Copper-loaded porous silicon-carbon composite material, preparation method and battery negative electrode material
By pretreating micron silicon and metal-assisted chemical etching, a copper-loaded porous silicon-carbon composite material was prepared, which solved the problems of poor conductivity and volume expansion of silicon-based negative electrodes in lithium-ion batteries, and improved the cycle stability and stability of the battery. Conductive, extending battery life.
Patent Information
- Application Number
- CN202410907797.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-10-29
AI Technical Summary
The poor conductivity and volume expansion of silicon-based anode materials in existing lithium-ion batteries limit the cycle life and energy density of the battery, making it difficult to meet the needs of fast charging and long battery life.
By pre-treating micron silicon, metal-assisted chemical etching and carbonization, a copper-loaded porous silicon-carbon composite material is prepared, forming a uniform porous structure and a dense carbon layer to improve conductivity and structural stability.
It significantly improves the cycle stability and conductivity of the material, alleviates the impact of volume expansion on the electrode, extends the charge and discharge cycle life of lithium-ion batteries, and reduces production energy consumption.
Smart Images

Figure CN118851178A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion battery materials, and more specifically, to a porous silicon-carbon composite material loaded with copper and a preparation method thereof, and a battery negative electrode material. Background Art
[0002] Silicon as lithium-ion battery has become the most advanced battery technology in electric vehicles and stationary energy storage applications, with high energy density, power density and long life. However, the energy density of the battery still limits the driving range of electric vehicles. Therefore, in addition to optimizing safety, sustainability and cost, there is an urgent need to develop new electrode materials with higher capacity. The limited capacity of existing lithium-ion batteries is difficult to meet the growing demand. As the market demand for fast charging and long battery life of lithium batteries increases, the requirements for negative electrode materials are also increasing. Silicon is regarded as a promising negative electrode material due to its high theoretical capacity, abundant reserves, suitable price, working potential and successful application. However, silicon has a large volume change during the cycle, which is unfavorable for the cycle life and has low conductivity. Silicon-carbon composites are considered to be a technology that can solve this challenge. At present, various strategies have been adopted to improve the problem of silicon-based negative electrodes, including the use of silicon nanoparticles of different sizes and shapes to reduce the volume effect and internal pressure and improve the cycle stability. Various methods are used to prepare silicon-based composites with different structures to mitigate the impact of silicon particle volume change and stress on the electrode. Silicon-carbon composites have attracted much attention because they can effectively alleviate the volume expansion of silicon and improve conductivity and dispersibility.
[0003] The present invention provides a carbon-coated porous silicon negative electrode material, which can inhibit silicon pulverization, reduce unstable formation of SEI film, and improve structural stability, conductivity and electrochemical performance. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a porous silicon-carbon composite material loaded with copper, comprising:
[0005] Preparation of copper-loaded micronized silicon;
[0006] Etching the copper-loaded micron silicon to form porous micron silicon loaded with copper;
[0007] The copper-loaded porous micron silicon is carbonized to obtain the copper-loaded porous silicon-carbon composite material.
[0008] Furthermore, the preparation of copper-loaded micron silicon comprises:
[0009] Adding micron silicon powder into a hydrofluoric acid solution to form a first solution;
[0010] Prepare a deposition liquid of copper sulfate and disodium ethylenediaminetetraacetate, add the deposition liquid dropwise to the first solution, and obtain a precursor of copper-loaded micron silicon after centrifugation and drying;
[0011] The precursor is subjected to heat treatment to obtain the copper-loaded micron silicon.
[0012] Furthermore, the molar ratio of the micron silicon powder, copper sulfate and sodium ethylenediaminetetraacetate is 355-357:1-50:10-100.
[0013] Furthermore, the micron silicon powder needs to be pretreated before being added into the hydrofluoric acid solution. The pretreatment includes ultrasonically treating the micron silicon in a solvent and / or soaking the micron silicon in a hydrofluoric acid solution.
[0014] Furthermore, the concentration of the hydrofluoric acid solution in the first solution is 1-10M.
[0015] Furthermore, the concentration of micron silicon powder in the first solution is 5-15 g / L.
[0016] Furthermore, the concentration of the copper sulfate is 10-500 mmol / L.
[0017] Furthermore, the concentration of disodium edetate is 100-1000 mmol / L.
[0018] Furthermore, the dropping speed is 0.5 mL-3 mL / min.
[0019] Furthermore, the drying conditions are: vacuum drying, temperature 50-120°C, time 8-12h;
[0020] Furthermore, the heat treatment conditions are: after heating to 300-600°C at a heating rate of 2-30°C min-1 in an inert gas atmosphere, an inert gas / H2 mixed gas is used as a carrier gas, and the temperature is kept at 300-600°C for 0.5-3h.
[0021] Further, etching the copper-loaded micron silicon to form copper-loaded porous micron silicon comprises:
[0022] Deionized water and an organic solvent are added to the copper-loaded micron silicon, and then an etching solution is added, and then an oxidant is dripped at a constant speed, separated, and dried to obtain the copper-loaded porous micron silicon.
[0023] Furthermore, the molar ratio of the copper-loaded micron silicon to the etching solution is 1:1-1:9.
[0024] Furthermore, the value of the solution concentration of the etching solution in the reaction system divided by the sum of the solution concentrations of the etching solution and the oxidant is 0.5-0.95.
