Slurry composition for functional layer of non-aqueous secondary battery, separator for non-aqueous secondary battery, and non-aqueous secondary battery

By using a specific combination of granular polymers and water-soluble polymers in the functional layer of the secondary battery, the problems of insufficient anti-adhesion, electrolyte injection properties and high-temperature cycle characteristics in the existing technology are solved, and non-aqueous secondary batteries are realized. Improved performance of secondary batteries.

CN118843979APending Publication Date: 2024-10-25ZEON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026427.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-10
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

It is difficult for existing secondary battery functional layers to balance anti-adhesion properties, electrolyte injection properties, and high-temperature cycle characteristics during the manufacturing process, especially when stacking battery components and electrolyte injection.

Method used

A non-aqueous functional layer composition containing a granular polymer and a water-soluble polymer is used. The glass transition temperature of the granular polymer is between 30°C and 95°C, and the water-soluble polymer contains more than 3% of sulfonic acid-containing groups. Monomer unit, and preferably core-shell structure and appropriate volume average particle size to improve the anti-adhesion and electrolyte injection properties of the functional layer.

Benefits of technology

It achieves a balance between excellent anti-adhesion properties of the functional layer, high electrolyte injection property, and high-temperature cycle characteristics, thereby improving the overall performance of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005034064950000371
    Figure BDA0005034064950000371
  • Figure BDA0005034064950000381
    Figure BDA0005034064950000381
Patent Text Reader

Abstract

Provided is a slurry composition for a functional layer of a non-aqueous secondary battery, which contains a particulate polymer having a glass transition temperature within a prescribed range and a water-soluble polymer having a sulfonic acid group-containing monomer unit content of 3 mass% or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a slurry composition for a non-aqueous secondary battery functional layer, a separator for a non-aqueous secondary battery, and a non-aqueous secondary battery. Background Art

[0002] Non-aqueous secondary batteries such as lithium-ion secondary batteries (hereinafter sometimes simply referred to as “secondary batteries”) are small, lightweight, have high energy density, and can be repeatedly charged and discharged, and are therefore used in a wide range of applications.

[0003] Here, the secondary battery generally has an electrode (positive electrode, negative electrode), and a separator that isolates the positive electrode from the negative electrode and prevents a short circuit between the positive electrode and the negative electrode. Moreover, sometimes a porous film layer for improving heat resistance and strength, an adhesive layer for improving the adhesion between battery components, etc. (hereinafter, sometimes referred to as "functional layer") are provided on the surface of the electrode and / or separator. Specifically, an electrode formed by further forming a functional layer on an electrode substrate formed by arranging an electrode composite material layer on a current collector, and a separator formed by forming a functional layer on a separator substrate are used as battery components.

[0004] In the past, various studies have been conducted on compositions for forming functional layers for the purpose of improving the electrochemical characteristics of the obtained secondary batteries. For example, Patent Documents 1 to 2 disclose a separator for a secondary battery, which has a layer comprising a water-soluble acrylic binder, a binder different from the binder, and inorganic particles. In addition, for example, Patent Documents 3 to 4 disclose a granular polymer having a glass transition temperature that satisfies specified conditions as a binder component in a composition for a functional layer.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent document 1: Korean registered patent publication No. 10-2071382;

[0008] Patent document 2: Japanese Patent No. 6901234;

[0009] Patent document 3: International Publication No. 2013 / 151144;

[0010] Patent document 4: International Publication No. 2020 / 175025. Summary of the invention

[0011] Problem that the invention aims to solve

[0012] Here, in the manufacture of secondary batteries, it is necessary that even when the battery components containing the functional layer are temporarily kept in a stacked state, the battery components are difficult to adhere to each other across the functional layer (hereinafter referred to as "anti-adhesion"). In addition, in the manufacture of secondary batteries, when the electrolyte is preferably injected into the outer packaging containing the battery components, the electrolyte can penetrate the battery components well (that is, the electrolyte injection is excellent). In addition, the secondary battery also needs excellent cycle characteristics at high temperatures. However, while improving the anti-adhesion property, the electrolyte injection and high temperature cycle characteristics of the secondary battery having the functional layer are taken into account at a high level, and there is still room for improvement in the functional layer formed using the functional layer composition according to the above-mentioned prior art.

[0013] Therefore, an object of the present invention is to provide a slurry composition for a non-aqueous secondary battery functional layer that can provide a functional layer having excellent anti-blocking properties while achieving both high levels of electrolyte injection properties and high-temperature cycle characteristics.

[0014] Another object of the present invention is to provide a separator for a nonaqueous secondary battery that can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics of the resulting secondary battery and has excellent anti-blocking properties.

[0015] Another object of the present invention is to provide a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics.

[0016] Solutions for solving problems

[0017] The present inventors have conducted intensive research for the purpose of solving the above problems, focusing on the properties of water-soluble polymers and particulate polymers used to form functional layers. They have newly found that when the glass transition temperature of the particulate polymer is within a specified range and the water-soluble polymer has 3% by mass or more of sulfonic acid group-containing monomer units, a functional layer with excellent anti-blocking properties can be provided, and a non-aqueous secondary battery with excellent electrolyte injection properties and high-temperature cycle characteristics can be provided, thereby completing the present invention.

[0018] That is, the object of the present invention is to advantageously solve the above-mentioned problems. [1] The slurry composition for a non-aqueous secondary battery functional layer of the present invention is characterized in that it contains a granular polymer and a water-soluble polymer, the granular polymer has at least one glass transition temperature in the temperature range of 30°C to 95°C, and the water-soluble polymer contains a sulfonic acid group-containing monomer unit at a ratio of 3.0% by mass or more. In this way, according to the slurry composition for a functional layer containing a granular polymer having a glass transition temperature in the above-mentioned temperature range and a water-soluble polymer having 3% by mass or more of a sulfonic acid group-containing monomer unit, the anti-blocking property of the obtained functional layer can be improved, while the electrolyte injection property and high-temperature cycle characteristics of the obtained secondary battery can be taken into account at a high level.

[0019] In addition, the "glass transition temperature" of the granular polymer is a value determined based on the differential scanning calorimetry (DSC) curve. When the DSC curve has multiple peaks, the temperature shown by the peak with the largest displacement is taken as the glass transition temperature of the polymer. When multiple peaks with equal displacement are detected and it is the maximum value among the detected peaks, the average value is taken as the glass transition temperature of the polymer. In addition, in this specification, "containing monomer units" means "the polymer obtained by using the monomer contains repeating units from the monomer". In addition, the polymer is "water-soluble" means that when 0.5g of the polymer is dissolved in 100g of water at a temperature of 25°C, the insoluble component is less than 1.0% by mass. Furthermore, the "content ratio (mass %)" of each monomer unit (each repeating unit) contained in the water-soluble polymer can be expressed using 1 H-NMR, 13 C-NMR and other nuclear magnetic resonance (NMR) methods.

[0020] [2] In the non-aqueous secondary battery functional layer slurry composition of [1], the particulate polymer preferably has a core-shell structure. If the particulate polymer has a core-shell structure, the adhesion of the functional layer can be improved, and the cycle characteristics of the obtained secondary battery can be further improved.

[0021] [3] In addition, in the slurry composition for the non-aqueous secondary battery functional layer of [1] or [2], the volume average particle size of the granular polymer is preferably greater than 0.25 μm and less than 5 μm. If the volume average particle size of the granular polymer is within the above range, the adhesion of the obtained functional layer can be improved, and the internal resistance of the secondary battery can be reduced. In addition, the "volume average particle size" of the granular polymer refers to the particle size D50 at which the cumulative volume calculated from the small particle size side becomes 50% in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution measuring device. Specifically, it can be measured using the method described in the examples of this specification.

[0022] [4] Here, in the slurry composition for a non-aqueous secondary battery functional layer according to any one of [1] to [3], the weight average molecular weight of the water-soluble polymer is preferably 50,000 to 1,000,000. If the weight average molecular weight of the water-soluble polymer is above the lower limit, the adhesion of the functional layer can be improved, and if it is below the upper limit, the dispersibility of the slurry composition is improved, the resistance of the obtained functional layer can be reduced, and the internal resistance of the secondary battery can be reduced.

[0023] [5] In addition, the slurry composition for a non-aqueous secondary battery functional layer according to any one of [1] to [4] may further contain heat-resistant particles. If the slurry composition contains heat-resistant particles, a functional layer that functions to improve the heat resistance of a battery member can be appropriately produced.

[0024] [6] In addition, the present invention aims to advantageously solve the above-mentioned problems. The separator for a non-aqueous secondary battery of the present invention is characterized by comprising a separator substrate and a functional layer formed on at least a portion of at least one surface of the separator substrate, wherein the functional layer is a dried product of the slurry composition for a non-aqueous secondary battery functional layer of any one of the above [1] to [5]. As described above, the separator having the separator substrate and the functional layer which is a dried product of any one of the above slurry compositions has excellent anti-blocking properties, and can simultaneously achieve both electrolyte injection properties and high-temperature cycle characteristics of the obtained secondary battery at a high level.

[0025] [7] In addition, the present invention aims to advantageously solve the above-mentioned problems. The non-aqueous secondary battery of the present invention is characterized by comprising a positive electrode, a negative electrode, a separator and an electrolyte, wherein the separator is the separator for a non-aqueous secondary battery of [6]. As described above, the secondary battery having the separator can achieve both electrolyte injection properties and high-temperature cycle characteristics at a high level.

[0026] Effects of the Invention

[0027] According to the present invention, a slurry composition for a nonaqueous secondary battery functional layer can provide a functional layer having excellent anti-blocking properties and a secondary battery having both high electrolyte injection properties and high-temperature cycle characteristics.

[0028] Furthermore, according to the present invention, it is possible to provide a separator for a nonaqueous secondary battery which can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics of the resulting secondary battery and has excellent anti-blocking properties.

[0029] Furthermore, according to the present invention, a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics can be provided. DETAILED DESCRIPTION

[0030] Hereinafter, embodiments of the present invention will be described in detail.

[0031] Here, the slurry composition for the functional layer of the non-aqueous secondary battery of the present invention can be used as a material for preparing a functional layer possessed by a battery component such as a separator or an electrode. Moreover, the separator for the non-aqueous secondary battery of the present invention has a functional layer formed by the dried product of the slurry composition for the functional layer of the non-aqueous secondary battery of the present invention. Moreover, the non-aqueous secondary battery of the present invention has the separator for the non-aqueous secondary battery of the present invention. In addition, the so-called functional layer may be an adhesive layer that exerts the bonding ability between a battery component having a functional layer and other battery components as an adherend, or the functional layer may also be a heat-resistant adhesive layer that contains heat-resistant particles and can exert the function of heat resistance in addition to the bonding ability.

[0032] (Slurry composition for non-aqueous secondary battery functional layer)

[0033] The slurry composition for a nonaqueous secondary battery functional layer of the present invention contains a particulate polymer and a water-soluble polymer, and may further contain a solvent and other components as desired.

[0034] Here, the granular polymer contained in the slurry composition of the present invention has at least one glass transition temperature in a temperature range of 30°C or more and 95°C or less. Furthermore, the water-soluble polymer contained in the slurry composition of the present invention contains a sulfonic acid group-containing monomer unit at a ratio of 3.0% by mass or more. According to the slurry composition containing both the granular polymer and the water-soluble polymer satisfying the specified properties, a functional layer with excellent anti-blocking properties can be provided, and at the same time, a secondary battery that can take into account both electrolyte injection properties and high-temperature cycle characteristics at a high level can be provided.

