A kind of BOPP matte film and preparation method thereof

By adding long-chain branched polypropylene and polypropylene-grafted high-density polyethylene to BOPP matte film, combined with fluoropolymer additives, the problems of insufficient melt strength and die head precipitation in matte masterbatch were solved, achieving more efficient production and a more uniform matte effect.

CN118849585BActive Publication Date: 2024-11-26GUANGDONG DECRO PACKAGE FILMS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411336336.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-26
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Existing BOPP matte film suffers from insufficient melt strength of the matte masterbatch during production, making it prone to cracking and die head precipitation, resulting in low production efficiency and poor economic benefits.

Method used

By adding long-chain branched polypropylene (LCBPP) and polypropylene-grafted high-density polyethylene (PP-g-HDPE) to the matte masterbatch, and combining it with fluoropolymer PPA processing aids, the coating force of copolymer polypropylene on high-density polyethylene and the melt temperature resistance are improved, reducing melt cracking and die exudation.

Benefits of technology

It improves the melt strength and temperature resistance of matte masterbatch, reduces die head precipitation and carbonization, extends the continuous production cycle of film making, and enhances the matte uniformity and production stability of matte film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118849585B_ABST
    Figure CN118849585B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of matte films, and in particular to a BOPP matte film and a preparation method thereof. The BOPP matte film of the present invention comprises an upper surface matte layer, an intermediate core layer and a lower surface layer which are arranged in sequence; the upper surface matte layer comprises a BOPP matte masterbatch; the matte masterbatch comprises 28-50wt% copolymerized polypropylene, 30-50wt% high-density polyethylene, 5-10wt% long-chain branched polypropylene and 8-15wt% polypropylene grafted high-density polyethylene; the intermediate core layer comprises homopolymerized polypropylene. The BOPP matte film of the present invention can improve the coating force of copolymerized polypropylene on high-density polyethylene, reduce the phenomenon of melt fracture and die precipitation of matte masterbatch in the process of film preparation, and at the same time improve the temperature resistance of the matte masterbatch melt, avoid the matte masterbatch from being accumulated for a long time at the die head and carbonized, extend the continuous production cycle of film making, and improve the matte uniformity of the matte film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of matte films, in particular to a BOPP matte film and a preparation method thereof. Background Art

[0002] BOPP matte film is a packaging film with a surface similar to paper, very low gloss, high haze, and diffuse reflection matte effect. Its surface reflects weak and soft light. It is mainly used for packaging of high-end food, gifts, candies, etc., as well as printing paper for large outdoor advertisements and covers of hardcover books.

[0003] At present, in order to achieve the matt effect of BOPP matt film, the common method is to add the matt masterbatch to the matt layer and stretch it biaxially. In the matt masterbatch system, copolymerized polypropylene is the continuous phase and high-density polyethylene is the dispersed phase. According to the principle of soft-hard, high-density polyethylene (hard phase) is mostly coated by copolymerized polypropylene (soft phase). The matt principle of matt film is that during the stretching process of the matt masterbatch, because the randomness of copolymerized polypropylene is relatively high, the crystallization speed is slow, and the crystallization temperature is relatively low, but the high viscosity, high crystallization rate and high crystallinity characteristics of high-density polyethylene, when the random copolymerized polypropylene is still a relatively soft phase, the high-density polyethylene has completed part or most of the crystallization, and the crystallized high-density polyethylene becomes a hard phase. Under the external tensile force, the high-density polyethylene phase of the matt layer will bulge out during the stretching process, forming a rough and uneven matt surface layer, thereby achieving the matt effect. In the microscopic "island" form of the matt film, high-density polyethylene is an island phase, and the sea phase of polypropylene will be coated on the high-density polyethylene. However, the existing BOPP matte film still has the following shortcomings: First, the melt strength of the matte masterbatch is insufficient, which is easy to break, resulting in rapid precipitation of the die head, which makes the matte masterbatch (mainly high-density polyethylene) easily adsorbed on the metal surface of the die head; second, the temperature resistance of the matte masterbatch is insufficient, which causes the matte masterbatch adsorbed on the metal surface of the die head to accumulate, carbonize and fall off for a long time, resulting in film breakage, which will cause frequent shutdowns to clean the die head, seriously affecting the production efficiency of the production line and the economic benefits of the enterprise. Summary of the invention

[0004] Based on this, the object of the present invention is to provide a BOPP matte film and a preparation method thereof, which can improve the coating force of copolymer polypropylene on high-density polyethylene, reduce the phenomenon of matte masterbatch melt fracture and die head precipitation during film preparation, and at the same time improve the temperature resistance of the matte masterbatch melt, reduce the long-term accumulation and carbonization of the matte masterbatch at the die head, extend the continuous production cycle of film making, and improve the matte uniformity of the matte film.

[0005] A BOPP matte film comprises an upper surface matte layer, an intermediate core layer and a lower surface layer which are arranged in sequence; the upper surface matte layer comprises a BOPP matte masterbatch; the matte masterbatch comprises 28-50wt% copolymerized polypropylene, 30-50wt% high-density polyethylene, 5-10wt% long-chain branched polypropylene and 8-15wt% polypropylene grafted high-density polyethylene; the intermediate core layer comprises homopolymerized polypropylene.

