High-barrier flexible organic solar cell and preparation method thereof
By adopting a double-layer barrier structure in flexible organic solar cells and using high transmittance photoresist or light-converting hydrophilic and hydrophobic material to modify the layer, the problems of barrier layer roughness and bending resistance are solved, and the efficiency and performance of the battery are improved. Stability and extended life.
Patent Information
- Application Number
- CN202410909893.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-11-17
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-25
AI Technical Summary
Flexible organic solar cells have poor stability and short lifespan, mainly because organic semiconductor active materials and electrode materials are susceptible to the influence of water and oxygen in the external environment, resulting in high roughness of the barrier layer, which affects device efficiency and bending resistance.
It adopts a double-layer barrier structure, including a barrier layer and a modification layer. The modification layer is composed of high transmittance photoresist, resin or light-converting hydrophilic and hydrophobic materials, which reduces the roughness of the barrier layer and improves the interface wettability, enhancing the connection between the substrate and the electrode. Bonding strength and improved bending resistance.
It effectively increases the water and oxygen transmittance, improves the efficiency and stability of the battery, reduces the surface roughness, enhances the bending resistance, and extends the service life of the battery.
Smart Images

Figure CN118843333A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cells and relates to a high-barrier flexible organic solar cell and a preparation method thereof. Background Art
[0002] With the rapid development of science and technology, it is accompanied by a large amount of energy consumption and environmental pollution. The use of clean energy is the key to solving this problem in the future. The current clean energy includes solar energy, wind energy and hydropower, but wind power generation and hydropower generation are subject to many geographical and spatial constraints, and the output of electricity cannot well meet the energy needs of today's society. Only solar power generation can be conveniently and widely used in various scenarios. Flexible organic solar cells have the characteristics of low cost, green, high efficiency, softness, colorful translucency, and can be prepared by roll-to-roll large-area printing. It is an ideal photoelectric conversion technology with broad market prospects.
[0003] Compared with inorganic crystalline silicon solar cells, flexible organic solar cells currently have another urgent problem to be solved, in addition to low conversion efficiency, which is poor stability and short life. This is mainly because organic semiconductor active materials and electrode materials are easily affected by water, oxygen, etc. in the external environment. Therefore, flexible organic solar cell devices must be protected by encapsulation layers, barrier layers and other protective layers to prevent water and oxygen from entering the internal system of organic solar cells. However, barrier layers formed in different ways will affect the transmittance, bending resistance, efficiency and other properties of flexible organic solar cells to a certain extent. Therefore, it is key to improve the stability of flexible organic solar cells while ensuring device efficiency.
[0004] In existing flexible solar cells, the stability of the device can be improved by growing or laminating a barrier layer on the substrate to make the device, but at the same time, the roughness of the barrier layer will affect the efficiency of the device, and laminating or in-situ growth will affect the light transmittance of the device to a certain extent, thereby affecting the battery efficiency. Secondly, flexible solar cells have certain requirements for resistance to bending when in use. During the bending process, the barrier film may crack due to uneven lamination stress or insufficient bonding strength of the in-situ grown barrier layer during the bending process, thereby affecting its barrier effect. Summary of the invention
[0005] The main purpose of the present invention is to provide a high-barrier flexible organic solar cell and a preparation method thereof, so as to overcome the shortcomings of the prior art.
[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0007] An embodiment of the present invention provides a high-barrier flexible organic solar cell, which includes a flexible substrate, a barrier layer, a modification layer, a silver nanowire electrode layer, an organic functional layer, a top electrode layer and an encapsulation layer stacked in sequence along a set direction, wherein the material of the modification layer includes at least one of a high-transmittance photoresist, a resin, and a light-converting hydrophilic and hydrophobic material.
[0008] In some embodiments, the modification layer has a thickness of 0.1-10 μm and a light transmittance of 75%-95%.
[0009] In some embodiments, the barrier layer has a thickness of 1-5 μm and a water vapor transmission rate of less than 10 -2 g / m 2 day, oxygen transmission rate is less than 10 -1 cm 3 / (m 2 ·day·0.1MPa), light transmittance is 70%-90%.
[0010] In some embodiments, the material of the barrier layer includes at least one of an inorganic substance and a polymer, wherein the inorganic substance includes any one or a combination of two or more of silicon oxide, aluminum oxide and silicon nitride, and the polymer includes at least one of polyvinylidene chloride, ethylene and vinyl alcohol copolymer.
[0011] The embodiment of the present invention further provides a method for preparing a high-barrier flexible organic solar cell, which comprises:
[0012] forming a barrier layer on a flexible substrate;
[0013] forming a modifying layer on the barrier layer;
[0014] forming a silver nanowire electrode layer on the modified layer;
[0015] forming an organic functional layer on the silver nanowire electrode layer;
[0016] forming a top electrode layer on the organic functional layer;
[0017] And, forming an encapsulation layer on the top electrode layer to obtain the high-barrier flexible organic solar cell.