[0035] <Particle polymer>

[0036] The particulate polymer has at least one glass transition temperature in the temperature range of 30°C to 95°C. In addition, the particulate polymer is preferably water-insoluble. Here, in this specification, the polymer is "water-insoluble" means that when 0.5 g of the polymer is dissolved in 100 g of water at a temperature of 25°C, the insoluble component is 90% by mass or more.

[0037] <<Glass transition temperature>>

[0038] The temperature range in which the granular polymer has at least one glass transition temperature needs to be above 30°C and below 95°C, preferably below 75°C, more preferably below 68°C, preferably above 35°C, and more preferably above 45°C. If the temperature range in which the granular polymer has at least one glass transition temperature is above the above lower limit, the anti-adhesion property of the obtained functional layer can be improved, and the internal resistance of the obtained secondary battery can be reduced. If the temperature range in which the granular polymer has at least one glass transition temperature is below the above upper limit, the deformability of the granular polymer during pressing when making a secondary battery is improved, the adhesion of the functional layer after impregnation with the electrolyte can be further improved, and the cycle characteristics of the obtained secondary battery can be improved. In addition, the glass transition temperature of the granular polymer can be adjusted, for example, by changing the type and proportion of the monomers used to prepare the granular polymer.

[0039] When the particulate polymer is a polymer having a core-shell structure as described below, or when a plurality of polymers are used in combination, as described in Examples below, the temperature shown by the peak with a large shift is taken as the glass transition temperature of the polymer.

[0040] <<Core-shell structure>>

[0041] The granular polymer preferably has a core-shell structure. The granular polymer with a core-shell structure has the following core-shell structure, which has a core and a shell covering the outer surface of the core. By using a granular polymer with a core-shell structure, if the granular polymer has a core-shell structure, the adhesion of the functional layer after electrolyte impregnation can be improved, and the cycle characteristics of the obtained secondary battery can be further improved. Here, the shell can cover the outer surface of the core as a whole, or it can be partially covered. In addition, even if it looks like the outer surface of the core is completely covered by the shell, as long as a hole connecting the inside and outside of the shell is formed, the shell is also a shell that partially covers the outer surface of the core. Therefore, for example, the granular polymer with the following shell belongs to a granular polymer in which the shell partially covers the outer surface of the core, and the shell has pores connected to the outer surface of the core from the outer surface of the shell (that is, the peripheral surface of the granular polymer).

[0042] In addition, the granular polymer may have any constituent elements except the above-mentioned core and shell as long as it does not significantly damage the desired effect. Specifically, for example, the granular polymer may have a part formed by a polymer different from the core inside the core. When citing a specific example, the seed particles used in the case of manufacturing the granular polymer by seed polymerization may remain inside the core. However, from the viewpoint of significantly exerting the desired effect, the granular polymer preferably only has a core and shell.

[0043] <<Volume average particle size>>

[0044] The volume average particle size of the granular polymer is preferably 0.25 μm or more, more preferably 0.30 μm or more, further preferably 0.40 μm or more, preferably 5.0 μm or less, more preferably 4.0 μm or less, further preferably 3.0 μm or less, and particularly preferably 1.4 μm or less. It is inferred that if the volume average particle size of the granular polymer is above the above lower limit, it is easy to ensure a small gap in the functional layer, so the internal resistance of the secondary battery obtained can be reduced. On the other hand, if the volume average particle size of the granular polymer is below the above upper limit, the adhesion of the functional layer after the electrolyte is impregnated can be further improved.

[0045] The volume average particle size of the particulate polymer can be adjusted by, for example, changing the type and ratio of monomers used to prepare the particulate polymer and / or changing the polymerization conditions of the particulate polymer (for example, the amount of emulsifier used).

[0046] <<Composition>>

[0047] The composition of the granular polymer is not particularly limited as long as it has at least one glass transition temperature below 95°C. For example, the granular polymer may be a homopolymer formed by repeating units of a single monomer, or a copolymer comprising copolymer units of a plurality of monomers. As a homopolymer, there is no particular limitation, and examples thereof include: polyvinyl acetate, polyvinylidene fluoride, and polymethyl methacrylate. Among them, in the case where the granular polymer is a homopolymer, polyvinyl acetate is preferred. In addition, as a copolymer, for example, a copolymer of the composition shown illustratively below can be cited. Moreover, in the case where the granular polymer is a polymer having the above-mentioned core-shell structure, the composition of the polymer forming the core portion can be the following composition.

[0048] The repeating unit contained in the particulate polymer is not particularly limited, and preferably includes an aromatic monovinyl monomer unit and a crosslinkable monomer unit. The particulate polymer may contain only one type of monomer unit (repeating unit) or may contain a plurality of types.

[0049] -Aromatic monovinyl monomer unit-

[0050] Examples of the aromatic monovinyl monomers that can form the aromatic monovinyl monomer units of the granular polymer include styrene, styrene sulfonic acid and its salts (e.g., sodium styrene sulfonate), α-methylstyrene, vinyltoluene, 4-(tert-butoxy)styrene, etc. These may be used alone or in combination of a plurality of them. Among these, styrene is preferred.

[0051] Moreover, with all repeating units as 100 mass %, the ratio of the aromatic monovinyl monomer units contained in the granular polymer is preferably 20 mass % or more, more preferably 30 mass % or more, more preferably 40 mass % or more, preferably 85 mass % or less, more preferably 75 mass % or less, and further preferably 70 mass % or less. If the proportion of the aromatic monovinyl monomer units in the polymer of the core is above the above lower limit, the glass transition temperature of the polymer of the core is improved, and the anti-adhesion property of the battery component with the functional layer can be improved. On the other hand, if the proportion of the aromatic monovinyl monomer units in the polymer of the core is below the above upper limit, the deformability of the granular polymer during the pressing when making the secondary battery can be fully ensured, so the adhesion of the functional layer after the electrolyte impregnation can be further improved.

[0052] - Cross-linking monomer unit-

[0053] The crosslinkable monomer that can form the crosslinkable monomer unit of the granular polymer is not particularly limited, and examples thereof include monomers that can form a crosslinked structure by polymerization. Examples of crosslinkable monomers generally include monomers having thermal crosslinkability. More specifically, examples thereof include: a crosslinkable monomer having a crosslinkable group having thermal crosslinkability and having one ethylenic double bond per molecule; and a crosslinkable monomer having two or more ethylenic double bonds per molecule.

[0054] Examples of the heat-crosslinkable crosslinkable group include an epoxy group, an N-methylolamide group, an oxetane group, Among these, an epoxy group is more preferred from the viewpoint of easy cross-linking and easy adjustment of cross-linking density.

[0055] Examples of crosslinkable monomers having an epoxy group as a heat-crosslinkable crosslinkable group and having an ethylenic double bond include unsaturated glycidyl ethers such as vinyl glycidyl ether, allyl glycidyl ether, butenyl glycidyl ether, and o-allylphenyl glycidyl ether; monoepoxides of dienes or polyenes such as butadiene monoepoxide, chloroprene monoepoxide, 4,5-epoxy-2-pentene, 3,4-epoxy-1-vinylcyclohexene, and 1,2-epoxy-5,9-cyclododecadiene; ; alkenyl epoxides such as 3,4-epoxy-1-butene, 1,2-epoxy-5-hexene, and 1,2-epoxy-9-decene; and glycidyl esters of unsaturated carboxylic acids such as glycidyl acrylate, glycidyl methacrylate, glycidyl crotonate, glycidyl 4-heptanoate, glycidyl sorbate, glycidyl linoleate, glycidyl-4-methyl-3-pentenoate, glycidyl ester of 3-cyclohexenecarboxylic acid, and glycidyl ester of 4-methyl-3-cyclohexenecarboxylic acid.

[0056] In addition, as an example of a crosslinkable monomer having an N-hydroxymethylamide group as a heat-crosslinkable crosslinkable group and having an ethylenic double bond, (meth)acrylamides having a hydroxymethyl group such as N-hydroxymethyl (meth)acrylamide can be cited. In addition, in this specification, "(meth)acrylamide" refers to acrylamide and / or methacrylamide.

[0057] Furthermore, examples of crosslinkable monomers having an oxetane group as a heat-crosslinkable crosslinkable group and having an olefinic double bond include: 3-((meth)acryloyloxymethyl)oxetane, 3-((meth)acryloyloxymethyl)-2-trifluoromethyloxetane, 3-((meth)acryloyloxymethyl)-2-phenyloxetane, 2-((meth)acryloyloxymethyl)oxetane, and 2-((meth)acryloyloxymethyl)-4-trifluoromethyloxetane. In addition, in the present specification, "(meth)acryloyl" refers to acryloyl and / or methacryloyl.

[0058] In addition, as a Examples of crosslinkable monomers having a thermally crosslinkable crosslinkable group and an ethylenic double bond include: 2-vinyl-2-oxazoline group. Oxazoline, 2-vinyl-4-methyl-2- Oxazoline, 2-vinyl-5-methyl-2- Oxazoline, 2-isopropenyl-2- Oxazoline, 2-isopropenyl-4-methyl-2- Oxazoline, 2-isopropenyl-5-methyl-2- Oxazoline and 2-isopropenyl-5-ethyl-2- Oxazoline.

[0059] Furthermore, examples of crosslinking monomers having two or more ethylenic double bonds per molecule include allyl (meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipropylene glycol diallyl ether, polyethylene glycol diallyl ether, triethylene glycol divinyl ether, hydroquinone diallyl ether, tetraallyloxyethane, trimethylolpropane diallyl ether, allyl or vinyl ethers of polyfunctional alcohols other than those mentioned above, triallylamine, methylenebisacrylamide and divinylbenzene.

[0060] In addition, in this specification, "(meth)acrylate" means acrylate and / or methacrylate.

[0061] The crosslinking monomer may be used alone or in combination of two or more. Among these, a crosslinking monomer having two or more ethylenic double bonds per molecule is preferred, ethylene glycol dimethacrylate and allyl methacrylate are more preferred, and ethylene glycol dimethacrylate is further preferred.

[0062] Moreover, with all repeating units as 100% by mass, the proportion of the crosslinkable monomer units contained in the granular polymer is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, preferably 15.0% by mass or less, more preferably 13.0% by mass or less, and further preferably 5.0% by mass or less. If the proportion of the crosslinkable monomer units in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte immersion and the rate characteristics and cycle characteristics of the secondary battery can be improved.

[0063] -Other monomer units-

[0064] The monomer units (other monomer units) other than the aromatic monovinyl monomer unit and the crosslinking monomer unit that the particulate polymer may contain are not particularly limited, and examples thereof include acidic group-containing monomer units, (meth)acrylic acid ester monomer units, and nitrile group-containing monomer units.

[0065] -Acidic group-containing monomer unit

[0066] As the acidic group-containing monomers that can form the acidic group-containing monomer units of the granular polymer, carboxylic acid group-containing monomers, sulfonic acid group-containing monomers, phosphoric acid group-containing monomers, etc. can be cited. These can be used alone or in combination. In addition, the acid group of the acidic group-containing monomer unit can also form salts with alkali metals, ammonia, etc.

[0067] Examples of the carboxylic acid group-containing monomer include ethylenically unsaturated monocarboxylic acids and derivatives thereof, ethylenically unsaturated dicarboxylic acids and anhydrides thereof, and derivatives thereof.

[0068] Examples of ethylenically unsaturated monocarboxylic acids include acrylic acid, methacrylic acid, crotonic acid, etc. Examples of derivatives of ethylenically unsaturated monocarboxylic acids include 2-ethylacrylic acid, isocrotonic acid, α-acetoxyacrylic acid, β-trans-aryloxyacrylic acid, α-chloro-β-E-methoxyacrylic acid, β-diaminoacrylic acid, etc.