[0006] The inventors have found that the following reasons exist for the melt fracture of BOPP matte masterbatch: First, the elastic effect of the matte masterbatch outlet. When the melt leaves the narrow channel of the die, extrusion expansion will occur. In the die, the melt is subjected to shear and stretching, and the molecular chains are in a certain orientation state. When the melt leaves the die, this constraint disappears, and the molecular chains will try to return to the original random curling state, causing the melt to expand at the outlet and trigger melt fracture; second, the melt strength of copolymerized polypropylene (high) does not match that of high-density polyethylene (low), resulting in insufficient coating force of copolymerized polypropylene on high-density polyethylene, severe phase separation, and melt bursting. The hard phase high-density polyethylene is easily adsorbed on the die; third, the matte masterbatch melt has wall slip inside the die, and the overall melt flow is unstable, resulting in melt fracture. Therefore, the present invention provides a BOPP matte film by improving the component formula of BOPP matte masterbatch, thereby improving the coating force of copolymerized polypropylene on high-density polyethylene, and at the same time improving the melt temperature resistance of the matte masterbatch, reducing the melt fracture of the matte masterbatch, reducing die head precipitation, reducing the long-term accumulation and carbonization of the matte masterbatch at the die head, improving the matte uniformity, and extending the continuous production cycle of film making.

[0007] Long-chain branched polypropylene (LCBPP) has a linear main chain and a branched structure with a certain length. The long branches can extend from different positions of the main chain to form a tree-like structure. The long branches of LCBPP can increase the degree of entanglement of the molecular chains, enhance the melt strength of the matte masterbatch, restrict the movement of the molecular chains, and form a physical cross-linking network in the state of the matte masterbatch melt to resist stretching and deformation. When the matte masterbatch melt is stretched, the long-chain branching makes it difficult for the molecular chains to be pulled apart, maintaining the integrity of the melt. Under higher temperatures and stresses, the LCBPP molecular chains can form a temporary three-dimensional network structure to transfer stress and enhance the overall strength of the melt. In addition, the long chain branches in LCBPP can become nucleation sites for copolymerized polypropylene, increase the crystallization nucleation density, increase the crystallization starting temperature, reduce the spherulite size, make light scattering more frequent, and enhance the extinction effect; on the other hand, it changes the phase morphology of the copolymerized polypropylene / high-density polyethylene (PP / HDPE) blend system, blurs the phase interface or forms a new microscopic phase structure, which is beneficial to the uniformity of extinction, and its long chain branch structure helps to improve the dispersibility of HDPE in copolymerized polypropylene, and can make high-density polyethylene and copolymerized polypropylene more closely combined, making light scattering more uniform and extinction more uniform. When LCBPP is added at less than 5wt%, the melt strength of the extinction masterbatch cannot be effectively improved. When LCBPP is added at more than 10wt%, on the one hand, the long chain branching structure will increase the entanglement of the molecular chain, which is not conducive to the dispersion of high-density polyethylene in copolymerized polypropylene, thereby affecting the extinction effect; on the other hand, it may cause a significant increase in the melt viscosity of the extinction masterbatch, which may make the processing process difficult, affect the fluidity and uniformity of the extinction masterbatch melt, and affect the processing and film formation.

[0008] Polypropylene grafted high-density polyethylene (PP-g-HDPE) improves the compatibility of polypropylene and high-density polyethylene through grafting. The long-chain branched structure of LCBPP helps to entangle with PP-g-HDPE during the blending process, increase physical bonding points, and form a strong interface bonding force. The present invention enhances the interaction and interface bonding force through the synergistic effect of PP-g-HDPE and LCBPP, so that HDPE is more evenly dispersed in the copolymerized polypropylene matrix to form a better microscopic phase structure, and the coating force of the copolymerized polypropylene on HDPE is increased. The HDPE segment in PP-g-HDPE can be used as a nucleation point for HDPE crystallization. PP-g-HDPE improves the compatibility of the phase interface, is conducive to uniform light scattering and extinction uniformity, reduces phase separation, and reduces the regional difference in the extinction effect of the film. The special microstructure formed by the addition of PP-g-HDPE can increase the light scattering path and uniformity, and improve the extinction uniformity. When PP-g-HDPE is added in an amount greater than 15wt%, it may lead to excessive entanglement of the molecular chains, making it difficult for the material to transmit stress when under force, significantly increasing the melt viscosity and significantly reducing the fluidity, making processing more difficult, requiring higher processing temperatures and pressures, increasing energy consumption and costs, and prone to problems such as extrusion instability. When PP-g-HDPE is added in an amount less than 8wt%, PP-g-HDPE does not significantly improve the melt strength of the matte masterbatch, and cannot effectively improve the coating of HDPE by copolymer polypropylene.

[0009] Furthermore, at 230°C and a load of 2.16kg, the melt index of the long-chain branched polypropylene is 3~5g / 10min, the melting point is 160~170°C, and the degree of branching is 0.1~0.2%. Controlling the melt index, melting point and degree of branching of LCBPP within the above range is conducive to maintaining appropriate melt strength and fluidity of the matting masterbatch, while improving the temperature resistance of the matting masterbatch. If the degree of branching is greater than 0.2%, it means that the number of grafted branches of LCBPP is large. At this time, the grafting reaction causes the entanglement between the long-chain branched structure molecular chains introduced on the polypropylene molecular chain to be too large, making it difficult for the material to transfer stress when it is stressed, the melt viscosity is greatly increased, and the fluidity is significantly reduced, which increases the difficulty of processing. If the degree of branching is less than 0.1%, the melt strength of the matting masterbatch is not significantly improved, and it is also impossible to effectively improve the coating of the copolymerized polypropylene on HDPE.