[0018] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0019] 1) The high-barrier flexible organic solar cell provided by the present invention modifies the barrier layer to achieve a double-layer barrier effect, which can effectively reduce the water and oxygen permeability, improve the barrier property, light transmittance and bending resistance, and reduce the surface roughness, thereby further improving the efficiency and stability of the battery device;
[0020] 2) The modified layer of the present invention can effectively reduce the roughness of the barrier layer and improve the interface wettability, making the silver wire electrode distribution more uniform, which can effectively improve the device efficiency;
[0021] 3) The modified layer of the present invention can enhance the bonding force between the substrate and the electrode, and can also improve the anti-bending performance of the barrier layer itself, thereby improving the anti-bending performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 is a schematic cross-sectional view of a double-layer barrier structure implemented by a barrier layer and a modification layer in a typical embodiment of the present invention;
[0024] Figure 2 is a schematic diagram of the cross-sectional structure of a high-barrier flexible organic solar cell in a typical embodiment of the present invention;
[0025] Figure 3 Schematic diagram of the hydrophilic-hydrophobic conversion of the photoconvertible hydrophilic-hydrophobic material modification layer in a typical embodiment of the present invention;
[0026] Figure 4a-4b is a SEM photograph of the silver nanowire electrode with a PVA modified layer in Example 1 of the present invention;
[0027] Figure 5a-Figure 5b is a SEM photograph of a silver nanowire electrode with a SU-8 photoresist modification layer in Example 2 of the present invention;
[0028] Figure 6a-6b is a SEM photograph of the silver nanowire electrode without a modification layer in Comparative Example 1 of the present invention;
[0029] Figure 7 This is a SEM photograph of the silver nanowire electrode without a barrier layer and a modification layer in Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0030] As mentioned above, in response to the deficiencies in the prior art, the inventors of this case, after long-term research and extensive practice, have provided a structure of a high-barrier flexible organic solar cell and a method for preparing the same, aiming to modify the barrier film so as to improve the barrier properties, light transmittance and bending resistance, while reducing the surface roughness to improve the efficiency and stability of the battery.
[0031] The technical solution, its implementation process and principle will be further explained as follows.
[0032] An aspect of an embodiment of the present invention provides a high-barrier flexible organic solar cell structure comprising a flexible substrate, a barrier layer, a modification layer, a silver nanowire electrode layer, an organic functional layer, a top electrode layer and an encapsulation layer stacked in sequence along a set direction.
[0033] In some preferred embodiments, reference Figure 2 As shown, the structure of the high-barrier flexible organic solar cell is, from bottom to top, a flexible substrate, a barrier layer, a modification layer, a silver nanowire electrode layer, an organic functional layer, a top electrode layer and an encapsulation layer.
[0034] In some embodiments, the thickness of the flexible substrate should be 50-150 μm, and its light transmittance should be 70%-95%.
[0035] Furthermore, the material of the flexible substrate may include any one or a combination of two or more of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polyimide (PI), but is not limited thereto.
[0036] In some embodiments, the thickness of the barrier layer should be 1-5 μm, and the water vapor transmission rate should be less than 10 -2 g / m 2 ·24h, oxygen transmission rate should be less than 10 -1 cm 3 / (m 2 ·24h·0.1MPa), its light transmittance is 70%-90%.
[0037] Furthermore, the material of the barrier layer can be at least one of an inorganic substance, a polymer, etc. Specifically, the inorganic substance can include any one of silicon oxide, aluminum oxide, and silicon nitride, etc., or a combination of two or more thereof, and the polymer can be any one of polyvinylidene chloride, ethylene and vinyl alcohol copolymer, etc., or a combination of two or more thereof. The barrier layer and the modification layer of the present invention can achieve a double-layer barrier effect, as shown in the schematic diagram. Figure 1 , which can effectively reduce the water and oxygen permeability and further improve the stability of the device.
[0038] Furthermore, the barrier layer may be prepared by any one of vacuum thermal evaporation vapor deposition, chemical vapor deposition, anodization deposition, spin coating, solution coating, and electrostatic spray deposition, but is not limited thereto.
[0039] In some embodiments, the thickness of the modification layer should be 0.1-10 μm, and its light transmittance should be 75%-95%.
[0040] In some embodiments, the material of the modification layer can be at least one of a high-transmittance photoresist, a resin, a photoconvertible hydrophilic material, etc. The modification layer of the present invention can effectively reduce the roughness of the barrier layer, improve the interface wettability, make the silver wire electrode distribution more uniform, and effectively improve the device efficiency. In addition, the modification layer can also enhance the bonding force between the substrate and the electrode, and can also improve the anti-bending performance of the barrier layer itself, thereby improving the anti-bending performance of the device.
[0041] Furthermore, the high-transmittance photoresist may include any one or a combination of two or more of high-transmittance photoresists such as SU-8, SUN-2300N, SUN-5400N, etc., and the resin may be any one or a combination of two of polyvinyl alcohol (PVA), epoxy resin, etc.
[0042] In some embodiments, the photoconvertible hydrophilic-hydrophobic material includes a combination of a photosensitive olefin monomer or a photosensitive alkyne monomer and a thiol compound.
[0043] Further, the photoconvertible hydrophilic and hydrophobic material includes any one of photosensitive olefin monomers or photosensitive alkyne monomers such as (2-nitro-1,4-phenyl)bis(methylene) diacrylate (acrylate-NBE), (2-nitro-1,4-phenyl)bis(methylene) 1-hexynoate (hexyl-NBE), 1,4-phenylbis(methylene) di(but-3-yn-1-yl) bis(carbonate) (butyl-NBC), and any one of thiol compounds such as hexane-1,6-dithiol (HDT), 2-ethyl-2-(((3-mercaptopropionyl)oxy)methyl)propane-1,3-diylbis(3-mercaptopropionate) (TMPMP), 2,2-bis(((3-mercaptopropionyl)oxy)methyl)propane-1,3-diylbis(3-mercaptopropionate) (PETMP), but is not limited thereto.