[0025] Furthermore, the etching solution is hydrofluoric acid. Preferably, the concentration of the hydrofluoric acid in the reaction system is 3-6M.
[0026] Furthermore, the oxidant is hydrogen peroxide.
[0027] Furthermore, the etching time is 0.5-6h.
[0028] Furthermore, the drying conditions are: vacuum drying, temperature 50-120° C., time 8-12 h.
[0029] Furthermore, the dropping speed of the hydrogen peroxide is 6 mL-24 mL / h.
[0030] Further, carbonizing the copper-loaded porous micron silicon comprises:
[0031] The copper-loaded porous micron silicon is placed in a tubular heat treatment furnace, and a carbon source gas is introduced to heat the furnace.
[0032] Furthermore, the carbon source gas is a carbon-containing hydrocarbon gas.
[0033] Furthermore, the heating conditions are: heating to 600-1000°C at a heating rate of 2-30°C min-1 in an inert gas atmosphere; using an inert gas / carbon source gas mixture as a carrier gas, and keeping the temperature at 600-1000°C for 1-6h.
[0034] Furthermore, the volume ratio of the inert gas to the carbon source gas in the mixed gas is 1:1-9:1.
[0035] The invention provides a porous silicon-carbon composite material loaded with copper, which is prepared by the above method.
[0036] The present invention provides a battery negative electrode material, comprising the above-mentioned copper-loaded porous silicon-carbon composite material.
[0037] Beneficial effects of this patent:
[0038] 1) Pretreatment of micron silicon can remove organic matter and oxide layer on the surface of micron silicon, thereby increasing the loading sites of copper metal particle catalyst.
[0039] 2) Micron silicon can be uniformly deposited with nano-metal particles and porous etching through a controllable two-step copper metal-assisted chemical etching, providing a method for preparing uniform porous silicon. The reduction of copper ions reduces the aggregation of copper particles, controls the particle size, and makes the porous silicon etching effect better.
[0040] 3) The porous silicon material prepared by the metal-assisted chemical etching method has a porous structure. This structure provides an effective buffer for volume expansion, thereby improving the cycle stability of the material. At the same time, the insertion of metal copper nanoparticles can increase the conductivity of the composite material, significantly reduce the bulk resistance of micron silicon, and promote the transmission and diffusion of lithium ions.
[0041] 4) The deposited copper metal particles themselves have a catalytic effect. They can provide a catalytic effect for the formation of amorphous carbon in the high-temperature chemical vapor deposition process of the particles, reduce the reaction temperature, thereby reducing the activation temperature or activation time and reducing production energy consumption.
[0042] 5) The present invention uses chemical vapor deposition technology to successfully coat a dense and uniform carbon layer on the surface of the porous silicon-carbon material. The carbon layer acts as a binder and can effectively combine micron silicon and copper metal particles to improve the structural stability of the composite material. At the same time, this carbon layer also has excellent electrochemical properties, acting as an electrolyte barrier in lithium-ion batteries, reducing side reactions at the interface between liquid electrolytes and electrodes, forming a stable solid electrolyte layer to stabilize the electrodes and improve long-term cycle performance. The carbon layer works synergistically with the metal particles to improve the conductivity of the material and promote the transmission capacity of lithium ions. Compared with traditional solid / liquid coating methods, chemical vapor deposition has the advantages of high density and good consistency, which can improve the efficiency of the material.
[0043] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures particularly pointed out in the description, claims, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] The accompanying drawings are used to provide a further understanding of the technical solution of the present invention and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of the present invention and do not constitute a limitation on the technical solution of the present invention.
[0045] Figure 1 a and b are scanned images of micron silicon, porous silicon loaded with copper (i.e., porous silicon / copper), and porous silicon-carbon composite material loaded with copper, respectively, in Example 1;
[0046] Figure 2 is a STEM image of the copper-loaded porous silicon in Example 1;
[0047] Figure 3 a and b are nitrogen adsorption-desorption curves and pore size distribution diagrams of micron silicon, copper-loaded porous silicon and copper-loaded porous silicon-carbon composite material in Example 1, respectively;
[0048] Figure 4 The black curve and the red curve are respectively infrared curves of the micron silicon and the porous silicon-carbon composite material loaded with copper in Example 2;
[0049] Figure 5 1 is the cyclic voltammetry curve of the porous silicon-carbon composite material loaded with copper in Example 2;
[0050] Figure 6 The first week charge-discharge curve of the copper-loaded porous silicon-carbon composite material prepared in Example 2;
[0051] Figure 7 Long cycle performance diagram of micron silicon, porous silicon / copper and porous silicon-carbon composite material loaded with copper prepared in Example 3;
[0052] Figure 8 This is a magnification diagram of the copper-loaded porous silicon-carbon composite material prepared in Example 3;
[0053] Fig. 9 These are the EIS graphs of the micron silicon, porous silicon / copper and porous silicon-carbon composite materials loaded with copper prepared in Example 3. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical solution and advantages of the embodiment of the present invention clearer, the technical solution of the embodiment of the present invention will be clearly and completely described in conjunction with the appendix of the specific embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, not all of the embodiments. Based on the described embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] The present invention provides a method for preparing a porous silicon-carbon composite material loaded with copper, comprising:
[0056] Step 1: preparing copper-loaded micron silicon;
[0057] Step 2: etching the copper-loaded micron silicon to form porous micron silicon loaded with copper;
[0058] Step 3: Carbonizing the copper-loaded porous micron silicon to obtain the copper-loaded porous silicon-carbon composite material.