[0069] Examples of ethylenically unsaturated dicarboxylic acids include maleic acid, fumaric acid, itaconic acid, mesaconic acid, etc. Also, examples of anhydrides of ethylenically unsaturated dicarboxylic acids include maleic anhydride, acrylic anhydride, methyl maleic anhydride, dimethyl maleic anhydride, etc. Furthermore, examples of derivatives of ethylenically unsaturated dicarboxylic acids include methyl maleic acid, dimethyl maleic acid, phenyl maleic acid, chloromaleic acid, dichloromaleic acid, fluoromaleic acid, diphenyl maleate, nonyl maleate, decyl maleate, dodecyl maleate, octadecyl maleate, fluoroalkyl maleate, etc.

[0070] Examples of the sulfonic acid group-containing monomer include vinyl sulfonic acid, methylvinyl sulfonic acid, (meth)allyl sulfonic acid, ethyl (meth)acrylate-2-sulfonate, 2-acrylamido-2-methylpropanesulfonic acid, and 3-allyloxy-2-hydroxypropanesulfonic acid.

[0071] In addition, in this specification, "(meth)allyl" means allyl and / or methallyl, and "(meth)acrylic acid" means acrylic acid and / or methacrylic acid.

[0072] Examples of the phosphoric acid group-containing monomer include 2-(meth)acryloyloxyethyl phosphate, methyl-2-(meth)acryloyloxyethyl phosphate, and ethyl-(meth)acryloyloxyethyl phosphate.

[0073] Among these, as the acidic group-containing monomer, a carboxylic acid group-containing monomer is preferred, acrylic acid, methacrylic acid, and itaconic acid are more preferred, and methacrylic acid is further preferred.

[0074] With all repeating units as 100 mass %, the ratio of the acidic group-containing monomeric unit that can be arbitrarily included in the granular polymer can be more than 1.0 mass %, can also be more than 1.5 mass %, is preferably below 7.0 mass %, more preferably below 6.0 mass %, further preferably below 5.0 mass %. If the shared ratio of the acidic group-containing monomeric unit in the granular polymer is more than the above-mentioned lower limit, the adhesion of the functional layer obtained in the electrolyte can be improved. On the other hand, if the shared ratio of the acidic group-containing monomeric unit in the granular polymer is below the above-mentioned upper limit, the cycle characteristics of the secondary battery can be further improved.

[0075] -(Meth)acrylate monomer unit-

[0076] Examples of the (meth)acrylate monomers that can form the (meth)acrylate monomer units of the particulate polymer include alkyl acrylates such as methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, tert-butyl acrylate, isobutyl acrylate, n-pentyl acrylate, isopentyl acrylate, hexyl acrylate, heptyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, nonyl acrylate, decyl acrylate, lauryl acrylate, n-tetradecyl acrylate, and stearyl acrylate; and alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, isobutyl methacrylate, n-pentyl methacrylate, isopentyl methacrylate, hexyl methacrylate, heptyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, nonyl methacrylate, decyl methacrylate, lauryl methacrylate, n-tetradecyl methacrylate, stearyl methacrylate, and glycidyl methacrylate. These may be used alone or in combination of two or more. Among these, 2-ethylhexyl acrylate, n-butyl acrylate, and ethyl acrylate are preferred, and 2-ethylhexyl acrylate is more preferred.

[0077] Moreover, with all repeating units as 100% by mass, the proportion of the (meth)acrylate monomer units that can be arbitrarily contained in the granular polymer is preferably 20% by mass or more, preferably 50% by mass or less, and more preferably 40% by mass or less. If the proportion of the (meth)acrylate monomer units in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte immersion and the rate characteristics and cycle characteristics of the secondary battery can be improved.

[0078] -Nitrile-containing monomer unit-

[0079] As the nitrile-containing monomers that can form nitrile-containing monomer units of the granular polymer, α, β-ethylenically unsaturated nitrile monomers can be mentioned. Specifically, as α, β-ethylenically unsaturated nitrile monomers, there are no particular limitations as long as they are α, β-ethylenically unsaturated compounds having nitrile groups, and examples thereof include: acrylonitrile; α-halogenated acrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitriles such as methacrylonitrile and α-ethylacrylonitrile, etc. These can be used alone or in combination. Moreover, among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred.

[0080] Moreover, taking all repeating units as 100 mass %, the proportion of the nitrile-containing monomeric unit that can be arbitrarily contained in the granular polymer can be 1 mass % or more, can also be 5 mass % or more, is preferably 20 mass % or less, and more preferably 15 mass % or less. If the proportion of the nitrile-containing monomeric unit in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte impregnation and the rate characteristics and cycle characteristics of the secondary battery can be improved.

[0081] Here, as described above, when the particulate polymer is a core-shell polymer having a core-shell structure, the polymer forming the core portion is preferably as described above, and the polymer forming the shell portion is preferably as described below.

[0082] [Shell]

[0083] When the particulate polymer is a core-shell polymer having a core-shell structure, the repeating units contained in the polymer forming the shell portion are not particularly limited, and preferably aromatic monovinyl monomer units and acidic group-containing monomer units can be mentioned. In addition, the polymer of the shell portion can contain only one monomer unit (repeat unit) or multiple monomer units.

[0084] -Aromatic monovinyl monomer unit-

[0085] As the aromatic monovinyl monomer of the aromatic monovinyl monomer unit of the polymer capable of forming the shell portion, the same monomers as those mentioned above can be cited. These can be used alone or in combination of multiple types. Moreover, among these, styrene is preferred.

[0086] Moreover, with all repeating units as 100 mass %, the ratio of the aromatic monovinyl monomer units contained in the polymer of the shell is preferably 10 mass % or more, more preferably 20 mass % or more. If the ratio of the aromatic monovinyl monomer units of the shell in the granular polymer is 10 mass % or more, then in the granular polymer with a core-shell structure, the glass transition temperature of the polymer of the shell is improved, and the anti-adhesion property of the battery component with a functional layer can be improved. In addition, the upper limit of the ratio of the aromatic monovinyl monomer units of the shell in the granular polymer is preferably 40 mass % or less, more preferably 30 mass % or less.

[0087] -Acidic group-containing monomer unit

[0088] As the acidic group-containing monomers of the acidic group-containing monomer units of the polymer capable of forming the shell portion, the same monomers as those described in the "core portion" can be cited. These can be used alone or in combination of multiple types. Moreover, among these, carboxylic acid group-containing monomers are preferred, acrylic acid, methacrylic acid, itaconic acid are more preferred, and methacrylic acid is further preferred.

[0089] And, with the whole repeating units contained in granular polymer (that is, the total of the polymer of core portion and the polymer of shell portion) as 100 mass %, the ratio of the acidic group-containing monomeric unit contained in the polymer of shell portion is preferably more than 0.01 mass %, more preferably more than 0.1 mass %, preferably below 1.0 mass %, more preferably below 0.6 mass %. If the shared ratio of the acidic group-containing monomeric unit of shell portion in granular polymer is more than the above-mentioned lower limit, then the adhesion of the functional layer in the electrolyte can be improved. On the other hand, if the shared ratio of the acidic group-containing monomeric unit of shell portion in granular polymer is below the above-mentioned upper limit, then the cycle characteristics of secondary battery can be further improved.

[0090] -Other monomer units-

[0091] The monomer units (other monomer units) other than the aromatic monovinyl monomer units and the acidic group-containing monomer units that can be included in the polymer forming the shell portion are not particularly limited, and examples thereof include the crosslinking monomer units, (meth)acrylate monomer units, and nitrile-containing monomer units. Moreover, among these, the polymer of the shell portion preferably includes nitrile-containing monomer units.

[0092] As the nitrile-containing monomers of the nitrile-containing monomer units of the polymer capable of forming the shell portion, the same monomers as those mentioned above can be cited. These can be used alone or in combination. Moreover, among these, acrylonitrile and methacrylonitrile are preferred, and acrylonitrile is more preferred.

[0093] Moreover, with all repeating units contained in the granular polymer (i.e., the total of the polymer of the core portion and the polymer of the shell portion) as 100 mass%, the ratio of the nitrile-containing monomeric unit contained in the polymer of the shell portion is preferably 0.5 mass% or more, more preferably 1.0 mass% or more, preferably 10.0 mass% or less, more preferably 5.0 mass% or less. If the ratio of the nitrile-containing monomeric unit of the shell portion in the granular polymer is within the above range, the adhesion of the functional layer after electrolyte impregnation and the rate characteristics and cycle characteristics of the secondary battery can be further improved.

[0094] <<Preparation method>>

[0095] Moreover, the preparation method of the granular polymer is not particularly limited, and can be a method following conventional methods such as emulsion polymerization. For example, in the case where the granular polymer is a core-shell polymer having a core-shell structure, it can be prepared by, for example, using monomers of the polymer of the core portion and monomers of the polymer of the shell portion to change the ratio of their monomers over time and polymerize in stages. Specifically, the granular polymer with a core-shell structure can be prepared by a continuous multi-stage emulsion polymerization method and a multi-stage suspension polymerization method such that the polymer in the later stage is sequentially coated on the polymer in the previous stage (for example, with reference to International Publication No. 2020 / 175025).

[0096] <Water-soluble polymer>

[0097] The slurry composition of the present invention contains a water-soluble polymer containing a sulfonic acid group-containing monomer unit at a ratio of 3% by mass or more. The water-soluble polymer is a component that can also function as a binder in the heat-resistant layer formed using the slurry composition, and can impart a binder ability to the functional layer formed using the slurry composition, while being able to keep components other than the water-soluble polymer, such as heat-resistant particles, contained in the functional layer from leaving the functional layer.

[0098] Here, the water-soluble polymer is not particularly limited as long as it contains the sulfonic acid group-containing monomeric unit at a ratio of 3% by mass or more, and optionally, it may contain repeating units other than the sulfonic acid group-containing monomeric unit (hereinafter referred to as "other repeating units"). Other repeating units are not particularly limited, and examples thereof include acidic group-containing monomeric units and nitrile group-containing monomeric units.

[0099] <<Sulfonic acid group-containing monomer unit>>

[0100] As the sulfonic acid group-containing monomer capable of forming the sulfonic acid group-containing monomer unit, for example, vinyl sulfonic acid, methyl vinyl sulfonic acid, (methyl) allyl sulfonic acid, styrene sulfonic acid, (methyl) acrylic acid-2-sulfonic acid ethyl ester, anethole sulfonic acid, acrylamidoalkanesulfonic acid, (methyl) acrylic acid sulfoalkyl ester or their salts can be cited. Here, the alkane in the acrylamidoalkanesulfonic acid preferably has a carbon number of 1 or more and a carbon number of 20 or less, more preferably a carbon number of 10 or less, and further preferably a carbon number of 6 or less. In addition, the alkyl in the (methyl) acrylic acid sulfoalkyl ester preferably has a carbon number of 1 or more and a carbon number of 20 or less, more preferably a carbon number of 10 or less, and further preferably a carbon number of 6 or less. The salt of the monomer listed above refers to a salt composed of a sulfonic acid group and an appropriate ion. As the ion, for example, an alkali metal ion can be cited, in which case the salt can be an alkali metal sulfonate. Specifically, examples of the acrylamidoalkanesulfonic acid include 2-acrylamide-2-methylpropanesulfonic acid, and examples of the sulfoalkyl(meth)acrylate include 2-sulfoethyl(meth)acrylate and 3-sulfopropyl(meth)acrylate.