[0044] Furthermore, the photosensitive olefin monomer or photosensitive alkyne monomer and thiol compound in the photoconvertible hydrophilic-hydrophobic material can undergo polymerization reaction under LED light with a wavelength greater than 400 nm, thereby realizing the conversion from hydrophilic to hydrophobic. When the modified layer is in a hydrophilic state, it is beneficial to the uniform preparation of the silver wire electrode. When the modified layer is hydrophobic, it is beneficial to achieve further water vapor barrier effect. See the schematic diagram. Figure 3 .
[0045] In some embodiments, the thickness of the silver nanowire electrode layer should be 60-120 nm, the square resistance should be 10-30 Ω / sq, and the optical transmittance should be 70%-90%.
[0046] In some embodiments, the thickness of the organic functional layer should be 100-250 nm.
[0047] In some embodiments, the organic functional layer includes an electron transport layer, an active layer, and a hole transport layer sequentially arranged along a set direction.
[0048] In some more preferred embodiments, the organic functional layer includes an electron transport layer / active layer / hole transport layer structure, and the electron transport layer is close to the silver nanowire electrode layer, that is, from another perspective, the structure of the organic functional layer from bottom to top is electron transport layer / active layer / hole transport layer. Among them, in the electron transport layer / active layer / hole transport layer structure, the material of the electron transport layer can include any one or a combination of two oxides such as zinc oxide and titanium oxide; the material of the hole transport layer can include any one or a combination of two or more oxides such as molybdenum oxide, nickel oxide, tungsten oxide, but is not limited thereto.
[0049] In some more preferred embodiments, the organic functional layer includes a hole transport layer / active layer / electron transport layer structure, and the hole transport layer is close to the silver nanowire electrode layer, that is, from another perspective, the structure of the organic functional layer is hole transport layer / active layer / electron transport layer from bottom to top. Among them, in the hole transport layer / active layer / electron transport layer structure, the material of the hole transport layer can include any one or a combination of two or more of PEDOT:PSS, graphene oxide, transition metal oxides, etc.; the material of the electron transport layer can include any one or a combination of two or more of PFN-Br, PNDIT-F3N, PDINN, etc., but is not limited thereto.
[0050] In some embodiments, in the organic functional layer, the material of the active layer is a binary or multi-component system consisting of a donor material, a fullerene acceptor and / or a non-fullerene acceptor.
[0051] Furthermore, the donor material includes any one or a combination of two or more of PM6, PTB7-Th, PBDB-T, etc., but is not limited thereto.
[0052] Furthermore, the fullerene acceptor comprises PC 61 BM, the non-fullerene acceptor includes any one or a combination of two or more of L8-BO, BTP-BO-4Cl, Y6, etc., but is not limited thereto.
[0053] In some more preferred embodiments, the active layer is composed of at least one of the donor materials such as PM6, PTB7-Th, PBDB-T and PC 61 Fullerene acceptors such as BM and / or at least one of non-fullerene acceptors such as L8-BO, BTP-BO-4Cl, Y6, etc. form a binary or multi-component system.
[0054] In some embodiments, the thickness of the top electrode layer should be 100-200 nm, and the material of the top electrode layer may include any one or a combination of two or more of Al, Ag, and Au, but is not limited thereto.
[0055] In some embodiments, the thickness of the encapsulation layer should be 10-300 μm, and the material of the encapsulation layer may include any one or a combination of two or more of epoxy resin, acrylic resin, synthetic rubber, etc., but is not limited thereto.
[0056] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned high-barrier flexible organic solar cell, which comprises:
[0057] forming a barrier layer on a flexible substrate;
[0058] forming a modification layer on the barrier layer;
[0059] forming a silver nanowire electrode layer on the modified layer;
[0060] forming an organic functional layer on the silver nanowire electrode layer;
[0061] forming a top electrode layer on the organic functional layer;
[0062] And, forming an encapsulation layer on the top electrode layer to obtain the high-barrier flexible organic solar cell.
[0063] In some more specific embodiments, the method for preparing the barrier layer includes: applying the barrier layer material to the flexible substrate by any of vacuum thermal evaporation vapor deposition, chemical vapor deposition, anodization deposition, spin coating, coating, electrostatic spray deposition, lamination, etc., to prepare the barrier layer.
[0064] In some more specific embodiments, when the modification material is a resin, the method for preparing the modification layer includes: applying the resin to the barrier layer by at least one of spin coating and coating, and then annealing at 100-120° C. for 20-30 minutes to form the modification layer.
[0065] In some other more specific embodiments, when the modification material is a high-transmittance photoresist, the method for preparing the modification layer comprises: applying the high-transmittance photoresist to the barrier layer by at least one of spin coating and coating, then baking at 95-110° C. for 1-3 min, and then heating at 60-200 mJ / cm 2 Expose, or bake at 95-110° C. for 1-3 minutes to prepare the modified layer.
[0066] In some other more specific embodiments, when the modifying material is a photo-convertible hydrophilic-hydrophobic material, the method for preparing the modifying layer includes: applying the photo-convertible hydrophilic-hydrophobic material to the barrier layer by at least one of spin coating and coating in a state avoiding white light, and then drying it to form a film at room temperature to prepare the modifying layer.
[0067] Furthermore, the preparation method further comprises: forming a silver nanowire electrode layer on the modified layer by at least one of gravure spin coating, coating and the like.