[0059] In another embodiment of the present invention, the step 1 of preparing the copper-loaded micron silicon comprises:
[0060] Add micron silicon powder (preferably 1-10 μm in size) into a hydrofluoric acid solution (commercial hydrofluoric acid can be selected, generally with a mass fraction of 40 wt.%) to form a first solution (the concentration of hydrofluoric acid in the reaction system formed by hydrofluoric acid and silicon powder is 1-10 M, preferably 5 M; the concentration of silicon powder is 5-15 g / L);
[0061] Dissolve copper sulfate and disodium ethylenediaminetetraacetate in an aqueous solution to form a deposition solution, wherein the concentration of copper sulfate in the deposition solution is 10-500mmol / L, and the concentration of disodium ethylenediaminetetraacetate is 100-1000mmol / L (the specific method is: weigh copper sulfate and disodium ethylenediaminetetraacetate according to the predetermined concentration, and add them to a clean beaker. Then, slowly add water to form a uniform precipitate). Add the deposition solution dropwise (the dropping speed is 0.5mL-3mL / min) to the first solution to promote uniform deposition of copper metal. After the deposition is completed, centrifuge the deposited micron silicon powder to remove the first step deposition solution, and then dry it in a vacuum drying oven at 50-120°C for 8-12h; then, in an inert gas atmosphere (wherein, inert gas refers to argon, nitrogen, and other gases that do not react with the reactants) at 2-10°C min -1 After heating to 300-600°C at a heating rate of 1:1, an inert gas / H2 (wherein the volume ratio of the inert gas to the hydrogen is 1:1 to 9:1, and the gas flow rate is 50-120 sccm) mixed gas is used as a carrier gas, and the temperature is kept at 300-600°C for 0.5-3h. After the reaction is completed, it is naturally cooled to room temperature to obtain the copper-loaded micron silicon.
[0062] In another embodiment of the present invention, the molar ratio of the micron silicon powder, copper sulfate and sodium ethylenediaminetetraacetate is 355-357:1-50:10-100.
[0063] In another embodiment of the present invention, etching the copper-loaded micron silicon to form copper-loaded porous micron silicon comprises:
[0064] Add deionized water and an organic solvent (including but not limited to anhydrous ethanol, methanol and acetone, etc., as long as the micron silicon can be dispersed) to the copper-loaded micron silicon, then add an etching solution, and then drip an oxidant at a constant rate for an etching time of 0.5-6 hours, separate and dry to obtain the copper-loaded porous micron silicon.
[0065] The oxidant drop rate is 6-24 mL / h. If the drop rate is too fast, the boiling phenomenon will occur and the experiment cannot be carried out. If the time is too long, the etching efficiency will be low.
[0066] The molar ratio of the copper-loaded micron silicon to the etching solution is 1:1-1:9.
[0067] The micron silicon of the present application can achieve uniform surface deposition of nano-metal particles and porous etching through controllable two-step copper metal-assisted chemical etching. The first step is reduction, and then a deposition solution (disodium ethylenediaminetetraacetic acid and copper sulfate solution) and a hydrofluoric acid solution are added, copper is self-deposited, and at the same time, the nano-copper particles are equivalent to catalysts to etch the micron silicon; the second step is etching, and an etching solution (hydrofluoric acid) is added. Since there is copper in the first step, the nano-copper particles are equivalent to catalysts, which accelerate the reaction speed and the etching rate for the silicon loaded with copper and the copper particles. The addition of an oxidant, hydrogen peroxide, further accelerates the reaction rate.
[0068] In another embodiment of the present invention, the etching solution is hydrofluoric acid.
[0069] In another embodiment of the present invention, the oxidant is hydrogen peroxide.
[0070] In another embodiment of the present invention, the concentration of HF (commercial hydrofluoric acid is generally used, with a mass fraction of 40wt.%) in the reaction system (referring to a reaction system comprising deionized water, an organic solvent, an etching solution and an oxidant) is 3-6M, and P is 0.5-0.95, wherein P=HF solution concentration / (HF solution concentration+H2O2 solution concentration) (herein, the HF and H2O2 solution concentrations both refer to the solution concentrations in the reaction system).
[0071] In another embodiment of the present invention, the drying conditions are: vacuum drying, temperature 50-120° C., time 8-12 h.
[0072] In another embodiment of the present invention, the etching time is 0.5-6h.
[0073] In another embodiment of the present invention, the dropping speed of the hydrogen peroxide is 6 mL-24 mL / h.
[0074] In another embodiment of the present invention, carbonizing the copper-loaded porous micron silicon comprises:
[0075] The copper-loaded porous micron silicon is placed in a tubular heat treatment furnace, and a carbon source gas is introduced to heat the furnace.
[0076] In another embodiment of the present invention, the carbon source gas is a carbon-containing hydrocarbon gas (including but not limited to methane, ethane, propane, acetylene, etc.).
[0077] In another embodiment of the present invention, the heating conditions are: heating to 600-1000°C at a heating rate of 2-30°C min-1 in an argon atmosphere; using an inert gas / carbon source gas mixture as a carrier gas, keeping warm at 600-1000°C for 1-6h; switching to argon after the reaction is completed, and naturally cooling to room temperature to obtain a porous micron silicon-carbon composite material loaded with copper.
[0078] In another embodiment of the present invention, the volume ratio of the inert gas to the carbon source gas in the mixed gas is 1:1-9:1, preferably 4:1.