[0101] Taking all repeating units contained in the water-soluble polymer as 100% by mass, the content ratio of the sulfonic acid group-containing monomer unit in the water-soluble polymer needs to be 3% by mass or more, preferably 10% by mass or more, preferably 22% by mass or less, and more preferably 16% by mass or less. If the content ratio of the sulfonic acid group-containing monomer unit in the water-soluble polymer is above the above lower limit, the adhesion of the obtained adhesive layer in the electrolyte can be improved, and the cycle characteristics of the obtained secondary battery can be improved. In addition, if the content ratio of the sulfonic acid group-containing monomer unit in the water-soluble polymer is below the above upper limit, the dispersion stability of the slurry composition can be improved, and the internal resistance of the obtained secondary battery can be reduced.

[0102] <<Acidic group-containing monomer unit>>

[0103] Examples of the acidic group-containing monomer capable of forming the acidic group-containing monomer unit include monomers containing an acidic group other than a sulfonic acid group as an acidic group. Examples of such monomers include the carboxylic acid group-containing monomers and phosphoric acid group-containing monomers described in the section of the particulate polymer.

[0104] Here, the acidic group-containing monomer may be used alone or in combination of two or more at any ratio. The acidic group-containing monomer capable of forming the acidic group-containing monomer unit is preferably a carboxylic acid-containing monomer, more preferably a monocarboxylic acid, and further preferably acrylic acid.

[0105] In addition, in the water-soluble polymer used in the present invention, when the amount of all repeating units in the water-soluble polymer is taken as 100% by mass, the content ratio of the acidic group-containing monomeric unit is preferably 5% by mass or more, more preferably 15% by mass or more, more preferably 25% by mass or more, preferably 70% by mass or less, more preferably 60% by mass or less, and more preferably 42% by mass or less. If the content ratio of the acidic group-containing monomeric unit in the water-soluble polymer is above the above lower limit, the adhesion of the obtained functional layer in the electrolyte can be improved. On the other hand, if the content ratio of the acidic group-containing monomeric unit in the water-soluble polymer is below the above upper limit, the cycle characteristics of the obtained secondary battery can be further improved.

[0106] <<Nitrile group-containing monomer unit>>

[0107] As the nitrile-containing monomers that can form nitrile-containing monomer units, α,β-ethylenically unsaturated nitrile monomers can be cited. Specifically, as α,β-ethylenically unsaturated nitrile monomers, there are no particular limitations as long as they are α,β-ethylenically unsaturated compounds having nitrile groups, and examples thereof include: acrylonitrile; α-halogenated acrylonitriles such as α-chloroacrylonitrile and α-bromoacrylonitrile; α-alkyl acrylonitriles such as methacrylonitrile and α-ethylacrylonitrile, etc. In addition, even if it is a monomer containing a nitrile group, in the case of having a sulfonic acid group, the monomer is also understood as a "sulfonic acid group-containing monomer" as long as it is used to form a monomer unit contained in a water-soluble polymer.

[0108] Here, the above-mentioned nitrile group-containing monomers may be used alone or in combination of two or more at any ratio. In addition, as the nitrile group-containing monomer capable of forming the nitrile group-containing monomer unit, acrylonitrile is preferred from the viewpoint of improving the adhesion of the obtained functional layer in the electrolyte.

[0109] In addition, in the water-soluble polymer used in the present invention, when the amount of all repeating units in the water-soluble polymer is taken as 100% by mass, the content of the nitrile-containing monomer unit is preferably 10% by mass or more, more preferably 20% by mass or more, further preferably 30% by mass or more, preferably 70% by mass or less, and more preferably 60% by mass or less. If the content of the nitrile-containing monomer unit in the water-soluble polymer is above the above lower limit, the adhesion of the obtained functional layer in the electrolyte can be improved. On the other hand, if the content of the nitrile-containing monomer unit in the water-soluble polymer is below the above upper limit, the adhesion of the obtained functional layer in the electrolyte can be improved.

[0110] <<Other repeating units>>

[0111] The other repeating units contained in the water-soluble polymer are not particularly limited. For example, as other repeating units, monomer units derived from known monomers such as the (meth)acrylate monomer unit and the cross-linking monomer unit described in the "granular polymer" item can be cited. Even if it is a monomer unit that can be equivalent to these monomer units, in the case where the monomer unit has a sulfonic acid group, as long as it is a constituent element of the water-soluble polymer, it is also understood as a "sulfonic acid group-containing monomer unit". In addition, the water-soluble polymer may contain one other repeating unit, or may contain two or more in any ratio.

[0112] Moreover, when all repeating units (all monomer units) contained in the water-soluble polymer are taken as 100 mass %, the content ratio of other repeating units is preferably 10 mass % or less, more preferably 5 mass % or less, further preferably 1 mass % or less, and particularly preferably 0 mass %.

[0113] [Weight average molecular weight]

[0114] Here, the weight average molecular weight of the water-soluble polymer used in the present invention is preferably 50,000 or more, more preferably 150,000 or more, more preferably 200,000 or more, preferably 1,000,000 or less, more preferably 600,000 or less, and more preferably 550,000 or less. If the weight average molecular weight of the water-soluble polymer is above the above lower limit, the rigidity of the water-soluble polymer is improved, so that the adhesion of the functional layer in the electrolyte can be improved. On the other hand, if the weight average molecular weight of the water-soluble polymer is 1,000,000 or less, the dispersibility of the slurry composition can be improved, so that the obtained functional layer has low resistance, and the rate characteristics of the obtained secondary battery can be improved.

[0115] The weight average molecular weight of the water-soluble polymer can be adjusted by, for example, changing the type and amount of the polymerization initiator and / or polymerization accelerator used to prepare the water-soluble polymer.

[0116] <<Method for preparing water-soluble polymer>>

[0117] The above-mentioned water-soluble polymer is not particularly limited, and for example, can be prepared by any method in solution polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. In addition, as a polymerization method, addition polymerization such as ionic polymerization, free radical polymerization, and living free radical polymerization can be used. In addition, the polymerization initiator, polymerization accelerator, emulsifier, dispersant, chain transfer agent, etc. used during polymerization can use commonly used substances, and their usage amount is also the commonly used amount. Among them, since the removal operation of the solvent is not required, the safety of the solvent is high, and there is no problem of mixing with a surfactant, it is preferably used as an aqueous solution polymerization method using water as a polymerization solvent.

[0118] Here, the polymerization initiator that can be used in the preparation of the water-soluble polymer is not particularly limited, and known polymerization initiators such as sodium persulfate, ammonium persulfate, and potassium persulfate can be cited. Among them, ammonium persulfate is preferably used. The polymerization initiator can be used alone or in combination of two or more in any ratio.

[0119] In addition, the polymerization accelerator is not particularly limited, and a known reducing polymerization accelerator can be used, such as L-ascorbic acid, sodium bisulfite, and tetramethylethylenediamine. Among them, L-ascorbic acid is preferably used. The polymerization accelerator can be used alone or in combination of two or more at any ratio.

[0120] <<Content>>

[0121] Moreover, the content of the above-mentioned specified water-soluble polymer in the slurry composition is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, preferably 20 parts by mass or less, and more preferably 10 parts by mass or less relative to 100 parts by mass of the granular polymer. If the amount of the water-soluble polymer is within the above range, the adhesion of the obtained functional layer can be improved, and the anti-blocking property of the obtained functional layer can be further improved.

[0122] <Adhesive material for functional layer>

[0123] In addition to the above-mentioned granular polymer and water-soluble polymer, the slurry composition of the present invention preferably contains a functional layer binder that is a polymer different from these polymers. As a functional layer binder, there is no particular limitation, and any polymer can be used as long as it can exert the bonding ability for maintaining the components such as granular polymers in the functional layer and / or exert the bonding ability between the functional layer and the adherend. Among them, as a functional layer binder, a polymer with a glass transition temperature of less than 20°C is preferred. In addition, the functional layer binder is preferably water-insoluble.

[0124] <<Glass transition temperature>>

[0125] The glass transition temperature of the functional layer adhesive material is preferably less than 20°C, preferably less than 15°C, more preferably less than 12°C, preferably above -40°C, more preferably above -20°C, and further preferably above -10°C. In addition to the above-mentioned particulate polymer, if a slurry composition containing a functional layer adhesive material having a glass transition temperature less than the above-mentioned upper limit is used, the adhesion of the functional layer after electrolyte impregnation can be improved, and the rate characteristics of the secondary battery can be further improved. On the other hand, if the glass transition temperature of the functional layer adhesive material is above the above-mentioned lower limit, the anti-blocking property of the obtained functional layer can be improved.

[0126] In addition, the glass transition temperature of the binder material for the functional layer can be adjusted by, for example, changing the type and ratio of monomers used to prepare the binder material for the functional layer.

[0127] <<Composition>>

[0128] The composition of the adhesive material for the functional layer is not particularly limited. For example, the adhesive material for the functional layer can be an aromatic vinyl polymer in which the content ratio of the aromatic monovinyl monomer unit is more than 50% by mass of the total repeating units, or it can be an acrylic polymer in which the content ratio of the (meth) acrylate monomer unit is more than 50% by mass of the total repeating units. As other monomer units other than the aromatic monovinyl monomer unit that can constitute the aromatic vinyl polymer, there is no particular limitation, and examples thereof include aliphatic conjugated diene monomer units from 1,3-butadiene, etc., hydroxyl-containing monomer units from 2-hydroxyethyl acrylate, etc., and acidic group-containing monomer units from itaconic acid, etc. In addition, as other monomer units other than the (meth) acrylate monomer unit that can constitute the acrylic polymer, there is no particular limitation, and examples thereof include acidic group-containing monomer units from (meth) acrylic acid, etc., and nitrile-containing monomer units from acrylonitrile, etc.

[0129] The polymerization method of the functional layer binder is not particularly limited and can be carried out in accordance with a conventional method. In addition, as the functional layer binder, a commercially available binder can also be used.

[0130] <<Amount>>

[0131] The amount of the functional layer binder that can be incorporated into the slurry composition of the present invention is not particularly limited, and is preferably 1 part by mass or more, more preferably 2 parts by mass or more, preferably 50 parts by mass or less, and more preferably 40 parts by mass or less, relative to 100 parts by mass of the granular polymer. If the amount of the functional layer binder incorporated is greater than the above lower limit relative to 100 parts by mass of the granular polymer, the adhesion of the functional layer after electrolyte immersion can be further improved, and if it is less than the above upper limit, the anti-adhesion property of the battery component having the functional layer can be ensured.

[0132] <Solvent>

[0133] As the solvent contained in the slurry composition of the present invention, a known solvent that can be used as at least a dispersion medium of the above-mentioned particulate polymer can be used. Among them, water is preferably used as the solvent. In addition, at least a part of the solvent of the slurry composition is not particularly limited, and can be a polymerization solvent for preparing a particulate polymer and / or a water-soluble polymer.

[0134] <Other ingredients>

[0135] The slurry composition of the present invention may include any other components in addition to the above-mentioned components. Other components are not particularly limited as long as they do not affect the battery reaction, and known components can be used. In addition, these other components can be used alone or in combination of two or more.

[0136] Furthermore, examples of other components include heat-resistant particles, wetting agents (polyethylene oxide, polypropylene oxide, etc.), and other water-soluble polymers different from the above-mentioned water-soluble polymers (carboxymethylcellulose and its salts, polyvinyl alcohol, etc.).

[0137] The heat-resistant particles that can be blended in the slurry composition are not particularly limited, and examples thereof include known heat-resistant particles used in non-aqueous secondary batteries.