[0068] Furthermore, the preparation method further comprises: forming a top electrode layer on the organic functional layer by at least one of vacuum evaporation, thermal evaporation vapor deposition, transfer method, magnetron sputtering, etc.
[0069] Furthermore, the preparation method further comprises: forming a packaging layer on the top electrode layer by at least one of spin coating, coating or lamination.
[0070] The preparation processes of the barrier layer, the silver nanowire electrode layer, the top electrode layer and the encapsulation layer all adopt process operations and parameter conditions well known to technicians in the industry.
[0071] Among them, in some more specific embodiments, a method for preparing a high-barrier flexible organic solar cell of the present invention comprises the following steps:
[0072] Step 1: preparing a flexible substrate as a solar cell substrate;
[0073] Step 2: Spin coating, coating, depositing or laminating a barrier layer on the substrate;
[0074] Step 3: Spin coating or coating the modifying layer on the barrier layer;
[0075] Step 4: gravure printing a silver nanowire electrode layer on the modified layer of the barrier film;
[0076] Step 5: preparing an organic functional layer on the silver nanowire electrode layer;
[0077] Step 6: Vacuum evaporating a top electrode layer on the organic functional layer;
[0078] Step 7: Spin-coat, apply or laminate the encapsulation layer on the top electrode layer.
[0079] In order to more clearly explain the technical features, objectives and beneficial effects of the present invention, the technical solution of the present invention will now be explained in detail. In the following description, many specific details are explained to facilitate a full understanding of the present invention, but the present invention can also be implemented in other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention, so the present invention is not limited to the specific embodiments disclosed below. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0080] Unless otherwise specified, the raw materials and reagents in the examples of this application were purchased through commercial channels.
[0081] Example 1
[0082] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, 125 μm thick PET, 3 μm thick polyvinylidene chloride, 100 nm thick PVA layer, 90 nm thick silver nanowire electrode layer, 30 nm thick ZnO layer, 100 nm thick PM6:L8-BO layer, 15 nm thick MoOx layer, 150 nm thick Al electrode layer and 10 μm thick tetramethyl biphenol type epoxy resin encapsulation layer.
[0083] The preparation method of the high-barrier flexible organic solar cell is as follows:
[0084] Step 1: Prepare a 125 μm thick PET substrate as a solar cell substrate, spin-coat about 3 μm thick polyvinylidene chloride on the substrate, and anneal at 100 ° C for 30 minutes;
[0085] Step 2: Spin-coat a PVA layer with a thickness of about 100 nm as a modification layer on the barrier layer prepared in step 1, and anneal at 120°C for 20 min;
[0086] Step 3: Gravure print a 90nm thick silver nanowire electrode layer on the modified layer prepared in step 2, with a square resistance of about 20Ω / sq. The morphology of the electrode can be found in Figure 4a-4b As shown;
[0087] Step 4: Spin-coat a 30nm thick ZnO layer on the silver nanowire electrode layer prepared in step 3 and anneal at 130℃ for 10min
[0088] Step 5: Spin-coat a 100 nm thick active layer PM6:L8-BO chloroform solution on the ZnO layer prepared in step 4 and anneal at 85°C for 5 min;
[0089] Step 6: Vacuum thermal evaporation is used to deposit a 15 nm thick MoOx layer on the active layer prepared in step 5;
[0090] Step 7: Deposit a 150 nm thick Al electrode layer on the MoOx layer prepared in step 6 by vacuum thermal evaporation deposition;
[0091] Step 8: Spin-coat a 10 μm thick tetramethyl biphenol epoxy resin encapsulation layer on the Al electrode layer prepared in step 7, and cure at 150° C. for 30 min to obtain the high-barrier flexible organic solar cell.
[0092] Example 2
[0093] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, a 50 μm thick PI, a 2 μm thick aluminum oxide, a 3 μm thick SU-8 photoresist layer, a 60 nm thick silver nanowire electrode layer, a 40 nm thick ZnO layer, a 100 nm thick PBDB-T:Y6 layer, a 20 nm thick MoOx layer, a 200 nm thick Al electrode layer and a 50 μm thick thermosetting acrylic resin encapsulation layer.
[0094] The preparation method of the high-barrier flexible organic solar cell is as follows:
[0095] Step 1: Prepare a 50 μm thick PI substrate as a solar cell substrate, and thermally deposit about 2 μm thick aluminum oxide on the substrate;
[0096] Step 2: Spin-coat a 3 μm thick SU-8 photoresist as a modification layer on the barrier layer prepared in step 1 and bake at 95 °C for 2 min, 100 mJ / cm 2 After exposure, bake at 95°C for 3 minutes;
[0097] Step 3: Gravure print a 60nm thick silver nanowire electrode layer on the modified layer prepared in step 2. The square resistance is about 30Ω / sq. The morphology of the electrode can be found in Figure 5a-Figure 5b As shown;
[0098] Step 4: Spin-coat a ZnO layer with a thickness of about 40 nm on the silver nanowire electrode layer prepared in step 3, and anneal at 130°C for 10 min;
[0099] Step 5: Spin-coat a 100 nm thick active layer of PBDB-T:Y6 chloroform solution on the ZnO layer prepared in step 4 and anneal at 100 °C for 10 min;
[0100] Step 6: Vacuum thermal evaporation is used to deposit a 20 nm thick MoOx layer on the active layer prepared in step 5;
[0101] Step 7: Vacuum thermal evaporation is used to deposit a 200 nm thick Al electrode layer on the MoOx layer prepared in step 6;
[0102] Step 8: A 50 μm thick thermosetting acrylic resin encapsulation layer is scraped onto the Al electrode layer prepared in step 7, and cured at 120° C. for 10 min to obtain the high-barrier flexible organic solar cell.