[0010] Furthermore, the preparation method of the long-chain branched polypropylene is a melt extrusion grafting method, which specifically comprises the following steps: 1wt% maleic anhydride and 98.7wt% homopolymerized polypropylene are pre-blended and then added to a barrel, 0.2wt% initiator (DCP) and 0.1wt% bridging agent (EDA) are fed from two sides of the extruder and added to a twin-screw extruder for melt extrusion, and the long-chain branched polypropylene is obtained by strand drawing, cooling, drying, pelletizing, vibrating and screening, and packaging. The preparation method can be produced continuously, greatly improving production efficiency.

[0011] Furthermore, at 230°C and a load of 2.16kg, the melt index of the polypropylene grafted high-density polyethylene is 2-4g / 10min, and the grafting rate of the high-density polyethylene in the polypropylene grafted high-density polyethylene is 0.7-0.9%. Limiting PP-g-HDPE within the above-mentioned melt index range and grafting rate range is beneficial to maintaining the matting effect and melt processing fluidity, reducing melt fracture and die head precipitation. The HDPE grafting rate of PP-g-HDPE is greater than 0.9%, and the introduction of excessive HDPE side chains greatly increases the creeping resistance of the molecular chain, which will cause the matting masterbatch melt index to be too low, which is not conducive to the processing of BOPP matting film. The HDPE grafting rate of PP-g-HDPE is less than 0.7%, which will result in the matting masterbatch melt strength not being significantly improved, and it is still unable to effectively improve the coating of copolymerized polypropylene on high-density polyethylene, the die head precipitation phenomenon is not significantly improved, and the crystallization nucleation points are reduced, which is not conducive to ensuring the matting effect.

[0012] Furthermore, the polypropylene grafted high-density polyethylene is prepared by solution group grafting reaction, comprising the following steps:

[0013] (1) PP-g-MAH and 2 times the molar amount of ethylenediamine were dissolved in xylene and reacted at 80°C for 6 hours under nitrogen protection to generate PP-g-NH2;

[0014] (2) The PP-g-NH2 and HDPE-g-MAH are dissolved in xylene and reacted at 80° C. for 6 hours under nitrogen protection to generate the polypropylene grafted high-density polyethylene with a long-chain branched structure.

[0015] The above preparation method has the advantages of high determinability of reactive groups and high reaction activity. The reactions between the groups are determinable, generally have structural designability, and the product structure is relatively clear.

[0016] Furthermore, the copolymerized polypropylene is one or more of ethylene-propylene binary copolymerized polypropylene or ethylene-propylene-butylene terpolymer; the melt index of the copolymerized polypropylene is 6-10g / 10min at 230°C and a load of 2.16kg; the melt index of the high-density polyethylene in the matte masterbatch is 12-18g / 10min at 190°C and a load of 21.6kg. High-density polyethylene and copolymerized polypropylene require a certain difference in melt index. If the difference in melt index is appropriately increased, the HDPE phase will be more likely to be an island phase, and the matte effect will be better accordingly. However, if the difference in melt index is too large, the high-density polyethylene will be difficult to disperse and will easily produce crystal points, resulting in a poor matte effect. If the difference in melt index is too small, the two phases will have better compatibility, which will reduce the haze of the matte film. The melt index of high-density polyethylene is selected as 12-18g / 10min, and the melt index of copolymerized polypropylene is selected as 6-10g / 10min, which can make the overall haze of the matte masterbatch more ideal.

[0017] Furthermore, the matte masterbatch also includes 2~3wt% PPA processing aid; the PPA processing aid is a fluorine-containing polymer. Fluorine-containing high molecular polymers have a tendency to move to the outer layer of the melt and adhere to the surface of the die head, migrate to the die head and form a lubricating layer between the matte masterbatch melt, reduce the friction between the melt and the die head during movement, and then reduce the shear rate and viscous drag of the melt in the die head, delay the occurrence of melt fracture, thereby reducing wall slip and matte masterbatch melt fracture, and achieve dynamic balance during continuous extrusion. When the dynamic balance is stable, the extrusion process and product quality will be stable. Since PPA is incompatible with polyolefins themselves, if the PPA processing aid is added in an amount greater than 3wt%, too much PPA will be accumulated on the die head, affecting the smoothness and efficiency of film production; if the PPA processing aid is added in an amount less than 2wt%, it is not conducive to forming a continuous PPA lubricating layer in and on the die head, affecting melt slip and production stability.

[0018] Furthermore, the method for preparing the matte masterbatch comprises the following steps:

[0019] (1) Adding the copolymerized polypropylene, the high-density polyethylene, the long-chain branched polypropylene, the polypropylene grafted high-density polyethylene, and the PPA processing aid in the matte masterbatch into a high-speed mixer and mixing them thoroughly;

[0020] (2) Feed the mixed material into the twin-screw extruder stably at a set flow rate, and control the extrusion temperature between 220 and 245°C for extrusion granulation;

[0021] (3) Extruding the tie rods, cooling, drying, pelletizing, vibrating and screening, and packaging to obtain the matte masterbatch.