[0138] Specifically, as heat-resistant particles, inorganic particles and organic particles other than the above-mentioned granular polymer and the functional layer binding material can be used, and inorganic particles are generally used. Among them, as the material of the heat-resistant particles, it is preferred that the material is stably present and electrochemically stable under the use environment of the non-aqueous secondary battery. When the preferred example of the material of the heat-resistant particles is given from such a viewpoint, oxide particles such as aluminum oxide (Alumina), hydrated aluminum oxide (boehmite), silicon oxide, magnesium oxide (magnesia), calcium oxide, titanium oxide (Titania), BaTiO3, ZrO, aluminum oxide-silicon dioxide composite oxide, etc.; nitride particles such as aluminum nitride and boron nitride; covalent bond grains such as silicon and diamond; insoluble ionic grains such as barium sulfate, calcium fluoride, and barium fluoride; clay particles such as talc and montmorillonite, etc. In addition, these particles can be subjected to element substitution, surface treatment, solid solution, etc. as needed.

[0139] When organic fine particles are used as heat-resistant particles, the glass transition temperature and / or melting point of the organic fine particles is usually higher than 150°C, preferably 180°C or higher, and more preferably 200°C or higher.

[0140] The above-mentioned heat-resistant particles may be used alone or in combination of two or more.

[0141] Here, the amount of the heat-resistant particles contained in the slurry composition is not particularly limited, but is preferably 200 parts by mass or more and 1500 parts by mass or less relative to 100 parts by mass of the particulate polymer.

[0142] <Preparation method>

[0143] The preparation method of the slurry composition is not particularly limited. For example, the granular polymer, the water-soluble polymer and the solvent can be mixed with the functional layer binder and / or other components used as needed to prepare the slurry composition. The mixing method is not particularly limited, and in order to disperse the components efficiently, a disperser is usually used as a mixing device for mixing.

[0144] The dispersing machine is preferably a device capable of uniformly dispersing and mixing the above-mentioned components. When giving examples, ball mills, sand mills, pigment dispersing machines, attritors, ultrasonic dispersing machines, homogenizers, planetary mixers, etc. can be cited. In addition, from the viewpoint of being able to apply high dispersing shearing force, it is preferred to use high dispersing devices such as bead mills, roll mills, and Filmix.

[0145] (Functional layer)

[0146] The non-aqueous secondary battery functional layer slurry composition of the present invention can be used to form a functional layer on a suitable substrate. Specifically, a functional layer can be formed by drying the slurry composition on a suitable substrate. That is, the functional layer is formed by the dried product of the above-mentioned slurry composition, usually containing the above-mentioned granular polymer and water-soluble polymer, and arbitrarily containing the above-mentioned functional layer binding material and / or other components. In addition, in the case where the above-mentioned granular polymer, water-soluble polymer and / or functional layer binding material contain crosslinking monomer units, the granular polymer, water-soluble polymer and / or functional layer binding material can be crosslinked during the drying of the slurry composition or the heat treatment arbitrarily implemented after drying (that is, the functional layer can include the crosslinked product of the above-mentioned granular polymer, water-soluble polymer and / or functional layer binding material). In addition, the preferred existence ratio of each component contained in the functional layer is the same as the preferred existence ratio of each component in the non-aqueous secondary battery functional layer slurry composition of the present invention.

[0147] Furthermore, the functional layer formed using the slurry composition of the present invention has excellent anti-blocking properties, and further, excellent electrolyte injection properties and adhesion. Therefore, if a battery component having the functional layer is used, a secondary battery with excellent electrolyte injection properties and cycle characteristics can be manufactured.

[0148] <Base material>

[0149] As a substrate for coating the slurry composition and forming a functional layer thereon, there is no particular limitation. For example, in the case of using a functional layer as a component constituting a part of a spacer, for example, a spacer substrate can be used as a substrate, and in the case of using a functional layer as a component constituting a part of an electrode, an electrode substrate formed by forming an electrode composite material layer on a current collector can be used as a substrate. In addition, the usage of the functional layer formed on the substrate is not particularly limited, for example, a functional layer can be formed on a spacer substrate, etc. and used directly as a battery component such as a spacer, a functional layer can also be formed on an electrode substrate as an electrode, and a functional layer formed on a demoulding substrate can also be temporarily peeled off from the substrate and pasted on other substrates as a battery component.

[0150] However, from the viewpoint of omitting the step of peeling the release substrate from the functional layer and improving the production efficiency of the battery member, it is preferable to use a separator substrate or an electrode substrate as the substrate.

[0151] <<Spacer base material>>

[0152] As the separator substrate, there is no particular limitation, and for example, the separator substrate described in Japanese Patent Publication No. 2012-204303 can be used. Among these, from the aspect of being able to make the overall film thickness of the separator thinner, thereby being able to increase the ratio of the electrode active material in the secondary battery and increasing the capacity per unit volume, a microporous membrane formed of a polyolefin resin (polyethylene, polypropylene, polybutylene, polyvinyl chloride) is preferred.

[0153] In addition, the spacer substrate may include any layer that can play the desired function in addition to the functional layer formed by the slurry composition of the present invention in a part thereof. For example, the spacer substrate may include a porous film layer containing heat-resistant particles and a bonding material in a part thereof, and does not contain at least one of the above-mentioned granular polymer and the water-soluble polymer. More specifically, the spacer substrate may have a porous film layer containing heat-resistant particles and a bonding material on one or both sides of the microporous film formed by the above-mentioned polyolefin resin. In addition, as the "heat-resistant particles" in the porous film layer, the heat-resistant particles exemplified in the "slurry composition for non-aqueous secondary battery functional layer" item can be used. In addition, as the "bonding material" in the porous film layer, the bonding material exemplified as the "bonding material for functional layer" in the "slurry composition for non-aqueous secondary battery functional layer" item, a known bonding material can be used.

[0154] <<Electrode base material>>

[0155] The electrode substrate (positive electrode substrate and negative electrode substrate) is not particularly limited, and examples thereof include an electrode substrate in which an electrode composite material layer is formed on a current collector.

[0156] Here, the components of the current collector, the electrode composite material layer (for example, electrode active materials (positive electrode active materials, negative electrode active materials) and binding materials for electrode composite material layers (binding materials for positive electrode composite material layers, binding materials for negative electrode composite material layers)), and the method for forming an electrode composite material layer on the current collector can use known ones, for example, those described in Japanese Patent Gazette No. 2013-145763 can be used.

[0157] Furthermore, the electrode substrate may include, in part, any layer having a desired function other than the functional layer formed from the slurry composition of the present invention (eg, the porous film layer including heat-resistant particles and a binder as described in the section "separator substrate").

[0158] <<Release base material>>

[0159] The release substrate is not particularly limited, and a known release substrate can be used.

[0160] <Method for forming functional layer>

[0161] As a method for forming a functional layer on the above-mentioned substrate such as the separator substrate and the electrode substrate, the following methods can be mentioned:

[0162] 1) A method of applying the slurry composition to the surface of a separator substrate or an electrode substrate (in the case of an electrode substrate, the surface on the electrode composite material layer side, the same below), followed by drying;

[0163] 2) A method of dipping a separator substrate or an electrode substrate into a slurry composition and then drying it;

[0164] 3) A method in which the slurry composition is applied onto a release substrate, dried to produce a functional layer, and the obtained functional layer is transferred to the surface of a separator substrate or an electrode substrate.

[0165] Among these, the method 1) is particularly preferred because it is easy to control the film thickness of the functional layer. The method 1) specifically includes a step of applying the slurry composition to a separator substrate or an electrode substrate (coating step), and a step of drying the functional layer composition applied to the separator substrate or the electrode substrate to form a functional layer (drying step).

[0166] In the coating step, the method for coating the slurry composition on the separator substrate or the electrode substrate is not particularly limited, and examples thereof include spray coating, doctor blade coating, reverse roll coating, direct roll coating, gravure printing, extrusion, and brush coating.

[0167] In the drying step, the method for drying the slurry composition on the substrate is not particularly limited, and a known method can be used, for example, drying using warm air, hot air, or low-humidity air; vacuum drying; and drying using irradiation of infrared rays, electron beams, etc. The drying conditions are not particularly limited, but the drying temperature is preferably 30 to 80° C., and the drying time is preferably 30 seconds to 10 minutes.

[0168] The thickness of the functional layer formed on the substrate is preferably 0.1 μm or more, more preferably 0.3 μm or more, further preferably 0.5 μm or more, and is preferably 3.0 μm or less, more preferably 1.5 μm or less, further preferably 1.0 μm or less.

[0169] Here, the shape of the functional layer formed on the substrate is not particularly limited, and can be formed into any top view shape such as stripe, dot, grid, etc. Among them, from the viewpoint of reducing the resistance of the secondary battery, the adhesive layer can be formed into a dot shape. The dot-shaped functional layer can be obtained by, for example, using a coater to implement an inkjet method.

[0170] The diameter of the dots of the functional layer arranged in a dot pattern is preferably 10 μm or more, more preferably 20 μm or more, preferably 300 μm or less, and more preferably 200 μm or less. If the diameter of the dots of the functional layer is above the lower limit, the adhesion between the electrode and the separator can be improved. On the other hand, if the diameter of the dots of the functional layer is below the upper limit, the deterioration of the output characteristics of the secondary battery can be suppressed.

[0171] The thickness of the dots of the functional layer arranged in a dot pattern is preferably 5 μm or more. When the thickness of the dots of the functional layer is equal to or greater than the above lower limit, the adhesive force between the electrode and the separator can be increased.

[0172] (Separator for non-aqueous secondary battery)

[0173] The spacer of the present invention has a spacer substrate and a functional layer formed by the slurry composition of the present invention on at least one surface of the spacer substrate. In addition, the spacer substrate and the functional layer constituting the spacer are the same as the spacer substrate and the functional layer described in the "functional layer" item.

[0174] Moreover, the separator of the present invention has a functional layer formed using the slurry composition of the present invention, so it has excellent anti-blocking properties before being impregnated with the electrolyte, and after being impregnated with the electrolyte, it can be well bonded to other adjacent battery components (such as electrodes) through the functional layer. In addition, the separator of the present invention can improve the electrolyte injection property of the secondary battery and enable the secondary battery to exhibit excellent cycle characteristics.

[0175] (Non-aqueous secondary battery)

[0176] The nonaqueous secondary battery of the present invention has the above-mentioned separator for the nonaqueous secondary battery of the present invention. More specifically, the nonaqueous secondary battery of the present invention has a positive electrode, a negative electrode, a separator and an electrolyte, and the above-mentioned separator is the separator for the nonaqueous secondary battery of the present invention having a separator substrate and a functional layer.

[0177] Since the nonaqueous secondary battery of the present invention includes the separator for a nonaqueous secondary battery of the present invention, it is excellent in electrolyte injection properties and cycle characteristics.

[0178] <Positive and negative electrodes>

[0179] In the secondary battery of the present invention, at least the separator has a functional layer, and the positive electrode and the negative electrode may also have functional layers respectively. As the positive electrode and the negative electrode having the functional layer, an electrode having a functional layer arranged on an electrode substrate can be used, and the above-mentioned electrode substrate is formed by forming an electrode composite material layer on a current collector. In addition, as the electrode substrate and the separator substrate, the same electrode substrate and the separator substrate as those listed in the "functional layer" item can be used.

[0180] In addition, the positive electrode and the negative electrode having no functional layer are not particularly limited, and electrodes formed of the above-mentioned electrode substrates can be used.

