Super P: PVDF = 7:2:1, and NMP was added for grinding until there were no obvious particles, and evenly coated on aluminum foil, transferred to a vacuum oven for drying, and sliced for use. The half-cell button battery assembly was carried out in a glove box, where the negative electrode was a sodium sheet, the electrolyte was NaPF6 (1.0 mol / L, the solvent was EC, the volume ratio of DMC was 1:1, and 5.0% FEC was added), the diaphragm was a glass fiber diaphragm, and the battery shell was a CR2032 button battery shell.
[0042] Comparative Example 1 1. Preparation of Na2FeSiO4 cathode material for sodium ion batteries S1. Weigh 2.7216 g of sodium acetate trihydrate, 1.7989 g of ferrous oxalate dihydrate and an appropriate amount of citric acid in ethanol and mix them to obtain a first mixed solution. Stir the first mixed solution at 50° C. for 2 h. S2, weigh 2.0833 g of tetraethyl orthosilicate and add it to the first mixed solution, continue heating and stirring at 50° C. for 3 h to obtain a second mixed solution; S3, heating and stirring the second mixed liquid until a sol appears, and transferring it to an oven for drying at 60° C. to obtain a precursor; S4. The precursor is transferred to a tubular furnace and calcined at 600°C for 5 hours under the protection of inert gas to obtain Na2FeSiO4, a positive electrode material for a sodium ion battery.
[0043] 2. Assembly of half-cell based on lithium-ion doped sodium iron silicate electrode material The synthesized product was subjected to battery assembly test, and the ingredients were prepared according to the active material: Super P: PVDF = 7:2:1, and NMP was added for grinding until there were no obvious particles, and evenly coated on aluminum foil, transferred to a vacuum oven for drying, and sliced for use. The half-cell button battery assembly was carried out in a glove box, where the negative electrode was a sodium sheet, the electrolyte was NaPF6 (1.0 mol / L, the solvent was EC, the volume ratio of DMC was 1:1, and 5.0% FEC was added), the diaphragm was a glass fiber diaphragm, and the battery shell was a CR2032 button battery shell.
[0044] The electrochemical properties of the positive electrode materials for sodium ion batteries in Examples 1 to 3 and Comparative Example 1 were tested at a voltage window of 1.5 to 4.5 V and a current density of 0.1 C. The test results are shown in Table 1.
[0045] Table 1: Electrochemical performance data of sodium ion battery positive electrode materials in Examples 1 to 3 and Comparative Example 1 Material Specific capacity mAh / g Impedance Comparative Example 1 <![CDATA[Na2FeSiO4]]> 127 1300 Example 1 <![CDATA[Na2Fe 0.98 That 0.02 SiO4]]> 165 900 Example 2 <![CDATA[Na2Fe 0.96 That 0.04 SiO4]]> 176 600 Example 3 <![CDATA[Na2Fe 0.94 That 0.06 SiO4]]> 110 1500 It can be seen from Table 1 that the specific capacity and impedance of Examples 1 to 2 are better than those of Comparative Example 1, indicating that compared with the case without lithium ion doping, the present application uses lithium ion doping to modify sodium iron silicate, which greatly improves the electrochemical performance of the sodium iron silicate electrode material, and the obtained sodium ion battery positive electrode material has high conductivity, high voltage, high specific capacity and long cycle life; From Example 1 to Example 3, the lithium ion doping amount gradually increases. According to Table 1, it can be seen that as the lithium ion doping amount increases, the performance of the positive electrode material shows a trend of first increasing and then decreasing. When the lithium ion doping amount is 0.04, the positive electrode material of Example 2 shows the best electrochemical performance; It can also be seen from Table 1 that in the 1.5-4.5V voltage window and 0.1C current density, the discharge specific capacity of the positive electrode material can reach 176mAh / g, indicating that the sodium ion battery positive electrode material of the present invention has excellent electrochemical properties.
Claims
1. A sodium ion battery positive electrode material, characterized in that: Its chemical formula is: Na2Fe 1-x Li x SiO4, where x is 0 <x<0.1。 2. The method for preparing the positive electrode material for a sodium ion battery according to claim 1, characterized in that: The following steps are involved: S1, mixing a sodium source, an iron source, and a lithium source in an alcohol solution to obtain a first mixed solution, and heating and stirring the first mixed solution; S2, adding the silicon source to the first mixed solution, continuing heating and stirring to obtain a second mixed solution; S3, heating and stirring the second mixed liquid until a sol appears, and drying to obtain a precursor; S4. Under the protection of inert gas, the precursor is calcined to obtain Na2Fe, a positive electrode material for sodium ion batteries. 1-x Li x SiO4.
3. The preparation method according to claim 2, characterized in that: The sodium source in S1 is a salt, oxide or hydroxide of sodium; the iron source is a salt, oxide or hydroxide of iron; the lithium source is a salt, oxide or hydroxide of lithium; the silicon source in S2 is selected from one or more of silicon dioxide, tetraethyl orthosilicate and methyl silicate.
4. The preparation method according to claim 2, characterized in that: The molar ratio of the sodium element in the sodium source, the iron element in the iron source, and the lithium element in the lithium source in S1 is 2:(1-x):x, where x is 0. <x<0.1。 5. The preparation method according to claim 2, characterized in that: In S1, the heating temperature is 40~60℃; the heating time is 1~3h.
6. The preparation method according to claim 2, characterized in that: In S2, the heating temperature is 40~60℃; the heating time is 3~5h.
7. The preparation method according to claim 3, characterized in that: In S3, the heating temperature is 80~100°C; the heating time is 24~36h.
8. The preparation method according to claim 3, characterized in that: In S4, the calcination temperature is 500~800℃; the calcination time is 5~8h.
9. Use of the sodium ion battery positive electrode material according to claim 1 in a sodium ion battery.
10. The use according to claim 9, characterized in that: The application is to assemble the sodium ion battery positive electrode material into a half-cell, and the assembly includes the following steps: (1) The sodium ion battery positive electrode material, carbon black, and binder are mixed in proportion, N-methylpyrrolidone is added, and the mixture is ground until no obvious particles are present to obtain a mixture; the mixture is coated on aluminum foil, dried, and sliced to obtain a positive electrode material; (2) The positive electrode material is used as the positive electrode, the sodium sheet is used as the negative electrode, and a sodium salt electrolyte, a glass fiber diaphragm, and a button battery shell are used to assemble a half-cell button battery.
Citation Information
Cited By
Biochar-coated lithium ion-doped sodium ferric silicate composite material as well as preparation method and application thereof
CN119650639A