[0079] In another embodiment of the present invention, the gas flow rate of the gas is 50-120 sccm.
[0080] In another embodiment of the present invention, the micron silicon powder needs to be pretreated before being added to the hydrofluoric acid solution, and the pretreatment includes placing the micron silicon in an acetone solvent for ultrasonic treatment for 0.5-3 hours to remove organic matter on the surface of the micron silicon. Subsequently, immersing the micron silicon in a 1-10M hydrofluoric acid (HF) solution for 1-3 hours to remove the surface oxide layer, and finally washing with water and drying at 50-120°C to obtain the micron silicon powder.
[0081] In another embodiment of the present invention, a porous silicon-carbon composite material loaded with copper is provided, which is prepared by any of the above methods.
[0082] In another embodiment of the present invention, a battery negative electrode material is provided, comprising the above-mentioned copper-loaded porous silicon-carbon composite material.
[0083] Example 1
[0084] 1. The preparation of the porous silicon-carbon composite material is carried out according to the following steps:
[0085] 1) Pretreatment of micron silicon
[0086] 1g of micron silicon (1-10μm) was placed in an acetone solvent for ultrasonic treatment for 1h to remove organic matter on the surface of the micron silicon. Subsequently, it was soaked in a 5M hydrofluoric acid (HF) solution for 3h to remove the surface oxide layer, and finally washed with water and dried at 60°C to obtain the micron silicon raw material.
[0087] 2) Precursor of micron silicon loaded with copper
[0088] Add the treated micron silicon powder to a 5M hydrofluoric acid (HF) solution (add 23.5mL of 40% hydrofluoric acid by mass, mix it with water and ethanol to form a 100mL solution, and ensure that the hydrofluoric acid concentration is 5M.). Prepare 50mL of 100mmol / L copper sulfate and 200mmol / L disodium ethylenediaminetetraacetic acid deposition solution, and then add 5mL of deposition solution to the hydrofluoric acid solution added to the silicon powder at a constant rate of 1mL / min to promote uniform deposition of copper metal. After the deposition is completed, the deposited micron silicon powder is centrifuged to remove the first step deposition solution, and then dried in a vacuum drying oven at 60°C for 10h to obtain a precursor of micron silicon loaded with copper.
[0089] 3) Preparation of size-controlled copper-loaded micron silicon
[0090] The micron silicon precursor powder obtained in (2) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. After heating to 450°C at a heating rate of 5°C min-1 in an argon atmosphere, an Ar / H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to H2 was 4:1 and the gas flow rate was 100 sccm), and the temperature was kept at 450°C for 1 hour. After the reaction was completed, it was naturally cooled to room temperature to obtain a copper-loaded micron silicon material.
[0091] 4) Preparation of copper-loaded porous silicon
[0092] The copper-loaded micron silicon powder obtained in (3) was transferred to a beaker and added with 53.9 mL of deionized water and 15 mL of anhydrous ethanol, and 23.5 mL of hydrofluoric acid with a mass fraction of 40 wt.% was added, and the hydrofluoric acid concentration of the reaction system was 5 M. Then, 7.6 mL of an oxidant (hydrogen peroxide with a mass fraction of 30 wt.%) was added dropwise at a constant rate of 12 mL / h, and the hydrogen peroxide concentration of the reaction system was 0.75 M. After 2 hours of dropwise addition, the copper-loaded micron silicon powder was separated from the etching solution by centrifugal separation. The copper-loaded porous silicon material was dried at 60°C in a vacuum drying oven for 10 hours to obtain a copper-loaded porous silicon material, which was recorded as P-Si / Cu.
[0093] 5) Preparation of porous silicon-carbon composite materials loaded with copper
[0094] The copper-loaded porous silicon material powder obtained in (4) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. It was heated to 650°C at a heating rate of 5°C min-1 in an argon atmosphere, and then acetylene was used as a carbon source, and an Ar / C2H2 mixed gas (wherein the volume ratio of Ar to C2H2 was 4:1 and the gas flow rate was 100 sccm) was used as a carrier gas. At the same time, it was kept at 650°C for 3 hours. After the reaction was completed, it was naturally cooled to room temperature, and the black powder was taken out for use to obtain a copper-loaded porous silicon-carbon composite material, which was recorded as a copper-loaded porous silicon-carbon composite material.
[0095] 2. Battery assembly
[0096] The lithium storage performance test of the copper-loaded porous silicon-carbon composite material uses a 2032-type button half-cell. The negative electrode sheet uses a copper-loaded porous silicon-carbon composite material as the active material, acetylene black as the conductive agent, and sodium carboxymethyl cellulose (CMC) as the binder. The three are dispersed in deionized water in a mass ratio of 7:1.5:1.5 to form a slurry. The slurry is evenly coated on the copper foil and dried in a vacuum drying oven at 60°C for 12 hours. The button cell assembly is completed in an argon glove box, and a lithium sheet is used as the electrode. The electrolyte is 1M lithium hexafluorophosphate (LiPF6) dissolved in a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) with a volume ratio of 1:1 (EC:DEC=1:1, v / v), and 3% volume fraction of fluoroethylene carbonate (FEC) is added as an electrolyte additive. The separator is Celgard 2500, and its thickness is 25μm.