[0181] <Electrolyte>

[0182] As the electrolyte, an organic electrolyte in which a supporting electrolyte is dissolved in an organic solvent can generally be used. As a supporting electrolyte, a lithium salt can be used in, for example, a lithium ion secondary battery. As a lithium salt, for example, LiPF6, LiAsF6, LiBF4, LiSbF6, LiAlCl4, LiClO4, CF3SO3Li, C4F9SO3Li, CF3COOLi, (CF3CO)2NLi, (CF3SO2)2NLi, (C2F5SO2)NLi, etc. can be cited. Among them, LiPF6, LiClO4, CF3SO3Li are preferred because they are easily soluble in solvents and show a high degree of dissociation. In addition, the electrolyte can be used alone or in combination of two or more. Generally, there is a tendency that the higher the degree of dissociation of the supporting electrolyte, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted according to the type of supporting electrolyte.

[0183] As an organic solvent used in the electrolyte, there is no particular limitation as long as it can dissolve the supporting electrolyte. For example, in lithium-ion secondary batteries, preferably used are: carbonates such as dimethyl carbonate (DMC), ethylene carbonate (EC), diethyl carbonate (DEC), propylene carbonate (PC), butylene carbonate (BC), and methyl ethyl carbonate (MEC); esters such as γ-butyrolactone and methyl formate; ethers such as 1,2-dimethoxyethane and tetrahydrofuran; sulfur-containing compounds such as cyclopentane and dimethyl sulfoxide, etc. In addition, a mixture of these solvents can also be used. Among them, carbonates are preferred because of their high dielectric constant and wide stable potential region. Generally, there is a tendency that the lower the viscosity of the solvent used, the higher the lithium ion conductivity, so the lithium ion conductivity can be adjusted according to the type of solvent.

[0184] In addition, the concentration of the electrolyte in the electrolytic solution can be appropriately adjusted. In addition, a known additive can be added to the electrolytic solution.

[0185] <Method for producing non-aqueous secondary battery>

[0186] The secondary battery can be prepared, for example, by overlapping the positive electrode and the negative electrode through the separator for the non-aqueous secondary battery of the present invention, and winding, folding, etc. as needed to place them in a battery container, injecting electrolyte into the battery container, and sealing. Here, a metal mesh, a fuse, a PTC element, and other overcurrent prevention elements, a guide plate, etc. can be placed in the battery container as needed to prevent the internal pressure of the battery from rising and overcharging and discharging. The shape of the battery can be any of a coin type, a button type, a sheet type, a cylindrical type, a square type, a flat type, etc.

[0187] Example

[0188] Hereinafter, the present invention will be specifically described based on Examples, but the present invention is not limited to these Examples. In the following description, "%" and "part" indicating an amount are based on mass unless otherwise specified.

[0189] In a polymer produced by copolymerizing a plurality of monomers, the proportion of a monomer unit formed by polymerizing a certain monomer in the polymer is usually the same as the ratio (charging ratio) of the certain monomer in all monomers used for polymerization of the polymer unless otherwise specified.

[0190] In addition, in Examples and Comparative Examples, various properties were measured and evaluated according to the following methods.

[0191] <Glass transition temperature>

[0192] The aqueous dispersion of the polymer to be measured (particulate polymer, binder for the functional layer) was dried at 25° C. for 48 hours to obtain a powdery measurement sample.

[0193] 10 mg of the sample was weighed in an aluminum pan, and the differential thermal analysis measuring device (manufactured by Seiko Nanotech Co., Ltd., product name "EXSTAR DSC6220") was used to measure the temperature range of -100°C to 200°C at a heating rate of 20°C / min under the conditions specified in JIS Z8703 to obtain a differential scanning calorimetry (DSC) curve. In addition, an empty aluminum pan was used as a reference. The temperature at which the differential signal (DDSC) shows a peak during the heating process was determined as the glass transition temperature (°C). In addition, when multiple peaks were measured, the temperature shown by the peak with the largest displacement was taken as the glass transition temperature of the polymer.

[0194] <Volume average particle size>

[0195] The volume average particle size of the polymer is measured by laser diffraction. Specifically, the aqueous dispersion of the polymer adjusted to 0.1% by mass of the solid content concentration is used as a sample. Then, in the particle size distribution (volume basis) measured using a laser diffraction particle size distribution measuring device (Beckman Coulter, product name "LS-13 320"), the particle size D50 at which the cumulative volume calculated from the small particle size side becomes 50% is used as the volume average particle size.

[0196] <Weight average molecular weight>

[0197] The aqueous solution containing the water-soluble polymer prepared in the examples and comparative examples was diluted to adjust the concentration to 0.5%. Then, caustic soda was added to a pH of 10 to 12, and after soaking in a hot water bath at 80°C or above for 1 hour, it was diluted to 0.025% with the following eluent to prepare a sample. The sample was analyzed by gel permeation chromatography under the following conditions to determine the weight average molecular weight of the water-soluble polymer.

[0198] Apparatus: Gel Permeation Chromatography GPC (Equipment No. GPC-26)

[0199] Detector: Differential refractive index detector RI (manufactured by Showa Denko K.K., product name "RI-201", sensitivity 32)

[0200] Chromatographic columns: TSKgel GMPWXL 2 pieces ( Tosoh Corporation)

[0201] Solvent: 0.1M Tris buffer (pH 9, 0.1M potassium chloride added)

[0202] Flow rate: 0.7 mL / min

[0203] Column temperature: 40°C

[0204] Injection volume: 0.2mL

[0205] Standard samples: Monodisperse polyethylene oxide (PEO), polyethylene glycol (PEG) manufactured by Tosoh Corporation and Sigma-Aldrich

[0206] <Adhesion after electrolyte immersion>

[0207] A single-layer polyethylene spacer (thickness: 12 μm) manufactured by a wet process was prepared as a spacer substrate. The slurry composition prepared in the examples and comparative examples was applied to one surface of the spacer substrate, and the slurry composition on the spacer substrate was dried at 50° C. for 10 minutes to form a functional layer (coated unit area mass: 0.2 g / m 2 ). A separator having the functional layer on one side was used as an evaluation separator.

[0208] In addition, a negative electrode was produced in the same manner as in Example 1 described later, and used as a negative electrode for evaluation.

[0209] The evaluation negative electrode and the evaluation spacer obtained above were cut into rectangular shapes of 10mm×100mm respectively. Then, the negative electrode composite material layer of the negative electrode was made along the functional layer surface of the spacer to make a test piece, and was placed in a laminated packaging material together with about 400μL of electrolyte (solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) / vinyl carbonate (VC) (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 with a concentration of 1M). After 12 hours, the test piece was pressed together with the laminated packaging material at 80°C and a pressure of 1.0MPa for 10 minutes.

[0210] Afterwards, take out the test piece and wipe off the electrolyte attached to the surface. Next, the surface of the current collector side of the negative electrode of the test piece is facing down, and a transparent tape is pasted on the surface of the current collector side of the negative electrode. At this time, the transparent tape specified in JIS Z1522 is used as the transparent tape. In addition, the transparent tape is fixed on a horizontal test bench. Then, one end of the spacer is stretched vertically upward at a tensile speed of 50mm / min to measure the stress during peeling. This measurement is carried out three times, and the average value of the stress is calculated as the peel strength, which is evaluated according to the following benchmarks. The greater the peel strength, the better the adhesion of the functional layer after immersion in the electrolyte, and the more firmly the spacer and the electrode (negative electrode) can be bonded across the functional layer in the electrolyte.

[0211] A: Peel strength is 6.0N / m or more

[0212] B: Peel strength is 2.0 N / m or more and less than 6.0 N / m

[0213] C: Peel strength is 0.5 N / m or more and less than 2.0 N / m

[0214] D: Peel strength less than 0.5N / m

[0215] <Electrolyte injection properties>

[0216] An electrolyte (solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) / vinyl carbonate (VC) (volume ratio) = 68.5 / 30 / 1.5, electrolyte: LiPF6 at a concentration of 1 M) is injected into the lithium-ion secondary battery produced in the embodiments and comparative examples. Then, the interior of the lithium-ion secondary battery is depressurized to -100 kPa and maintained in this state for 1 minute. Heat sealing is then performed. Then, after 10 minutes, the electrode (positive electrode) is disassembled and the impregnation state of the electrolyte in the electrode is visually confirmed. Then, evaluation is performed using the following criteria. The more parts of the electrode that are impregnated with the electrolyte, the higher the electrolyte injection property.

[0217] A: The electrolyte impregnates all surfaces of the electrode.

[0218] B: In the electrode, the part without electrolyte is less than 1cm 2 (Except when all surfaces are impregnated).

[0219] C: 1 cm of the electrode remains without electrolyte. 2 Over and less than 2cm 2 .

[0220] D: In the electrode, 2 cm of the part not impregnated with electrolyte remains 2 above.

[0221] <Anti-blocking properties>

[0222] The same spacer as the spacer having a functional layer on one side formed in the evaluation of "adhesion after electrolyte immersion" is cut into a square of 5 cm wide × 5 cm long to obtain two square pieces. Next, the two square pieces are overlapped in such a way that the surfaces of the functional layer formed on the spacer substrate are opposite to each other, and then placed under a temperature of 40°C and a pressure of 0.1MPa for 24 hours, thereby preparing a test piece in a pressed state (pressed test piece). Then, in the pressed test piece after being placed for 24 hours, the bonding state of the two overlapping square pieces is visually confirmed, and the anti-blocking property is evaluated according to the following benchmarks. In addition, in the case where the two overlapping square pieces are bonded to each other, one of the two square pieces is fixed as a whole, and the other is stretched with a force of 0.3N / m to confirm whether the square pieces can be peeled off from each other. The less the two overlapping square pieces are bonded to each other, the better the anti-blocking property of the spacer having the functional layer.

[0223] A: The two square pieces do not stick to each other

[0224] B: Two square sheets are bonded to each other but can be separated by stretching

[0225] C: Two square sheets are bonded to each other and cannot be separated by stretching

[0226] <High temperature cycle characteristics>

[0227] After injecting the electrolyte into the secondary battery prepared in the embodiment and the comparative example, let it stand for 24 hours at 25°C. Use a caliper to measure the thickness of the battery at this time. After that, the following charge and discharge operations are performed at 25°C: charge to 4.2V (cutoff condition: 0.02C) by constant voltage constant current (CC-CV) at a charge rate of 1C, and discharge to 3.0V by constant current (CC) at a discharge rate of 1C. Furthermore, repeat the same charge and discharge operation at 45°C, and use a caliper to measure the thickness of the battery after 300 cycles. Then, the increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is evaluated as the expandability of the battery. The smaller the increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle, the better the expandability.

[0228] A: The increase in the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is less than 1%

[0229] B: The increase ratio of the thickness of the battery after the cycle relative to the thickness of the battery before the cycle is 1% or more and less than 5%

[0230] C: The thickness of the battery after the cycle increases by 5% or more relative to the thickness of the battery before the cycle

[0231] <Rate characteristics>

[0232] After injecting the electrolyte into the secondary batteries made in the examples and comparative examples, let them stand at a temperature of 25°C for 5 hours. Next, charge at a temperature of 25°C with a constant current method of 0.2C until the battery cell voltage is 3.65V, and then perform an aging treatment at a temperature of 60°C for 12 hours. Then, discharge at a temperature of 25°C with a constant current method of 0.2C until the battery cell voltage is 3.00V. After that, CC-CV charging is performed at a constant current of 0.2C (upper limit battery cell voltage 4.35V), and CC discharge is performed at a constant current of 0.2C until the battery cell voltage is 3.00V. Repeat this 0.2C charge and discharge 3 times.