[0103] Example 3
[0104] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, 100 μm thick PEN, 1 μm thick silicon oxide, 8 μm thick SUN-2300N photoresist layer, 120 nm thick silver nanowire electrode layer, 30 nm thick PEDOT:PSS layer, 50 nm thick PM6:L8-BO layer, 20 nm thick PDINN layer, 100 nm thick Ag electrode layer and 300 μm thick butyl rubber encapsulation layer.
[0105] The preparation method of the high-barrier flexible organic solar cell is as follows;
[0106] Step 1: Prepare a 100 μm thick PEN substrate as a solar cell substrate, and thermally deposit about 1 μm thick aluminum oxide on the substrate;
[0107] Step 2: Spin-coat about 8 μm thick SUN-2300N photoresist as a modification layer on the barrier layer prepared in step 1 and bake at 110°C for 3 min, 100 mJ / cm 2 exposure;
[0108] Step 3: Gravure print a 120nm thick silver nanowire electrode layer on the modified layer prepared in step 2, with a square resistance of about 10Ω / sq;
[0109] Step 4: Spin-coat a 30 nm thick PEDOT:PSS on the silver nanowire electrode layer prepared in step 3, and anneal at 150°C for 20 min;
[0110] Step 5: Spin-coat a 50 nm thick active layer of PM6:L8-BO chloroform solution on the PEDOT:PSS layer prepared in step 4 and anneal at 85 °C for 5 min;
[0111] Step 6: Spin-coat 20 nm thick PDINN on the active layer prepared in step 5;
[0112] Step 7: Vacuum thermal evaporation is used to deposit a 100 nm thick Ag electrode layer on the PDINN layer prepared in step 6;
[0113] Step 8: A 300 μm thick butyl rubber encapsulation layer is applied to the Ag electrode layer prepared in step 7 to obtain the high-barrier flexible organic solar cell.
[0114] Example 4
[0115] The difference between this embodiment and embodiment 3 is that the SUN-2300N photoresist modification layer is baked at 110°C for 3 minutes and then heated at 200mJ / cm 2 exposure.
[0116] Example 5
[0117] The difference between this embodiment and embodiment 3 is that the SUN-2300N photoresist modification layer is baked at 110°C for 2 minutes, 60mJ / cm 2 Expose and bake at 100℃ for 2min.
[0118] Example 6
[0119] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, 150 μm thick PET, 5 μm thick silicon nitride, 10 μm thick SUN-5400N photoresist layer, 100 nm thick silver nanowire electrode layer, 50 nm thick ZnO layer, 50 nm thick PTB7-Th:BTP-BO-4C1 layer, 100 nm thick tungsten oxide layer, 100 nm thick Au electrode layer and 100 μm thick fluororubber encapsulation layer.
[0120] The preparation method of the high-barrier flexible organic solar cell is as follows:
[0121] Step 1: Prepare a 150 μm thick PET substrate as a solar cell substrate, and thermally deposit about 5 μm thick silicon nitride on the substrate;
[0122] Step 2: Spin-coat a 100nm thick SUN-5400N layer as a modification layer on the barrier layer prepared in step 1, and bake at 110℃ for 1min, 60mJ / cm 2 After exposure, bake at 110℃ for 1min;
[0123] Step 3: Gravure print a 100 nm thick silver nanowire electrode layer on the modified layer prepared in step 2, with a square resistance of about 15Ω / sq;
[0124] Step 4: Spin-coat a ZnO layer with a thickness of about 50 nm on the silver nanowire electrode layer prepared in step 3, and anneal at 130°C for 10 min;
[0125] Step 5: Spin-coat a 50 nm thick active layer of PTB7-Th: BTP-BO-4Cl xylene solution on the ZnO layer prepared in step 4, and anneal at 100°C for 10 min;
[0126] Step 6: Vacuum thermal evaporation is used to deposit a 100 nm thick tungsten oxide layer on the active layer prepared in step 5;
[0127] Step 7: Vacuum thermal evaporation is used to deposit a 100 nm thick Au electrode layer on the tungsten oxide layer prepared in step 6;
[0128] Step 8: A 100 μm thick fluororubber packaging layer is attached to the Au electrode layer prepared in step 7 to obtain the high-barrier flexible organic solar cell.
[0129] Example 7
[0130] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, 50 μm thick PEN, 4 μm thick ethylene and vinyl alcohol copolymer, 1 μm thick cyanuric acid epoxy resin layer, 90 nm thick silver nanowire electrode layer, 100 nm thick graphene oxide layer, 100 nm thick PM6:Y6 layer, 50 nm thick PFN-Br layer, 200 nm thick Ag electrode layer and 100 μm thick thermosetting acrylic resin encapsulation layer.