[0022] Furthermore, the intermediate core layer also includes 0.5~1wt% antistatic agent masterbatch; the homopolypropylene of the intermediate core layer has a melt index of 2~4g / 10min at 230°C and a load of 2.16kg; the lower surface layer is a glossy layer including 99~99.5wt% homopolypropylene and 0.5~1wt% anti-blocking agent masterbatch or a matte layer including 52wt% copolymer polypropylene and 48wt% high-density polyethylene.

[0023] Furthermore, the preparation method of the BOPP matte film comprises the following steps: the raw materials of each layer are weighed in a dry condition according to a ratio and then added into each extruder, after being melted and plasticized, they are metered by a metering pump, then enter different extruder flow channels to merge and extrude at a T-die, and are cast into thick sheets by a chilled roller, first enter a longitudinal stretching zone for longitudinal stretching, and then enter a transverse stretching zone for transverse stretching to form a film, the film is air-cooled and then corona-treated, the thickness is measured and controlled by a trimming machine, and the film master roll is collected, and the film master roll is subjected to aging treatment, slitting, and packaging to obtain a finished product.

[0024] For better understanding and implementation, the present invention is described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 Schematic diagram of the structure of the BOPP matte film described in Examples 1 to 4 of the present invention. DETAILED DESCRIPTION

[0026] It should be clear that the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the embodiments of the present application.

[0027] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the embodiments of the present application. The singular forms of "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0028] When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the present application. Instead, they are only examples of devices and methods consistent with some aspects of the present application as detailed in the attached claims.

[0029] In the description of the present invention, it is necessary to understand that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "left", "right", "top", "bottom", "inside", "outside", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0030] It should be understood that the embodiments of the present application are not limited to the precise structures described above and shown in the drawings, and various modifications and changes can be made without departing from the scope thereof. The scope of the embodiments of the present application is limited only by the appended claims.

[0031] See also Figure 1 A BOPP matte film comprises an upper surface matte layer 1, an intermediate core layer 2 and a lower surface layer 3 which are arranged in sequence.

[0032] The upper surface matte layer 1 includes BOPP matte masterbatch; the matte masterbatch includes 28-50wt% copolymerized polypropylene, 30-50wt% high-density polyethylene, 5-10wt% long-chain branched polypropylene, 8-15wt% polypropylene grafted high-density polyethylene, and 2-3wt% PPA processing aid.

[0033] Furthermore, the copolymerized polypropylene is one or more of ethylene-propylene binary copolymerized polypropylene or ethylene-propylene-butylene terpolymer.

[0034] Furthermore, at 230° C. and a load of 2.16 kg, the melt index of the copolymerized polypropylene is 6 to 10 g / 10 min.

[0035] Furthermore, at 190° C. and a load of 21.6 kg, the melt index of the high-density polyethylene is 12-18 g / 10 min.

[0036] Furthermore, at 230° C. and a load of 2.16 kg, the long-chain branched polypropylene has a melt index of 3-5 g / 10 min, a melting point of 160-170° C., and a degree of branching of 0.1-0.2%.

[0037] Furthermore, the preparation method of the long-chain branched polypropylene is a melt extrusion grafting method, which specifically comprises the following steps: 1wt% maleic anhydride and 98.7wt% homopolypropylene are pre-blended and added to a barrel, 0.2wt% initiator (DCP) and 0.1wt% bridging agent (EDA) are added to a twin-screw extruder through feeding at two sides of the extruder, melt extruded at a processing temperature of 190°C, and subjected to strand drawing, cooling, drying, pelletizing, vibrating screening, and packaging to obtain the long-chain branched polypropylene. At 230°C and a load of 2.16kg, the melt index of the homopolypropylene used to prepare the long-chain branched polypropylene is in the range of 7-9g / 10min.

[0038] Furthermore, at 230° C. and a load of 2.16 kg, the melt index of the polypropylene grafted high-density polyethylene is 2-4 g / 10 min, and the grafting rate of the high-density polyethylene in the polypropylene grafted high-density polyethylene is 0.7-0.9%.

[0039] Furthermore, the polypropylene grafted high-density polyethylene is prepared by solution group grafting reaction, and the specific steps are as follows:

[0040] 1) Step 1: PP-g-MAH and 2 times the molar amount of ethylenediamine are dissolved in xylene and reacted at 80°C for 6 hours under nitrogen protection to generate PP-g-NH2.

[0041] 2) Step 2: The PP-g-NH2 and HDPE-g-MAH are dissolved in xylene and reacted at 80° C. for 6 hours under nitrogen protection to generate the polypropylene grafted high-density polyethylene with a long-chain branched structure.

[0042] The polypropylene in the PP-g-MAH is a copolymer polypropylene with high grafting activity, and its melt index range is: 6~10g / 10min (230℃, 2.16kg); the high-density polyethylene in the HDPE-g-MAH has a melt index range of 12~18g / 10min (190℃, 21.6kg).

[0043] Furthermore, the PPA processing aid is a fluorine-containing polymer.

[0044] Furthermore, the preparation method of the matte masterbatch is as follows:

[0045] (1) Add the copolymerized polypropylene, the high-density polyethylene, the long-chain branched polypropylene, the polypropylene grafted high-density polyethylene, and the PPA processing aid in the matte masterbatch into a high-speed mixer and mix them thoroughly.

[0046] (2) The mixed material is fed into the twin-screw extruder at a set flow rate and the extrusion temperature is controlled between 220 and 245 °C for extrusion granulation.

[0047] (3) Extruding the tie rods, cooling, drying, pelletizing, vibrating and screening, and packaging to obtain the matte masterbatch.