[0097] 3. Battery test
[0098] (1) Cyclic voltammetry curves of porous silicon-carbon composites loaded with copper
[0099] The experiment used an electrochemical workstation (CHI 660D) for cyclic voltammetry testing. The scan rate was 0.1mVs-1 and the scan range was 0.01-1.0V. During the test, the working electrode (WE) was connected to the electrode on the active material side, and the counter electrode (CE) and reference electrode (RE) were connected to the electrode on the lithium sheet side. Three scans were performed.
[0100] Electrochemical Impedance Spectroscopy of Copper-Loaded Porous Silicon-Carbon Composites
[0101] The experiment used an electrochemical workstation (CHI 420D) for cyclic voltammetry testing. The scan rate was 0.1mVs-1 and the scan range was 0.01~1.0V. During the test, the working electrode (WE) was connected to the electrode on the active material side, and the counter electrode (CE) and reference electrode (RE) were connected to the electrode on the lithium sheet side. Three scans were performed.
[0102] (2) Charge and discharge curves of the first week of porous silicon-carbon composite material loaded with copper
[0103] After sealing the assembled button cell, let it stand for a period of time, and then connect it to the Blue Electric charge and discharge tester for constant current charge and discharge test. The charge and discharge cut-off voltage range of the button cell is 0.005V~1.0V. The test steps include standing, constant current discharge, constant current charging, and constant voltage charging, and each cycle is a complete cycle. After the battery completes the first week of cycling, the Blue Electric monitoring system will display the first week charge and discharge capacity, voltage, and coulomb efficiency of the porous silicon composite material. The first week charge and discharge data can be exported and graphed to obtain the first week charge and discharge capacity and the first week coulomb efficiency.
[0104] (3) Cycling performance and rate performance curves of porous silicon-carbon composites loaded with copper
[0105] After the assembled button cell is sealed, after a certain period of standing, it is connected to the Blue Electric charge and discharge tester for constant current charge and discharge test. The charge and discharge cut-off voltage range of the button cell is 0.01V~1.0V. The weekly cycle includes five steps: standing, constant current discharge, constant current charging, constant voltage charging and cycling. In the first five weeks, a small current (200mAh g-1) is used for charge and discharge tests for activation. After the first five weeks, a large current (500mAh g-1) is used for cycle tests to evaluate the long cycle performance and stability of the material. The rate performance test steps are as above. The battery is charged and discharged at 0.2A g-1, 0.5A g-1, 1A g-1, 2A g-1, and 4A g-1 for 5 cycles of constant current, and after the high rate test, a constant current charge and discharge test is performed at 0.2A g-1.
[0106] 4. The experimental results are as follows:
[0107] Figure 1 Figures a, b, and c are SEM images of micron silicon, porous silicon / copper, and porous silicon-carbon composite materials. By comparison, the porous structure of micron silicon can be clearly seen. The surface of micron silicon is smooth, without porous structure, with a particle size range of 1-3μm and irregular shape. Figure 1 -b shows the SEM image of the prepared porous silicon / copper composite material. From the scanning image, we can see that there are many nanopores on the surface of the porous silicon / copper composite material. In addition, Figure 1 -c is a porous silicon-carbon composite material, which is obtained by calcining at 650°C using acetylene gas as the carbon source. A uniform carbon layer is formed on the surface, while the porous structure disappears, leaving only partial etching traces.
[0108] Figure 2 This is a STEM image of porous silicon / copper. It can be observed that a porous structure is formed and metallic copper particles are loaded on the structure.
[0109] Figure 3 a and b in the figure are nitrogen adsorption-desorption curves and pore size distribution diagrams of micron silicon, porous silicon / copper and porous silicon-carbon composite materials, respectively. The specific surface areas of micron silicon, porous silicon / copper and porous silicon-carbon composite materials are 22.456, 41.478 and 96.213 m2 / g, respectively. By comparison, it is found that after metal-assisted chemical etching, porous silicon is formed and the surface of the particles becomes rough, which increases the specific surface area of porous silicon to a certain extent. This can also be verified in the previous scanning electron microscope images and transmission electron microscope images. However, the reduction in the specific surface area of the porous silicon-carbon composite material is due to chemical vapor deposition, which generates a dense carbon layer on the surface of micron silicon, indicating that the carbon layer reduces the surface area of the composite material in the composite material.
[0110] The porous silicon-carbon composite material was used as the negative electrode active material to assemble a 2032-type button-type half-cell, with a first-week discharge capacity of 2565.5mAh g-1, a charge capacity of 1944.6mAh g-1, and a coulombic efficiency of 75.8%. After 200 cycles at a current density of 500mA g-1, the reversible capacity was still 1710.5mAh g-1, and the capacity retention rate was 76.5%, showing good electrochemical stability.
[0111] Example 2
[0112] 1. The preparation of the porous silicon-carbon composite material is carried out according to the following steps:
[0113] 1) Pretreatment of micron silicon
[0114] 1g of micron silicon (1-10μm) was placed in an acetone solvent for ultrasonic treatment for 1h to remove organic matter on the surface of the micron silicon. Subsequently, it was soaked in a 5M hydrofluoric acid (HF) solution for 3h to remove the surface oxide layer, and finally washed with water and dried at 60°C to obtain the micron silicon raw material.