[0233] Next, at a temperature of 25°C, a constant current charge and discharge of 0.2C is performed between the battery cell voltage of 4.2 and 3.00V, and the discharge capacity at this time is defined as C0. After that, CC-CV charging is performed at a constant current of 0.2C in the same manner, and discharge is performed at a constant current of 0.5C to 3.0V at a temperature of -10°C, and the discharge capacity at this time is defined as C1. Then, the capacity retention rate represented by ΔC = (C1 / C0) × 100 (%) is calculated as the rate characteristic, and evaluated according to the following criteria. The larger the value of the capacity retention rate ΔC, the lower the internal resistance, and the higher the high current discharge capacity in a low temperature environment.

[0234] A: Capacity retention rate ΔC is 70% or more

[0235] B: Capacity retention rate ΔC is less than 70%

[0236] (Example 1)

[0237] <Preparation of granular polymer>

[0238] As the particulate polymer, a polymer having a core-shell structure is prepared.

[0239] When forming the core part, 45.7 parts of styrene as an aromatic monovinyl monomer, 28.2 parts of 2-ethylhexyl acrylate as a (meth)acrylate monomer, 8.5 parts of acrylonitrile as a nitrile-containing monomer, 0.1 parts of ethylene glycol dimethacrylate as a crosslinking monomer, 2.5 parts of methacrylic acid as an acidic group-containing monomer, 0.3 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion exchange water, and 0.3 parts of potassium persulfate as a polymerization initiator were added to a 5 MPa pressure-resistant container equipped with a stirrer, and after sufficient stirring, the mixture was heated to 70° C. to initiate polymerization. The polymerization was continued until the polymerization conversion rate reached 96%, thereby obtaining an aqueous dispersion containing a particulate polymer constituting the core part. Next, in order to form the shell part, 10.0 parts of styrene as an aromatic monovinyl monomer, 4.5 parts of acrylonitrile as a nitrile group-containing monomer, and 0.5 parts of methacrylic acid as an acidic group-containing monomer were continuously added when the polymerization conversion rate reached 96%, and the polymerization was continued by heating to 70°C. When the conversion rate reached 96%, the reaction was terminated by cooling to obtain an aqueous dispersion of a granular polymer. The obtained granular polymer has a core-shell structure in which the outer surface of the core part is partially covered by the shell part.

[0240] Then, the glass transition temperature and volume average particle size of the obtained particulate polymer were measured. The results are shown in Table 1.

[0241] <Preparation of adhesive material for functional layer>

[0242] In a 5MPa pressure-resistant container with a stirrer, 62.2 parts of styrene as an aromatic monovinyl monomer, 33.0 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 3.8 parts of itaconic acid as an acidic group-containing monomer, 1 part of 2-hydroxyethyl acrylate as a hydroxyl-containing monomer, 0.4 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts by mass of ion exchange water, and 0.5 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the mixture was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the mixture was cooled to terminate the reaction and a mixture containing a polymer was obtained. After adding 5% sodium hydroxide aqueous solution to the mixture containing the polymer to adjust the pH to 8, the unreacted monomers were removed from the mixture by heating and reduced pressure distillation. After that, the mixture was cooled to below 30°C to obtain an aqueous dispersion of an adhesive material for a functional layer.

[0243] Then, the glass transition temperature of the obtained adhesive material for the functional layer was measured. The results are shown in Table 1.

[0244] <Preparation of aqueous solution containing water-soluble polymer>

[0245] 6335g of ion exchange water and 170g of 2.0% aqueous solution of L-ascorbic acid as a polymerization accelerator were added to a 10L flask with a rubber stopper, heated to a temperature of 40°C, and replaced with nitrogen at a flow rate of 100mL / min in the flask. Next, 468g (36.0% by mass) of acrylic acid as an acidic group-containing monomer, 676g (52.0% by mass) of acrylonitrile as a nitrile-containing monomer, and 156g (12.0% by mass) of 2-acrylamide-2-methylpropane sulfonic acid as a sulfonic acid-containing monomer were mixed and injected into the flask with a syringe. Afterwards, 180g of 5.0% aqueous solution of ammonium persulfate as a polymerization initiator was added to the flask with a syringe, and the reaction temperature was set to 60°C. After 2 hours, in order to further improve the reaction conversion rate, 90g of a 5.0% aqueous solution of ammonium persulfate as a polymerization initiator and 85g of a 2.0% aqueous solution of L-ascorbic acid as a polymerization accelerator were added. After another 2 hours, 90g of a 5.0% aqueous solution of ammonium persulfate as a polymerization initiator and 85g of a 2.0% aqueous solution of L-ascorbic acid as a polymerization accelerator were added. After 2 hours, 34g of a 5% aqueous solution of sodium nitrite as a reaction terminator was added to the flask and stirred. The flask was then cooled to 40°C, set to an air environment, and an 8% lithium hydroxide aqueous solution was used to make the pH in the system 8.0 to prepare an aqueous solution containing a water-soluble polymer.

[0246] <Preparation of slurry composition for non-aqueous secondary battery functional layer>

[0247] 100 parts (equivalent amount of solid content) of an aqueous dispersion of a granular polymer, 10 parts (equivalent amount of solid content) of an aqueous dispersion of a binder for a functional layer, 2 parts (equivalent amount of solid content) of an aqueous dispersion of a water-soluble polymer, and 2 parts (equivalent amount of solid content) of "NOPTEX (registered trademark) ED-052" (manufactured by SAN NOPCO Co., Ltd.) as a wetting agent are mixed in a stirring container to obtain a mixture.

[0248] The obtained mixture was diluted with ion exchange water to obtain a slurry composition (solid content concentration: 10%). The slurry composition was used to prepare a separator having a functional layer on one side, and the adhesion of the functional layer after electrolyte immersion and the anti-blocking property of the separator having the functional layer were evaluated. The results are shown in Table 1.

[0249] <Production of a spacer having functional layers on both sides>

[0250] A polyethylene microporous membrane (manufactured by Asahi Kasei Corporation, product name "ND412", thickness: 12 μm) was prepared. A ceramic slurry (manufactured by Japan Zeon Co., Ltd., product name "BM-2000M", containing alumina as heat-resistant particles and a binder) was applied to the surface of the prepared microporous membrane, and dried at a temperature of 50° C. for 3 minutes to obtain a spacer substrate having a porous membrane layer on one side (thickness of the porous membrane layer: 3 μm).

[0251] The above-mentioned non-aqueous secondary battery functional layer slurry composition was applied to the surface of the separator substrate provided with the porous membrane layer, and dried for 3 minutes at a temperature of 50° C. The same operation was performed on the other side of the separator substrate to obtain a separator having functional layers on both sides (the thickness of the functional layers: each was 0.6 μm).

[0252] <Production of negative electrode>

[0253] 33 parts of 1,3-butadiene as an aliphatic conjugated diene monomer, 3.5 parts of itaconic acid as an acidic group-containing monomer, 63.5 parts of styrene as an aromatic monovinyl monomer, 0.4 parts of sodium dodecylbenzene sulfonate as an emulsifier, 150 parts of ion exchange water, and 0.5 parts of potassium persulfate as a polymerization initiator were added to a 5MPa pressure-resistant container with a stirrer, and after sufficient stirring, the mixture was heated to 50°C to initiate polymerization. When the polymerization conversion rate reached 96%, the polymerization reaction was terminated to obtain a mixture containing a granular binder (styrene-butadiene copolymer). After adding 5% sodium hydroxide aqueous solution to the above mixture to adjust the pH to 8, the mixture was heated and distilled under reduced pressure to remove unreacted monomers. After that, the mixture was cooled to below 30°C to obtain an aqueous dispersion containing a binder for the negative electrode.

[0254] In a planetary mixer, 48.75 parts of artificial graphite (theoretical capacity: 360 mAh / g), 48.75 parts of natural graphite (theoretical capacity: 360 mAh / g), and 1 part of carboxymethyl cellulose as a thickener were added as negative electrode active materials. Furthermore, the mixture was diluted with ion exchange water in a manner such that the solid content concentration was 60%, and then kneaded at a speed of 45 rpm for 60 minutes. After that, 1.5 parts of an aqueous dispersion containing a negative electrode binder obtained as described above was added in a solid content equivalent, and kneaded at a speed of 40 rpm for 40 minutes. Then, ion exchange water was added in a manner such that the viscosity became 3000 ± 500 mPa·s (B-type viscometer, measured at 25°C and 60 rpm), thereby preparing a slurry composition for a negative electrode composite material layer.

[0255] The negative electrode composite material layer slurry composition was coated with a notch wheel coater at a coating amount of 11±0.5 mg / cm 2 The copper foil with the negative electrode composite material layer was coated on the surface of the copper foil with a thickness of 15 μm as the current collector. Then, the copper foil coated with the negative electrode composite material layer slurry composition was conveyed in an oven at a temperature of 80°C for 2 minutes at a speed of 400 mm / min, and then conveyed in an oven at a temperature of 110°C for another 2 minutes, thereby drying the slurry composition on the copper foil to obtain a negative electrode raw material having a negative electrode composite material layer formed on the current collector.

[0256] Afterwards, the negative electrode composite material layer side of the prepared negative electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 11 t (tons) to obtain a negative electrode composite material layer with a density of 1.60 g / cm 3 Then, the negative electrode was placed in an environment of temperature 25±3°C and relative humidity 50±5% for 1 week.

[0257] <Manufacturing of positive electrode>

[0258] 96 parts of Co-Ni-Mn lithium composite oxide (CellSeed (registered trademark), NMC111, LiNi) as a positive electrode active material were added to a planetary mixer. 1 / 3 Co 1 / 3 Mn 1 / 3 O2), 2 parts of acetylene black (manufactured by Denka Co., Ltd., product name "HS-100") as a conductive material, 2 parts of polyvinylidene fluoride (manufactured by Kureha Chemical Co., Ltd., product name "KF-1100") as a binder, and then N-methyl-2-pyrrolidone (NMP) as a dispersant was added to mix in a manner such that the total solid content concentration became 67% to prepare a slurry composition for a positive electrode composite material layer.

[0259] Then, the obtained slurry composition for positive electrode composite material layer was coated with a notch wheel coater at a coating amount of 20±0.5 mg / cm 2 The 20 μm thick aluminum foil was coated on the current collector.

[0260] The slurry composition on the aluminum foil was dried by conveying it in an oven at 90°C for 2 minutes at a speed of 200 mm / min and in an oven at 120°C for another 2 minutes to obtain a positive electrode raw material having a positive electrode composite material layer formed on the current collector.

[0261] Afterwards, the positive electrode composite material layer side of the prepared positive electrode raw material was rolled at a temperature of 25±3°C and a linear pressure of 14 t (tons) to obtain a positive electrode composite material layer density of 3.40 g / cm 3 Thereafter, the positive electrode was placed in an environment of a temperature of 25±3° C. and a relative humidity of 50±5% for 1 week.

[0262] <Manufacturing of secondary batteries>

[0263] The separator having functional layers on both sides, the negative electrode and the positive electrode obtained as described above were used to prepare a wound battery unit (discharge capacity equivalent to 520 mAh) and placed in an aluminum packaging material. The wound battery unit and the aluminum packaging material were pressed together at a temperature of 70°C and a pressure of 1.0 MPa using a heated flat press for 8 seconds to bond the separator to the electrodes (negative and positive electrodes).