[0131] The preparation method of the high-barrier flexible organic solar cell is as follows:
[0132] Step 1: Prepare a 50 μm thick PEN substrate as a solar cell substrate, apply a 4 μm thick ethylene and vinyl alcohol copolymer on the substrate, and cure it at 100°C for 10 minutes;
[0133] Step 2: On the barrier layer prepared in step 1, a 1 μm thick cyanuric acid epoxy resin layer is scraped and cured at 100°C for 30 minutes;
[0134] Step 3: Gravure print a 90nm thick silver nanowire electrode layer on the modified layer prepared in step 2, with a square resistance of about 20Ω / sq;
[0135] Step 4: Spin-coat a 100 nm thick graphene oxide layer on the silver nanowire electrode layer prepared in step 3, and anneal at 150°C for 30 min;
[0136] Step 5: Spin-coat a 100 nm thick active layer of PM6:Y6 chloroform solution on the graphene oxide layer prepared in step 4, and anneal at 85°C for 5 min;
[0137] Step 6: Spin-coat a 50 nm thick PFN-Br layer on the active layer prepared in step 5 and anneal at 120 °C for 10 min
[0138] Step 7: A 200 nm thick Ag electrode layer is deposited on the PFN-Br layer prepared in step 6 by vacuum thermal evaporation deposition;
[0139] Step 8: A 100 μm thick thermosetting acrylic resin encapsulation layer is scraped onto the Ag electrode layer prepared in step 7, and cured at 120° C. for 10 min to obtain the high-barrier flexible organic solar cell.
[0140] Example 8
[0141] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, 125 μm thick PET, 4 μm thick ethylene and vinyl alcohol copolymer, 1 μm thick cyanuric acid epoxy resin layer, 90 nm thick silver nanowire electrode layer, 100 nm thick PEDOT:PSS layer, 80 nm thick PM6:L8-BO layer, 50 nm thick PNDIT-F3N layer, 200 nm thick Ag electrode layer and 100 μm thick thermosetting acrylic resin encapsulation layer.
[0142] The preparation method of the high-barrier flexible organic solar cell is as follows:
[0143] Step 1: Prepare a 125 μm thick PET substrate as a solar cell substrate, apply a 4 μm thick ethylene and vinyl alcohol copolymer on the substrate, and cure it at 100°C for 10 minutes;
[0144] Step 2: On the barrier layer prepared in step 1, a 1 μm thick cyanuric acid epoxy resin layer is scraped and cured at 100°C for 30 minutes;
[0145] Step 3: Gravure print a 90nm thick silver nanowire electrode layer on the modified layer prepared in step 2, with a square resistance of about 20Ω / sq;
[0146] Step 4: Spin-coat a 100 nm thick PEDOT:PSS on the silver nanowire electrode layer prepared in step 3, and anneal at 150°C for 30 min;
[0147] Step 5: Spin-coat an active layer PM6:L8-BO chloroform solution with a thickness of 80 nm on the graphene oxide layer prepared in step 4, and anneal at 85°C for 5 min;
[0148] Step 6: Spin-coat a 50 nm thick PNDIT-F3N layer on the active layer prepared in step 5 and anneal at 120 °C for 10 min;
[0149] Step 7: A 200 nm thick Ag electrode layer is deposited on the PNDIT-F3N layer prepared in step 6 by vacuum thermal evaporation deposition;
[0150] Step 8: A 100 μm thick thermosetting acrylic resin encapsulation layer is scraped onto the Ag electrode layer prepared in step 7, and cured at 120° C. for 10 min to obtain the high-barrier flexible organic solar cell.
[0151] Example 9
[0152] The structure of a high-barrier flexible organic solar cell provided in this embodiment is, from bottom to top, 125 μm thick PET, 1 μm thick silicon nitride, 1 μm thick photoconversion hydrophilic and hydrophobic material modification layer (components are acrylate-NBE and PETMP), 90 nm thick silver nanowire electrode layer, 40 nm thick ZnO layer, 100 nm thick PM6:L8-BO layer, 20 nm thick MoOx layer, 200 nm thick Al electrode layer and 20 μm thick thermosetting acrylic resin encapsulation layer.
[0153] The preparation method of the high-barrier flexible organic solar cell is as follows:
[0154] Step 1: Prepare a 125 μm thick PET substrate as a solar cell substrate, and thermally deposit about 1 μm thick silicon nitride on the substrate;
[0155] Step 2: On the barrier layer prepared in step 1, a photoconvertible hydrophilic and hydrophobic material with a thickness of about 1 μm is scraped as a modification layer, and dried at room temperature to form a film;
[0156] Step 3: Gravure print a 90nm thick silver nanowire electrode layer on the modified layer prepared in step 2, with a square resistance of about 20Ω / sq;
[0157] Step 4: Spin-coat a ZnO layer with a thickness of about 40 nm on the silver nanowire electrode layer prepared in step 3, and anneal at 130°C for 10 min;
[0158] Step 5: Spin-coat a 100 nm thick active layer PM6:L8-BO chloroform solution on the ZnO layer prepared in step 4 and anneal at 85°C for 5 min;
[0159] Step 6: Vacuum thermal evaporation is used to deposit a 20 nm thick MoOx layer on the active layer prepared in step 5;
[0160] Step 7: Vacuum thermal evaporation is used to deposit a 200 nm thick Al electrode layer on the MoOx layer prepared in step 6;
[0161] Step 8: A 20 μm thick thermosetting acrylic resin encapsulation layer is scraped onto the Al electrode layer prepared in step 7, and cured at 120° C. for 10 min to obtain the high-barrier flexible organic solar cell.
[0162] Example 10
[0163] The present embodiment is different from the embodiment 9 in that the components of the photoconvertible hydrophilic and hydrophobic material are hexyl-NBE and HDT.
[0164] Embodiment 11
[0165] The present embodiment is different from the embodiment 9 in that the photoconvertible hydrophilic and hydrophobic material comprises butyl-NBC and TMPMP.