[0115] 2) Micronized silicon loaded with copper
[0116] Add the treated micron silicon powder to a 5M hydrofluoric acid (HF) solution (when preparing this solution, first add 23.5mL of 40% hydrofluoric acid by mass, then add water and ethanol to mix, and finally form a 100mL solution, ensuring that the hydrofluoric acid concentration is 5M.). Prepare 50mL of a deposition solution of 50mmol / L copper sulfate and 200mmol / L disodium ethylenediaminetetraacetate, and then drop 5mL of the deposition solution at a constant rate of 1mL / min to promote uniform deposition of copper metal. After the deposition is completed, centrifuge the deposited micron silicon powder to remove the first step deposition solution, and then dry it in a vacuum drying oven at 60°C for 10h to obtain copper-loaded micron silicon.
[0117] 3) Preparation of size-controllable copper-loaded micron silicon.
[0118] The micron silicon powder obtained in (2) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. After heating to 500°C at a heating rate of 5°C min-1 in an argon atmosphere, an Ar / H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to H2 was 5:1 and the gas flow rate was 100 sccm), and the temperature was kept at 500°C for 2 hours. After the reaction was completed, it was naturally cooled to room temperature to obtain a copper-loaded micron silicon material.
[0119] 4) Preparation of porous silicon
[0120] The copper-loaded micron silicon powder obtained in (3) was transferred to a beaker and added with 53.7 mL of deionized water and 15 mL of anhydrous ethanol, and 23.5 mL of hydrofluoric acid with a mass fraction of 40 wt.% was added, and the hydrofluoric acid concentration of the reaction system was 5 M. Then, 12.2 mL of hydrogen peroxide with a mass fraction of 30 wt.% as an oxidant was added dropwise at a constant rate of 12 mL / h, and the hydrogen peroxide concentration of the reaction system was 1.25 M. After the addition was continued for 1 hour, the micron silicon powder was separated from the etching solution by centrifugal separation. The porous silicon material obtained after drying at 60°C in a vacuum drying oven for 10 hours was recorded as P-Si / Cu.
[0121] 5) Preparation of porous silicon-carbon composite materials
[0122] The porous silicon material powder obtained in (4) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. It was heated to 700°C at a heating rate of 5°C min-1 in an argon atmosphere, and then acetylene was used as a carbon source and an Ar / C2H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to C2H2 was 4:1 and the gas flow rate was 100 sccm). At the same time, it was kept at 700°C for 3 hours. After the reaction was completed, it was naturally cooled to room temperature, and the black powder was taken out for use to obtain a porous silicon-carbon composite material, which was recorded as a porous silicon-carbon composite material.
[0123] 2. Battery assembly
[0124] Same as Example 1.
[0125] 3. Battery test
[0126] Same as Example 1.
[0127] 4. The experimental results are as follows:
[0128] The porous silicon-carbon composite material was used as the negative electrode active material to assemble a 2032-type button-type half-cell, with a first-week discharge capacity of 2378.3mAh g-1, a charge capacity of 1812.3mAh g-1, and a coulombic efficiency of 76.2%. After 200 cycles at a current density of 500mA g-1, the reversible capacity was still 1656.4mAh g-1, showing good electrochemical stability.
[0129] Example 3
[0130] 1. The preparation of the porous silicon-carbon composite material is carried out according to the following steps:
[0131] 1) Pretreatment of micron silicon
[0132] 1g of micron silicon (1-10μm) was placed in an acetone solvent for ultrasonic treatment for 1h to remove organic matter on the surface of the micron silicon. Subsequently, it was soaked in a 5M hydrofluoric acid (HF) solution for 3h to remove the surface oxide layer, and finally washed with water and dried at 60°C to obtain the micron silicon raw material.
[0133] 2) Micronized silicon loaded with copper
[0134] The treated micron silicon powder is added to 100 ml of 5M hydrofluoric acid (HF) solution (the method is the same as in Example 1). 50 mL of a deposition solution of 100 mmol / L copper sulfate and 300 mmol / L disodium ethylenediaminetetraacetate is prepared, and then 5 mL of the deposition solution is added dropwise at a constant rate of 1 mL / min to promote uniform deposition of copper metal. After the deposition is completed, the deposited micron silicon powder is centrifuged to remove the first step deposition solution, and then dried in a vacuum drying oven at 60° C. for 10 hours to obtain copper-loaded micron silicon.
[0135] 3) Preparation of size-controllable copper-loaded micron silicon.
[0136] The micron silicon powder obtained in (2) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. After heating to 350°C at a heating rate of 5°C min-1 in an argon atmosphere, an Ar / H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to C2H2 was 4:1 and the gas flow rate was 100 sccm), and the temperature was kept at 350°C for 2 hours. After the reaction was completed, it was naturally cooled to room temperature to obtain a copper-loaded micron silicon material.
[0137] 4) Preparation of porous silicon
[0138] The copper-loaded micron silicon powder obtained in (3) was transferred to a beaker and added with 39.8 mL of deionized water and 15 mL of anhydrous ethanol. 23.5 mL of hydrofluoric acid with a mass fraction of 40 wt.% was added, and the hydrofluoric acid concentration of the reaction system was 5 M. Then, 21.7 mL of hydrogen peroxide with a mass fraction of 30 wt.% as an oxidant was added dropwise at a constant rate of 12 mL / h, and the hydrogen peroxide concentration of the reaction system was 2.14 M. After 0.5 h of the addition, the micron silicon powder was separated from the etching solution by centrifugation. The porous silicon material obtained after drying at 60°C in a vacuum drying oven for 10 h was recorded as P-Si / Cu.