[0264] After that, the aluminum packaging material is filled with an electrolyte. In addition, as an electrolyte, a solution prepared by dissolving LiPF6 (supporting electrolyte) at a concentration of 1 mol / liter in a mixed solvent of ethylene carbonate (EC), diethyl carbonate (DEC) and vinylene carbonate (VC) (volume ratio: EC / DEC / VC=68.5 / 30 / 1.5) is used. Furthermore, in order to seal the opening of the aluminum packaging material, the aluminum packaging material is sealed by heat sealing at a temperature of 150°C to manufacture a lithium ion secondary battery. Using the lithium ion secondary battery, the electrolyte injection properties, rate characteristics and cycle characteristics are evaluated. The results are shown in Table 1.

[0265] (Examples 2-3)

[0266] When preparing the granular polymer, the types and usage ratios of the monomers used to form the core portion were changed as shown in Table 1, and various operations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core portion was partially covered by the shell portion. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0267] (Example 4)

[0268] As the particulate polymer, a polymer not having a core-shell structure was prepared.

[0269] In a 5 MPa pressure-resistant container equipped with a stirrer, 65.5 parts of styrene as an aromatic monovinyl monomer, 24.0 parts of butyl acrylate as a (meth)acrylate monomer, 0.5 parts of ethylene glycol dimethacrylate and 10.0 parts of glycidyl methacrylate as crosslinking monomers, 0.3 parts of sodium dodecylbenzenesulfonate as an emulsifier, 150 parts of ion exchange water, and 0.3 parts of potassium persulfate as a polymerization initiator were added, and after sufficient stirring, the mixture was heated to 70° C. to initiate polymerization. The polymerization was continued until the polymerization conversion rate reached 96%, thereby obtaining an aqueous dispersion containing a particulate polymer having no core-shell structure.

[0270] Other than this, various operations, measurements, and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1.

[0271] (Example 5)

[0272] A polymer without a core-shell structure was prepared in the same manner as in Example 4 except that the preparation conditions of the granular polymer were changed so that the volume average particle size of the obtained granular polymer was 4 μm. When preparing the slurry composition, 30 parts (solid content equivalent) of the aqueous dispersion of the granular polymer obtained in this way, 3 parts (solid content equivalent) of the aqueous dispersion of the functional layer binder, 0.6 parts (solid content equivalent) of the aqueous dispersion of the water-soluble polymer, 70 parts of alumina (AKP-3000 manufactured by Sumitomo Chemical, volume average particle size D50=0.7 μm) as heat-resistant particles, and 0.2 parts (solid content equivalent) of "NOPTEX (registered trademark) ED-052" (manufactured by San Nopco Co., Ltd.) as a wetting agent were mixed in a stirring container to obtain a mixture.

[0273] The obtained mixture was diluted with ion exchange water to obtain a slurry composition (solid content concentration: 40%). The slurry composition was used to make a spacer having a functional layer on one side, and the adhesion of the functional layer after immersion in the electrolyte and the anti-blocking property of the spacer having the functional layer were evaluated. The results are shown in Table 1. In addition, using the slurry composition obtained in this way, various operations, measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 1.

[0274] (Example 6)

[0275] The various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the granular polymer prepared below was used as the binder for the functional layer.

[0276] <Manufacturing of adhesive material for functional layer>

[0277] 70 parts of ion exchange water, 0.15 parts of sodium lauryl sulfate (manufactured by Kao Chemical Co., Ltd., product name "EMAL (registered trademark) 2F") as an emulsifier, and 0.5 parts of ammonium persulfate were respectively supplied to a reactor equipped with a stirrer, the gas phase was replaced with nitrogen, and the temperature was raised to 60°C.

[0278] In another container, 50 parts of ion exchange water, 0.5 parts of sodium dodecylbenzene sulfonate as a dispersant, 79.0 parts of n-butyl acrylate as a (meth)acrylate monomer, 2.5 parts of methacrylic acid as an acidic group-containing monomer, 3.5 parts of N-hydroxymethyl acrylamide as a crosslinking monomer, and 15.0 parts of acrylonitrile as a nitrile-containing monomer were mixed to obtain a monomer composition. The monomer composition was continuously added to the above reactor over 4 hours to polymerize. During the addition, the reaction was carried out at 60°C. After the addition was completed, the reaction was terminated by further stirring at 70°C for 3 hours to prepare an aqueous dispersion containing a binder for a functional layer.

[0279] (Example 7)

[0280] The various operations, measurements, and evaluations were performed in the same manner as in Example 1, except that the granular polymer prepared below was used as the binder for the functional layer.

[0281] <Manufacturing of adhesive material for functional layer>

[0282] The composition of the monomer composition for preparing the binder for the functional layer was changed as shown in Table 1. Specifically, the amounts of n-butyl acrylate and acrylonitrile were reduced as shown in Table 1, and 15 parts of glycidyl methacrylate were added as a crosslinking monomer in addition to 3.5 parts of N-methylol acrylamide. A water dispersion containing a binder for the functional layer was prepared in the same manner as in Example 6 except for the above.

[0283] (Examples 8 to 11)

[0284] The composition of the monomer composition when preparing the water-soluble polymer was changed as shown in Table 1. Here, regarding Example 11, styrene sulfonic acid was used instead of 2-acrylamide-2-methylpropane sulfonic acid as the sulfonic acid group-containing monomer. Other than this, various operations, measurements and evaluations were carried out in the same manner as in Example 1. The results are shown in Table 1 or Table 2.

[0285] (Example 12)

[0286] The same operations, measurements and evaluations as in Example 1 were performed except that the amounts of ammonium persulfate and L-ascorbic acid were increased so that the weight average molecular weight of the water-soluble polymer would be the values ​​shown in Table 1 when preparing the water-soluble polymer.

[0287] (Example 13)

[0288] The same operations, measurements and evaluations as in Example 1 were performed except that the amounts of ammonium persulfate and L-ascorbic acid were reduced so that the weight average molecular weight of the water-soluble polymer would be the values ​​shown in Table 1 when preparing the water-soluble polymer.

[0289] (Example 14)

[0290] The results are shown in Table 2, except that polyvinyl acetate (manufactured by Techno Chemical Co., Ltd., polyvinyl acetate) as a homopolymer was used as the particulate polymer, various operations, measurements, and evaluations were performed in the same manner as in Example 1.

[0291] (Comparative Example 1)

[0292] The various operations, measurements, and evaluations were performed in the same manner as in Example 1 except that the particulate polymer was not blended.

[0293] (Comparative Example 2)

[0294] When preparing the granular polymer, the composition of the monomer composition was changed as shown in Table 2, and a granular polymer having a glass transition temperature of more than 95° C. was prepared and used. Various operations, measurements and evaluations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core portion was partially covered by the shell portion. The results are shown in Table 2.

[0295] (Comparative Example 3)

[0296] When preparing the granular polymer, the composition of the monomer composition was changed as shown in Table 2, and as the water-soluble polymer, polyacrylic acid synthesized in the same manner as in Example 1 was used by blending only acrylic acid as a monomer. Other operations, measurements and evaluations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core portion was partially covered by the shell portion. The results are shown in Table 2.

[0297] (Comparative Example 4)

[0298] When preparing the granular polymer, the composition of the monomer composition was changed as shown in Table 2, and further, the composition of the monomer composition when preparing the water-soluble polymer was changed as shown in Table 1. Other than this, various operations, measurements and evaluations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core portion was partially covered by the shell portion. The results are shown in Table 2.

[0299] (Comparative Example 5)

[0300] When preparing the granular polymer, the composition of the monomer composition was changed as shown in Table 2 so that the glass transition temperature was 20°C, and various operations were performed in the same manner as in Example 1. In addition, the obtained granular polymer had a core-shell structure in which the outer surface of the core part was partially covered by the shell part. Then, various measurements and evaluations were performed in the same manner as in Example 1. The results are shown in Table 2.

[0301] In addition, in Tables 1 and 2 shown below,

[0302] "ST" represents styrene unit,

[0303] "EDMA" means ethylene glycol methacrylate units,

[0304] "AMA" means allyl methacrylate units,

[0305] "GMA" means glycidyl methacrylate unit,

[0306] "NMA" means N-methylol acrylamide unit,

[0307] "MAA" means methacrylic acid units,

[0308] "2EHA" means 2-ethylhexyl acrylate units,

[0309] "BA" represents n-butyl acrylate unit,

[0310] "AN" stands for acrylonitrile unit,

[0311] "MMA" means methyl methacrylate units,

[0312] "IA" represents itaconic acid unit,

[0313] "BD" represents 1,3-butadiene units,

[0314] "βHEA" means 2-hydroxyethyl acrylate unit,

[0315] "AMPS" means 2-acrylamide-2-methylpropane sulfonic acid units,

[0316] "SS" represents styrene sulfonic acid units.

[0317] [Table 1]

[0318]

[0319] [Table 2]

[0320]

[0321] As can be seen from Tables 1 to 2, in Examples 1 to 14 using a slurry composition for a functional layer comprising a particulate polymer having a glass transition temperature of 30° C. to 95° C. and a water-soluble polymer having a sulfonic acid group-containing monomer unit ratio of 3% by mass or more, a functional layer with excellent anti-blocking properties and a non-aqueous secondary battery with excellent electrolyte injection properties and high-temperature cycle characteristics were obtained.

[0322] On the other hand, it can be seen that in Comparative Example 1 in which the specified granular polymer is not formulated, Comparative Examples 2 and 5 in which a granular polymer is formulated but its glass transition temperature is outside the above range, Comparative Example 3 in which the water-soluble polymer does not contain sulfonic acid group-containing monomer units, and Comparative Example 4 in which the proportion of sulfonic acid group-containing monomer units in the water-soluble polymer is less than 3% by mass, a functional layer with excellent anti-blocking properties and a non-aqueous secondary battery with excellent electrolyte injection properties and high-temperature cycle characteristics cannot be obtained.

[0323] Industrial Applicability

[0324] According to the present invention, a slurry composition for a nonaqueous secondary battery functional layer can provide a functional layer having excellent anti-blocking properties and a secondary battery having both high electrolyte injection properties and high-temperature cycle characteristics.

[0325] Furthermore, according to the present invention, it is possible to provide a separator for a nonaqueous secondary battery which can achieve both high levels of electrolyte injection properties and high-temperature cycle characteristics of the resulting secondary battery and has excellent anti-blocking properties.

[0326] Furthermore, according to the present invention, a non-aqueous secondary battery having excellent electrolyte injection properties and high-temperature cycle characteristics can be provided.

Claims

1. A slurry composition for a non-aqueous secondary battery functional layer, comprising a granular polymer and a water-soluble polymer, The particulate polymer has at least one glass transition temperature in the temperature range of 30° C. or more and 95° C. or less, and The water-soluble polymer contains a sulfonic acid group-containing monomer unit in a ratio of 3.0% by mass or more.

2. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The particulate polymer has a core-shell structure.

3. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The volume average particle size of the particulate polymer is 0.25 μm or more and 5 μm or less.

4. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The weight average molecular weight of the water-soluble polymer is 50,000 or more and 1,000,000 or less.

5. The slurry composition for a non-aqueous secondary battery functional layer according to claim 1, wherein The slurry composition for a non-aqueous secondary battery functional layer further includes heat-resistant particles.

6. A separator for a non-aqueous secondary battery, comprising a separator substrate and a functional layer formed on at least a portion of at least one surface of the separator substrate, The functional layer is a dried product of the slurry composition for a non-aqueous secondary battery functional layer according to any one of claims 1 to 5.

7. A non-aqueous secondary battery comprising a positive electrode, a negative electrode, a separator and an electrolyte, The separator is the separator for a non-aqueous secondary battery according to claim 6.