[0166] Table 1 Performance parameters of flexible solar cells of Examples 1 to 11
[0167]
[0168]
[0169] Comparative Example 1
[0170] The difference between this comparative example and Example 1 is that the preparation of the modification layer in step 2 is not performed, and the remaining steps are the same, so as to obtain a barrier flexible organic solar cell without a modification layer.
[0171] The morphology of the silver nanowire electrode on the barrier layer without the modification layer obtained in step 3 can be found in Figure 6a-6b shown.
[0172] Comparative Example 2
[0173] The difference between this comparative example and Example 3 is that the preparation of the modification layer in step 2 is not performed, and the remaining steps are the same, so as to obtain a barrier flexible organic solar cell without a modification layer.
[0174] Comparative Example 3
[0175] The difference between this comparative example and Example 8 is that the preparation of the barrier layer in step 1 and the preparation of the modification layer in step 2 are not performed, and the remaining steps are the same to prepare a non-barrier flexible organic solar cell.
[0176] The morphology of the silver nanowire electrode on the substrate layer obtained in step 3 can be found in Figure 7 shown.
[0177] Table 2 Performance parameters of flexible solar cells of Comparative Examples 1 to 3
[0178]
[0179] Test Case
[0180] 1. The barrier film with a modified layer prepared in step 2 of Example 1 to Example 11 was tested for water vapor transmission rate before and after bending:
[0181] The 100mm×100mm film to be tested was subjected to a 1000-fold bending test with a bending diameter of about 50mm using an automatic bending machine, and the MOCON 2 The water vapor transmission rate tester tests the film to be tested before and after bending. The results are shown in Table 3.
[0182] Table 3 Water vapor transmission rate of barrier films of Examples 1 to 11 before and after bending
[0183]
[0184] 2. Test the water vapor transmission rate of the barrier film or substrate film prepared in step 1 of Comparative Examples 1 to 3 before and after bending:
[0185] The 100mm×100mm film to be tested was subjected to a 1000-fold bending test with a bending diameter of about 50mm using an automatic bending machine, and the MOCON 2 The water vapor transmission rate tester tests the film to be tested before and after bending. The results are shown in Table 4.
[0186] Table 4 Water vapor transmission rate of barrier films or base films of comparative examples 1 to 3 before and after bending
[0187]
[0188] 3. The silver nanowire electrodes prepared in step 4 of Examples 1 to 11 and Comparative Examples 1 to 3 were subjected to a square resistance test before and after bending:
[0189] An automatic bending machine was used to perform a cyclic bending test on a 25mm×25mm film with a bending diameter of about 10mm for 10,000 times, and an ST-2258C multifunctional digital four-probe tester was used to test the film before and after bending. The average value of the five test points was taken. The results are shown in Table 5.
[0190] Table 5 Table of square resistance changes of silver wire electrodes before and after bending of Examples 1-11 and Comparative Examples 1-3
[0191]
[0192] 4. The flexible organic solar cells prepared in step 8 of Examples 1 to 11 and Comparative Examples 1 to 3 were subjected to an air storage stability test at 25±5°C and 30±5% humidity for 2000 h. The average PCE comparison results of the eight devices are shown in Table 6.
[0193] Table 6 Average PCE variation of Example 1-Example 11 and Comparative Example 1-Comparative Example 3
[0194] Initial average PCE (%) Average PCE after 2000h (%) Example 1 14.22 12.27 Example 2 13.17 11.80 Example 3 15.55 14.03 Example 4 15.60 13.85 Example 5 15.29 13.78 Example 6 10.04 8.84 Example 7 14.61 13.09 Example 8 15.16 13.27 Example 9 14.41 13.01 Example 10 14.02 12.72 Embodiment 11 13.97 12.38 Comparative Example 1 9.68 7.23 Comparative Example 2 10.87 8.05 Comparative Example 3 13.80 2.42
[0195] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0196] Obviously, the embodiments of the present invention shown above are only intended to illustrate the principles of the present invention, rather than to limit its implementation. Those skilled in the art can make other forms of modifications or changes to the present invention based on the above description. Since it is impossible to list all implementations in detail, any obviously derivable technical solution changes are still protected by the present invention.
Claims
1. A high-barrier flexible organic solar cell, characterized in that: It includes a flexible substrate, a barrier layer, a modification layer, a silver nanowire electrode layer, an organic functional layer, a top electrode layer and an encapsulation layer which are sequentially stacked along a set direction, wherein the material of the modification layer includes at least one of a high-transmittance photoresist, a resin, and a light-converting hydrophilic-hydrophobic material.
2. The high barrier flexible organic solar cell according to claim 1, characterized in that: The thickness of the modified layer is 0.1-10 μm, and the light transmittance is 75%-95%.
3. The high barrier flexible organic solar cell according to claim 1, characterized in that: The high-transmittance photoresist includes any one of SU-8, SUN-2300N, and SUN-5400N, or a combination of two or more thereof; and / or, the resin includes any one of polyvinyl alcohol and epoxy resin, or a combination of two or more thereof; and / or, the photoconvertible hydrophilic and hydrophobic material includes a combination of a photosensitive olefin monomer or a photosensitive alkyne monomer and a thiol compound, preferably, the photosensitive olefin monomer includes (2-nitro-1,4-phenyl)bis(methylene) diacrylate, the photosensitive alkyne monomer includes (2-nitro- Preferably, the thiol compound comprises at least any one of hexane-1,6-dithiol, 2-ethyl-2-(((3-mercaptopropionyl)oxy)methyl)propane-1,3-diylbis(3-mercaptopropionate), and 2,2-bis(((3-mercaptopropionyl)oxy)methyl)propane-1,3-diylbis(3-mercaptopropionate).