[0139] 5) Preparation of porous silicon-carbon composite materials
[0140] The porous silicon material powder obtained in (4) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. It was heated to 650°C at a heating rate of 5°C min-1 in an argon atmosphere, and then acetylene was used as a carbon source and an Ar / C2H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to C2H2 was 4:1 and the gas flow rate was 100 sccm). At the same time, it was kept at 650°C for 4 hours. After the reaction was completed, it was naturally cooled to room temperature, and the black powder was taken out for use to obtain a porous silicon-carbon composite material, which was recorded as a porous silicon-carbon composite material.
[0141] 2. Battery assembly
[0142] Same as Example 1.
[0143] 3. Battery test
[0144] Same as Example 1.
[0145] 4. The experimental results are as follows:
[0146] A 2032-type button-type half-cell was assembled using this porous silicon-carbon composite material as the negative electrode active material. Its first-week discharge capacity was 2435.6 mAh g-1, the charging capacity was 1758.5 mAh g-1, the coulombic efficiency was 72.2%, and the capacity retention rate after 200 cycles was 71.6%, showing good electrochemical stability.
[0147] Example 4
[0148] 1. The preparation of the porous silicon-carbon composite material is carried out according to the following steps:
[0149] 1) Pretreatment of micron silicon
[0150] 1g of micron silicon (1-10μm) was placed in an acetone solvent for ultrasonic treatment for 2h to remove organic matter on the surface of the micron silicon. Subsequently, it was soaked in a 1M hydrofluoric acid (HF) solution for 5h to remove the surface oxide layer, and finally washed with water and dried at 50°C to obtain the micron silicon raw material.
[0151] 2) Micronized silicon loaded with copper
[0152] The treated micron silicon powder is added to 100 ml of 1M hydrofluoric acid (HF) solution (the method is the same as in Example 1). 50 mL of a deposition solution of 10 mmol / L copper sulfate and 100 mmol / L disodium ethylenediaminetetraacetate is prepared, and then 5 mL of the deposition solution is added dropwise at a constant rate of 0.5 mL / min to promote uniform deposition of copper metal. After the deposition is completed, the deposited micron silicon powder is centrifuged to remove the first step deposition solution, and then dried in a vacuum drying oven at 50°C for 12 hours to obtain copper-loaded micron silicon.
[0153] 3) Preparation of size-controllable copper-loaded micron silicon.
[0154] The micron silicon powder obtained in (2) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. After heating to 300°C at a heating rate of 2°C min-1 in an argon atmosphere, an Ar / H2 mixed gas was used as a carrier gas (the volume ratio of Ar and H2 was 1:1), and the temperature was kept at 300°C for 3 hours. After the reaction was completed, it was naturally cooled to room temperature to obtain a copper-loaded micron silicon material.
[0155] 4) Preparation of porous silicon
[0156] The micron silicon powder obtained in (3) was transferred to a beaker and added with 30 mL of deionized water and 15 mL of anhydrous ethanol. 23.59 mL of hydrofluoric acid with a mass fraction of 40 wt.% was added, and the concentration of hydrofluoric acid in the reaction system was 5 M. Then, 31.5 mL of hydrogen peroxide with a mass fraction of 30 wt.% as an oxidant was added dropwise at a constant rate of 12 mL / h, and the concentration of hydrogen peroxide in the reaction system was 3.05 M. After the addition was continued for 1 hour, the micron silicon powder was separated from the etching solution by centrifugation. The porous silicon material obtained after drying at 50°C in a vacuum drying oven for 12 hours was recorded as P-Si / Cu.
[0157] 5) Preparation of porous silicon-carbon composite materials
[0158] The porous silicon material powder obtained in (4) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. It was heated to 600°C at a heating rate of 2°C min-1 in an argon atmosphere, and then methane was used as a carbon source and a N2 / methane mixture was used as a carrier gas (the volume ratio of N2 to methane was 1:1). At the same time, it was kept at 600°C for 6 hours. After the reaction was completed, it was naturally cooled to room temperature, and the black powder was taken out for use to obtain a porous silicon-carbon composite material, which was recorded as a porous silicon-carbon composite material.
[0159] 2. Battery assembly
[0160] Same as Example 1.
[0161] 3. Battery test
[0162] Same as Example 1.
[0163] 4. The experimental results are as follows:
[0164] The porous silicon-carbon composite material was used as the negative electrode active material to assemble a 2032-type button-type half-cell, with a first-week discharge capacity of 2150.4mAh g-1, a charge capacity of 1574.1mAh g-1, and a coulombic efficiency of 73.2%. After 200 cycles at a current density of 500mA g-1, the reversible capacity was still 1423.5mAh g-1, showing good electrochemical stability.
[0165] Example 5
[0166] 1. The preparation of the porous silicon-carbon composite material is carried out according to the following steps:
[0167] 1) Pretreatment of micron silicon
[0168] 1g of micron silicon (1-10μm) was placed in an acetone solvent for ultrasonic treatment for 3h to remove organic matter on the surface of the micron silicon. Subsequently, it was soaked in a 10M hydrofluoric acid (HF) solution for 0.5h to remove the surface oxide layer, and finally washed with water and dried at 120°C to obtain the micron silicon raw material.