[0048] Furthermore, the intermediate core layer 2 comprises 99-99.5wt% homopolypropylene and 0.5-1wt% antistatic agent masterbatch, wherein the homopolypropylene of the intermediate core layer has a melt index of 2-4g / 10min at 230°C and a load of 2.16kg; the effective content of the antistatic agent in the antistatic agent masterbatch is 20-40wt%, and the carrier is polypropylene.

[0049] Further, the lower surface layer 3 is a smooth layer, including 99~99.5wt% homopolypropylene and 0.5~1wt% anti-blocking agent masterbatch, wherein the homopolypropylene of the lower surface layer 3 has a melt index of 2~4g / 10min at 230°C and a load of 2.16kg; the effective content of the anti-blocking agent in the anti-blocking agent masterbatch is 6wt%, the anti-blocking agent is fumed silica, D50 is 5μm, and the carrier is polypropylene; or the lower surface layer 3 is a matte layer, including 52wt% copolymer polypropylene and 48wt% high-density polyethylene.

[0050] Furthermore, the total thickness of the BOPP matte film is 15-20 μm, the thickness of the upper surface matte layer 1 is 1.4-2.0 μm, and the thickness of the lower surface layer 3 is 0.8-1.0 μm.

[0051] Furthermore, the preparation method of the BOPP matte film comprises the following steps: the raw materials of each layer are weighed in a dry condition according to a ratio and then added into each extruder, after being melted and plasticized, they are metered by a metering pump, then enter different extruder flow channels to merge and extrude at a T-die, and are cast into thick sheets by a chilled roller, first enter a longitudinal stretching zone for longitudinal stretching, and then enter a transverse stretching zone for transverse stretching to form a film, the film is air-cooled and then corona-treated, the thickness is measured and controlled by a trimming machine, and the film master roll is collected, and the film master roll is subjected to aging treatment, slitting, and packaging to obtain a finished product.

[0052] The physical properties and test methods of the embodiments or comparative examples of the present invention are as follows:

[0053] Glossiness is measured according to GB / T 10003-2008 standard, using the 45° angle method;

[0054] The haze is measured according to GB / T 10003-2008 standard;

[0055] Melt index is determined according to GB / T 3682.1-2018 standard;

[0056] The downtime interval refers to the time from the start of film production to the shutdown for die cleaning;

[0057] The matt uniformity is determined based on the haze index of the entire matt film and the quality of the film surface observed with the naked eye.

[0058] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. The proportions in the following embodiments or comparative examples are all weight percentages, and the components and contents of each layer in the embodiments of the present invention and comparative examples are shown in Table 1 below.

[0059] Table 1

[0060]

[0061] The ingredients are as follows:

[0062] Homopolymer polypropylene in the middle core layer and the lower surface layer: melt index is 3 g / 10 min.

[0063] Copolymer polypropylene: ethylene-propylene binary copolymer polypropylene, melt index is 9g / 10min.

[0064] PPA processing aid: fluorinated polymer.

[0065] Antistatic agent masterbatch: The effective component is propylene glycol monostearate, the effective content is 40wt%, and the carrier is polypropylene.

[0066] Anti-blocking agent masterbatch: fumed silica, D50 is 5μm, and the carrier is polypropylene.

[0067] Example 1

[0068] This embodiment provides a BOPP matte film, including an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to in Figure 1 .

[0069] The preparation method of each layer of resin of the BOPP matte film of this embodiment comprises the following steps:

[0070] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 5wt% long-chain branched polypropylene (melt index of 3g / 10min, melting point of 170°C, degree of branching of 0.2%), 15wt% polypropylene grafted high-density polyethylene (melt index of 4g / 10min, grafting rate of 0.7%), and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0071] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0072] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0073] The preparation method of the BOPP matte film of this embodiment comprises the following steps:

[0074] The raw materials of each layer are added to each extruder after being weighed in a dry ratio, wherein the temperatures of the extruders of the middle core layer 2 and the lower surface layer 3 are both 245°C, and the temperature of the extruder of the upper surface matte layer 1 is 240°C. The raw materials of each layer are melted and plasticized in each extruder and then metered by a metering pump, and then enter different extruder flow channels to converge and extrude at a T-die head, and are cast into thick sheets through a chilled roller, and are first preheated by longitudinal drawing, and then longitudinally stretched, with a longitudinal stretching multiple of 5 times and a longitudinal stretching temperature of 115°C. After longitudinal drawing and shaping, transverse drawing is preheated, and then transverse stretching is performed, with a transverse stretching multiple of 8 times and a transverse stretching temperature of 125°C. After the biaxial stretching of the film is completed, trimming and cutting are performed, and then corona treatment and winding are performed to obtain a BOPP matte film.

[0075] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0076] Example 2

[0077] This embodiment provides a BOPP matte film, including an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to in Figure 1 .

[0078] The preparation method of each layer of resin of the BOPP matte film of this embodiment comprises the following steps:

[0079] Preparation of the resin for the upper surface matte layer 1: 39.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 10wt% long-chain branched polypropylene (melt index of 5g / 10min, melting point of 160°C, degree of branching of 0.1%), 8wt% polypropylene grafted high-density polyethylene (melt index of 2g / 10min, grafting rate of 0.9%), and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0080] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0081] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0082] The preparation method of the BOPP matte film of this embodiment is the same as that of embodiment 1.