4. The high barrier flexible organic solar cell according to claim 1, characterized in that: The thickness of the barrier layer is 1-5 μm, and the water vapor transmission rate is less than 10 -2 g / m 2 day, oxygen transmission rate is less than 10 -1 cm 3 / (m 2 ·day·0.1MPa), light transmittance is 70%-90%.
5. The high-barrier flexible organic solar cell according to claim 1, characterized in that: The material of the barrier layer includes at least one of an inorganic substance and a polymer, wherein the inorganic substance includes any one of silicon oxide, aluminum oxide and silicon nitride or a combination of two or more thereof, and the polymer includes at least one of polyvinylidene chloride, ethylene and vinyl alcohol copolymer; And / or, the barrier layer is made by any one of vacuum thermal evaporation vapor deposition, chemical vapor deposition, anodization deposition, spin coating, coating and electrostatic spray deposition.
6. The high-barrier flexible organic solar cell according to claim 1, characterized in that: The thickness of the flexible substrate is 50-150 μm, and the light transmittance is 70%-95%; and / or the material of the flexible substrate includes any one of polyethylene terephthalate, polyethylene naphthalate and polyimide, or a combination of two or more thereof.
7. The high barrier flexible organic solar cell according to claim 1, characterized in that: The thickness of the silver nanowire electrode layer is 60-120nm, the square resistance is 10-30Ω / sq, and the optical transmittance is 70%-90%; And / or, the thickness of the organic functional layer is 100-250 nm; And / or, the organic functional layer comprises an electron transport layer, an active layer and a hole transport layer arranged in sequence along a set direction; Preferably, the organic functional layer comprises an electron transport layer / active layer / hole transport layer structure, the electron transport layer is close to the silver nanowire electrode layer, and in the electron transport layer / active layer / hole transport layer structure, the material of the electron transport layer comprises any one of zinc oxide and titanium oxide or a combination of two or more thereof; the material of the hole transport layer comprises any one of molybdenum oxide, nickel oxide and tungsten oxide or a combination of two or more thereof; Preferably, the organic functional layer comprises a hole transport layer / active layer / electron transport layer structure, the hole transport layer is close to the silver nanowire electrode layer, and in the hole transport layer / active layer / electron transport layer structure, the material of the hole transport layer comprises any one of PEDOT:PSS, graphene oxide, and transition metal oxides, or a combination of two or more thereof; the material of the electron transport layer comprises any one of PFN-Br, PNDIT-F3N, and PDINN, or a combination of two or more thereof; Preferably, the material of the active layer in the organic functional layer is a binary or multi-component system consisting of a donor material, a fullerene acceptor and / or a non-fullerene acceptor; wherein the donor material includes any one or a combination of two or more of PM6, PTB7-Th, and PBDB-T, and the fullerene acceptor includes PC 61 BM, the non-fullerene acceptor includes any one of L8-BO, BTP-BO-4C1, and Y6, or a combination of two or more thereof.
8. The high-barrier flexible organic solar cell according to claim 1, characterized in that: The thickness of the top electrode layer is 100-200nm; and / or, the material of the top electrode layer includes any one of Al, Ag and Au or a combination of two or more; and / or, the thickness of the encapsulation layer is 10-300μm; and / or, the material of the encapsulation layer includes any one of epoxy resin, acrylic resin, synthetic rubber or a combination of two or more.
9. The method for preparing a high-barrier flexible organic solar cell according to any one of claims 1 to 8, characterized in that: include: forming a barrier layer on a flexible substrate; forming a modification layer on the barrier layer; forming a silver nanowire electrode layer on the modified layer; forming an organic functional layer on the silver nanowire electrode layer; forming a top electrode layer on the organic functional layer; And, forming an encapsulation layer on the top electrode layer to obtain the high-barrier flexible organic solar cell.
10. The preparation method according to claim 9, characterized in that: include: Applying the barrier layer material to the flexible substrate by any one of vacuum thermal evaporation vapor deposition, chemical vapor deposition, anodization deposition, spin coating, coating, electrostatic spray deposition, and lamination to form the barrier layer; And / or, the preparation method comprises: applying the resin to the barrier layer by at least one of spin coating and coating, and then annealing at 100-120° C. for 20-30 min to prepare the modified layer; Alternatively, the preparation method comprises: applying a high-transmittance photoresist to the barrier layer by at least one of spin coating and coating, then baking at 95-110° C. for 1-3 min, and then heating at 60-200 mJ / cm 2 Exposure, or baking at 95-110° C. for 1-3 minutes to prepare the modified layer; Alternatively, the preparation method comprises: applying the photoconvertible hydrophilic and hydrophobic material to the barrier layer by at least one of spin coating and coating in a state avoiding white light, and then drying at room temperature to form a film, so as to prepare the modified layer; And / or, the preparation method comprises: preparing a silver nanowire electrode layer on the modified layer by at least one of gravure printing, spin coating, and coating; And / or, the preparation method comprises: forming a top electrode layer on the organic functional layer by at least one of vacuum evaporation, thermal evaporation vapor deposition, transfer method, and magnetron sputtering; And / or, the preparation method includes: forming an encapsulation layer on the top electrode layer by at least one of spin coating, coating or lamination.