[0083] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0084] Example 3

[0085] This embodiment provides a BOPP matte film, including an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to in Figure 1 .

[0086] The preparation method of each layer of resin of the BOPP matte film of this embodiment comprises the following steps:

[0087] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%), 12wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%), and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0088] Preparation of the intermediate core layer 2 resin: 99 wt% homopolypropylene (melt index is 3 g / 10 min) and 1 wt% antistatic agent masterbatch are uniformly mixed to obtain the intermediate core layer 2 resin.

[0089] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0090] The preparation method of the BOPP matte film of this embodiment is the same as that of embodiment 1.

[0091] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0092] Example 4

[0093] This embodiment provides a BOPP matte film, including an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to in Figure 1 .

[0094] The preparation method of each layer of resin of the BOPP matte film of this embodiment comprises the following steps:

[0095] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%), 12wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%), and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0096] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0097] Preparation of the resin for the lower surface layer 3: 52 wt% of copolymerized polypropylene (melt index is 9 g / 10 min) and 48 wt% of high-density polyethylene (melt index is 15 g / 10 min) are uniformly mixed to obtain the resin for the lower surface layer 3.

[0098] The preparation method of the BOPP matte film of this embodiment is the same as that of embodiment 1.

[0099] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0100] Comparative Example 1

[0101] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0102] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0103] Preparation of the resin for the upper surface matte layer 1: 50 wt% copolymerized polypropylene (melt index is 9 g / 10 min), 47.5 wt% high-density polyethylene (melt index is 15 g / 10 min) and 2.5 wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0104] Preparation of the intermediate core layer 2 resin: 99.0 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 1.0 wt % antistatic agent masterbatch are uniformly mixed to obtain the intermediate core layer 2 resin.

[0105] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0106] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0107] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0108] Comparative Example 2

[0109] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0110] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0111] Preparation of the resin for the upper surface matte layer 1: 39.5wt% copolymerized polypropylene (melt index of 9g / 10min), 50wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0112] Preparation of the intermediate core layer 2 resin: 99.0 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 1.0 wt % antistatic agent masterbatch are uniformly mixed to obtain the intermediate core layer 2 resin.

[0113] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0114] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0115] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0116] Comparative Example 3

[0117] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0118] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0119] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 48wt% high-density polyethylene (melt index of 15g / 10min), 12wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0120] Preparation of the intermediate core layer 2 resin: 99.0 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 1.0 wt % antistatic agent masterbatch are uniformly mixed to obtain the intermediate core layer 2 resin.

[0121] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0122] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0123] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0124] Comparative Example 4

[0125] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0126] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0127] Preparation of the resin for the upper surface matte layer 1: 30wt% copolymerized polypropylene (melt index of 9g / 10min), 34.5wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%), 25wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0128] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0129] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0130] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0131] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0132] Comparative Example 5

[0133] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0134] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0135] Preparation of the resin for the upper surface matte layer 1: 30wt% copolymerized polypropylene (melt index of 9g / 10min), 35.5wt% high-density polyethylene (melt index of 15g / 10min), 20wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%), 12wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0136] Preparation of the intermediate core layer 2 resin: 99 wt% homopolypropylene (melt index is 3 g / 10 min) and 1 wt% antistatic agent masterbatch are uniformly mixed to obtain the intermediate core layer 2 resin.

[0137] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0138] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0139] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0140] Comparative Example 6

[0141] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0142] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0143] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 8g / 10min, melting point of 150°C, degree of branching of 0.02%), 12wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0144] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0145] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0146] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0147] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0148] Comparative Example 7

[0149] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0150] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0151] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 180°C, degree of branching of 0.5%), 12wt% polypropylene grafted high-density polyethylene (melt index of 3g / 10min, grafting rate of 0.8%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0152] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0153] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0154] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0155] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0156] Comparative Example 8

[0157] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0158] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0159] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%), 12wt% polypropylene grafted high-density polyethylene (melt index of 6g / 10min, grafting rate of 0.2%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0160] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0161] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0162] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0163] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0164] Comparative Example 9

[0165] This comparative example provides a BOPP matte film, comprising an upper matte layer 1, an intermediate core layer 2 and a lower surface layer 3 arranged in sequence. The specific structure can be referred to Figure 1 .

[0166] The preparation method of each layer of resin of the BOPP matte film of this comparative example comprises the following steps:

[0167] Preparation of the resin for the upper surface matte layer 1: 37.5wt% copolymerized polypropylene (melt index of 9g / 10min), 40wt% high-density polyethylene (melt index of 15g / 10min), 8wt% long-chain branched polypropylene (melt index of 4g / 10min, melting point of 165°C, degree of branching of 0.15%), 12wt% polypropylene grafted high-density polyethylene (melt index of 1g / 10min, grafting rate of 1.5%) and 2.5wt% PPA processing aid are uniformly mixed to obtain the resin for the upper surface matte layer 1.

[0168] Preparation of the middle core layer 2 resin: 99.5 wt % homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt % antistatic agent masterbatch are uniformly mixed to obtain the middle core layer 2 resin.

[0169] Preparation of the resin for the lower surface layer 3: 99.5 wt% of homopolymer polypropylene (melt index is 3 g / 10 min) and 0.5 wt% of anti-blocking agent masterbatch are uniformly mixed to obtain the resin for the lower surface layer 3.

[0170] The preparation method of the BOPP matte film of this comparative example is the same as that of Example 1.

[0171] The total thickness of the film is 20 µm, the thickness of the upper surface matte layer 1 is 1.5 µm, the thickness of the middle core layer 2 is 17.6 µm, and the thickness of the lower surface layer 3 is 0.9 µm.

[0172] The performance test results of the BOPP matte films of Examples 1 to 4 and Comparative Examples 1 to 9 are shown in Table 2 below.

[0173] Table 2

[0174]

[0175] From the above performance test data, we can know that:

[0176] The upper surface matt layer 1 of the BOPP matt film of Comparative Example 1 does not contain long-chain branched polypropylene (LCBPP) and polypropylene grafted high-density polyethylene (PP-g-HDPE), the high-density polyethylene is unevenly dispersed in the copolymerized polypropylene matrix, the copolymerized polypropylene has poor coating ability on the high-density polyethylene, the matt masterbatch melt is easily broken, and the die head precipitates quickly; compared with the embodiments of the present application, the matt effect and matt uniformity of the BOPP matt film of Comparative Example 1 are poor, the matt masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0177] The upper surface matt layer 1 of the BOPP matt film of Comparative Example 2 does not contain polypropylene grafted high-density polyethylene (PP-g-HDPE). Due to the lack of long-chain branched structure in the matt masterbatch, the crystallization nucleation density of the copolymerized polypropylene is small, and the dispersibility of high-density polyethylene in the copolymerized polypropylene is poor, the matt effect and the matt uniformity are affected, the copolymerized polypropylene has poor coating ability for high-density polyethylene, the matt masterbatch melt is easy to break, and the die head precipitates quickly; compared with the embodiments of the present application, the BOPP matt film of Comparative Example 2 has poor matt effect and matt uniformity, the matt masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0178] The upper surface matt layer 1 of the BOPP matt film of Comparative Example 3 does not contain long-chain branched polypropylene (LCBPP), and the high-density polyethylene has poor dispersion in the copolymerized polypropylene matrix and severe phase separation, which not only causes the matt masterbatch melt to break easily and precipitate out of the die quickly, but also affects the matt effect and matt uniformity. Compared with the embodiments of the present application, the matt effect and matt uniformity of the BOPP matt film of Comparative Example 3 are poor, the matt masterbatch accumulates and carbonizes at the die for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0179] The polypropylene grafted high-density polyethylene (PP-g-HDPE) added to the upper surface matte layer 1 of the BOPP matte film of Comparative Example 4 is greater than 15wt%, the molecular chains are excessively entangled, the melt viscosity is greatly increased, the fluidity is significantly reduced, the processing difficulty is increased, and the extrusion is unstable. Compared with the embodiments of the present application, the BOPP matte film of Comparative Example 4 has poor matte effect and matte uniformity, the matte masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0180] The long-chain branched polypropylene (LCBPP) added to the upper surface matte layer 1 of the BOPP matte film of Comparative Example 5 is greater than 10wt%, the matte masterbatch crystallizes too quickly and has a low degree of crystallinity, which affects the matte effect and matte uniformity of the matte masterbatch, increases the melt viscosity of the matte masterbatch, and makes the processing difficult; compared with the embodiments of the present application, the matte effect and matte uniformity of the BOPP matte film of Comparative Example 5 are poor, the matte masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0181] The branching degree of the long-chain branched polypropylene (LCBPP) of the upper surface matt layer 1 of the BOPP matt film of Comparative Example 6 is less than 0.1%, and the matt masterbatch has low melt strength and is easily broken, resulting in rapid precipitation at the die head. Compared with the embodiments of the present application, the matt effect and matt uniformity of the BOPP matt film of Comparative Example 6 are poor, the matt masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0182] The branching degree of the long-chain branched polypropylene (LCBPP) of the upper surface matte layer 1 of the BOPP matte film of Comparative Example 7 is greater than 0.2%, the entanglement between the long-chain branched structure molecular chains of LCBPP is too large, the melt viscosity of the matte masterbatch is increased, and the processing process becomes difficult; compared with the embodiments of the present application, the matte effect and matte uniformity of the BOPP matte film of Comparative Example 7 are poor, the matte masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0183] The grafting rate of polypropylene grafted high-density polyethylene (PP-g-HDPE) in the upper surface matt layer 1 of the BOPP matt film of Comparative Example 8 is less than 0.7%, the melt index of the matt masterbatch is too high, the coating force of the copolymerized polypropylene on the high-density polyethylene is insufficient, and the crystallization nucleation points are reduced, so the matt effect is affected; compared with the embodiments of the present application, the matt effect and matt uniformity of the BOPP matt film of Comparative Example 8 are poor, the matt masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0184] The grafting rate of polypropylene grafted high-density polyethylene (PP-g-HDPE) in the upper surface matt layer 1 of the BOPP matt film of Comparative Example 9 is greater than 0.9%, the creeping resistance of the molecular chain is greatly increased, the melt viscosity of the matt masterbatch is increased, and the processing process becomes difficult; compared with the embodiments of the present application, the matt effect and matt uniformity of the BOPP matt film of Comparative Example 9 are poor, the matt masterbatch is accumulated and carbonized at the die head for a long time, the machine is frequently shut down for cleaning, and the continuous production cycle is short.

[0185] The BOPP matte film of the present invention is prepared by adding 5-10wt% of long-chain branched polypropylene having a melt index of 3-5g / 10min (230°C, 2.16kg), a melting point of 160-170°C, and a branching degree of 0.1-0.2% and 8-15wt% of Polypropylene grafted with high-density polyethylene with a melt index of 2~4g / 10min (230℃, 2.16kg) and a HDPE grafting rate of 0.7~0.9% utilizes the synergistic effect between them to improve the coating force of copolymerized polypropylene on high-density polyethylene, and at the same time improve the melt temperature resistance of the matte masterbatch; in addition, 2~3wt% fluorine-containing polymer PPA processing aid is added; the friction between the melt and the die head during movement is reduced, and the occurrence of melt fracture is delayed, thereby reducing wall slip and melt fracture of the matte masterbatch, improving the stability of the extrusion process and product quality, thereby reducing melt fracture of the matte masterbatch, reducing die head precipitation, avoiding long-term accumulation and carbonization of the matte masterbatch at the die head, improving the matte uniformity, and extending the continuous production cycle of film making.

[0186] The above-mentioned embodiments only express several implementation methods of the present invention, and the description is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, and the present invention is also intended to include these modifications and modifications.

Claims

1. A BOPP matte film, characterized in that: The invention comprises an upper surface matte layer, an intermediate core layer and a lower surface layer which are arranged in sequence; the upper surface matte layer comprises a BOPP matte masterbatch; the matte masterbatch comprises 28-50wt% copolymerized polypropylene, 30-50wt% high-density polyethylene, 5-10wt% long-chain branched polypropylene and 8-15wt% polypropylene grafted high-density polyethylene; the intermediate core layer comprises homopolymerized polypropylene; at 230°C and a load of 2.16kg, the melt index of the long-chain branched polypropylene is 3-5g / 10min, the melting point is 160-170°C, and the degree of branching is 0.1-0.2% ...%. The melt index of the polypropylene grafted high-density polyethylene under load is 2-4 g / 10 min, and the grafting rate of the high-density polyethylene in the polypropylene grafted high-density polyethylene is 0.7-0.9%; the preparation method of the long-chain branched polypropylene is a melt extrusion grafting method, which specifically comprises the following steps: 1 wt% of maleic anhydride and 98.7 wt% of homopolypropylene are pre-blended and then added into a barrel, 0.2 wt% of an initiator DCP and 0.1 wt% of a bridging agent EDA are fed into a twin-screw extruder at two sides of the extruder for melt extrusion, and the long-chain branched polypropylene is obtained by strand drawing, cooling, drying, pelletizing, vibrating and sieving, and packaging.

2. The BOPP matte film according to claim 1, characterized in that: The polypropylene grafted high-density polyethylene is prepared by solution group grafting reaction, comprising the following steps: (1) PP-g-MAH and 2 times the molar amount of ethylenediamine were dissolved in xylene and reacted at 80°C for 6 hours under nitrogen protection to generate PP-g-NH2; (2) The PP-g-NH2 and HDPE-g-MAH are dissolved in xylene and reacted at 80° C. for 6 hours under nitrogen protection to generate the polypropylene grafted high-density polyethylene with a long-chain branched structure.

3. The BOPP matte film according to claim 1, characterized in that: The copolymer polypropylene is one or more of EPDM binary copolymer polypropylene or EPDM terpolymer; the melt index of the copolymer polypropylene is 6-10 g / 10 min at 230° C. and a load of 2.16 kg; the melt index of the high-density polyethylene in the matte masterbatch is 12-18 g / 10 min at 190° C. and a load of 21.6 kg.

4. The BOPP matte film according to any one of claims 1 to 3, characterized in that: The matte masterbatch also includes 2-3wt% PPA processing aid; the PPA processing aid is a fluorine-containing polymer.

5. The BOPP matte film according to claim 4, characterized in that: The method for preparing the matting masterbatch comprises the following steps: (1) Adding the copolymerized polypropylene, the high-density polyethylene, the long-chain branched polypropylene, the polypropylene grafted high-density polyethylene, and the PPA processing aid in the matte masterbatch into a high-speed mixer and mixing them thoroughly; (2) Feed the mixed material into the twin-screw extruder stably at a set flow rate, and control the extrusion temperature between 220 and 245°C for extrusion granulation; (3) Extruding the tie rods, cooling, drying, pelletizing, vibrating and screening, and packaging to obtain the matte masterbatch.

6. The BOPP matte film according to claim 5, characterized in that: The intermediate core layer also includes 0.5-1wt% antistatic agent masterbatch; the homopolypropylene of the intermediate core layer has a melt index of 2-4g / 10min at 230°C and a load of 2.16kg; the lower surface layer is a glossy layer including 99-99.5wt% homopolypropylene and 0.5-1wt% anti-blocking agent masterbatch or a matte layer including 52wt% copolymer polypropylene and 48wt% high-density polyethylene.

7. A method for preparing a BOPP matte film according to any one of claims 1 to 6, characterized in that: The following steps are involved: The raw materials of each layer are weighed according to the ratio and added into each extruder under dry condition. After being melted and plasticized, they are metered by a metering pump and then enter different extruder flow channels to merge and extrude at the T-die head. They are cast into thick sheets through chilled rollers, first enter the longitudinal stretching zone for longitudinal stretching, and then enter the transverse stretching zone for transverse stretching to form a film. The film is cooled by air shower and then corona treated. The thickness is controlled by a trimming machine and collected into a film mother roll. The film mother roll is subjected to aging treatment, slitting and packaging to obtain the finished product.