[0169] 2) Micronized silicon loaded with copper
[0170] The treated micron silicon powder is added to 100 mL of 10M hydrofluoric acid (HF) solution (the method is the same as in Example 1). 50 mL of a deposition solution of 500 mmol / L copper sulfate and 1000 mmol / L disodium ethylenediaminetetraacetate is prepared, and then 5 mL of the deposition solution is added dropwise at a constant rate of 1 mL / min to promote uniform deposition of copper metal. After the deposition is completed, the deposited micron silicon powder is centrifuged to remove the first step deposition solution, and then dried in a vacuum drying oven at 120°C for 8 hours to obtain copper-loaded micron silicon.
[0171] 3) Preparation of size-controllable copper-loaded micron silicon.
[0172] The micron silicon powder obtained in (2) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. After heating to 600°C at a heating rate of 30°C min-1 in an argon atmosphere, an Ar / H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to H2 was 9:1 and the gas flow rate was 50 sccm), and the temperature was kept at 600°C for 0.5h. After the reaction was completed, it was naturally cooled to room temperature to obtain a copper-loaded micron silicon material.
[0173] 4) Preparation of porous silicon
[0174] The micron silicon powder obtained in (3) was transferred to a beaker and added with 53.9 mL of deionized water and 15 mL of anhydrous ethanol. 23.5 mL of hydrofluoric acid with a mass fraction of 40 wt.% was added, and the concentration of hydrofluoric acid in the reaction system was 5 M. Then, 7.6 mL of hydrogen peroxide with a mass fraction of 30 wt.% as an oxidant was added dropwise at a constant rate of 12 mL / h, and the concentration of hydrogen peroxide in the reaction system was 0.75 M. After the addition was continued for 1 hour, the micron silicon powder was separated from the etching solution by centrifugation, and dried in a vacuum drying oven at 120°C for 8 hours to obtain a porous silicon material, which was recorded as P-Si / Cu.
[0175] 5) Preparation of porous silicon-carbon composite materials
[0176] The porous silicon material powder obtained in (4) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. It was heated to 1000°C at a heating rate of 30°C min-1 in an argon atmosphere, and then ethane was used as a carbon source and an Ar / ethane mixture was used as a carrier gas (the volume ratio of Ar to ethane was 9:1). At the same time, it was kept at 1000°C for 1 hour. After the reaction was completed, it was naturally cooled to room temperature, and the black powder was taken out for use to obtain a porous silicon-carbon composite material, which was recorded as a porous silicon-carbon composite material.
[0177] 2. Battery assembly
[0178] Same as Example 1.
[0179] 3. Battery test
[0180] Same as Example 1.
[0181] 4. The experimental results are as follows:
[0182] The porous silicon-carbon composite material was used as the negative electrode active material to assemble a 2032-type button-type half-cell, with a first-week discharge capacity of 2250.6mAh g-1, a charge capacity of 1692.3mAh g-1, and a coulombic efficiency of 75.2%. After 200 cycles at a current density of 500mA g-1, the reversible capacity was still 1560.2mAh g-1, showing good electrochemical stability.
[0183] Comparative Example 1
[0184] No copper was loaded, and the rest was the same as in Example 1.
[0185] This porous silicon-carbon composite material is used as the negative electrode active material to assemble a 2032-type button-type half-cell. Its first-week discharge capacity is 2324.5mAh g-1, the charging capacity is 1659.7mAh g-1, the Coulomb efficiency is 71.4%, and the capacity after 50 cycles is 200mAh g-1, and the capacity decays quickly.
[0186] Comparative Example 2
[0187] 1. The preparation of the porous silicon-carbon composite material is carried out according to the following steps:
[0188] 1) Pretreatment of micron silicon
[0189] 1g of micron silicon (1-10μm) was placed in an acetone solvent for ultrasonic treatment for 1h to remove organic matter on the surface of the micron silicon. Subsequently, it was soaked in a 5M hydrofluoric acid (HF) solution for 3h to remove the surface oxide layer, and finally washed with water and dried at 60°C to obtain the micron silicon raw material.
[0190] 2) Precursor of micron silicon loaded with copper
[0191] Add the treated micron silicon powder to a 5M hydrofluoric acid (HF) solution. Prepare a deposition solution of 100mmol / L copper sulfate (10mL) and 200mmol / L disodium ethylenediaminetetraacetate (20mL), then drop 5mL at a constant rate of 1mL / min to promote uniform deposition of copper metal. After deposition, centrifuge the deposited micron silicon powder to remove the first step deposition solution, and then dry it in a vacuum drying oven at 60°C for 10h to obtain a precursor of micron silicon loaded with copper.
[0192] 3) Preparation of size-controllable copper-loaded micron silicon.
[0193] The micron silicon precursor powder obtained in (2) was evenly spread in a ceramic boat and placed in a tubular heat treatment furnace. After heating to 450°C at a heating rate of 5°C min-1 in an argon atmosphere, an Ar / H2 mixed gas was used as a carrier gas (wherein the volume ratio of Ar to H2 was 4:1 and the gas flow rate was 100 sccm), and the temperature was kept at 450°C for 1 hour. After the reaction was completed, it was naturally cooled to room temperature to obtain a copper-loaded micron silicon material.
[0194] 4) Preparation of copper-loaded porous silicon
[0195] The copper-loaded micron silicon powder obtained in (3) was transferred to a beaker and added with 53.9 mL of deionized water and 15 mL of anhydrous ethanol, and 23.5 mL of hydrofluoric acid with a mass fraction of 40 wt.% was added, and the hydrofluoric acid concentration of the reaction system was 5 M. Then, 7.6 mL of hydrogen peroxide with a mass fraction of 30 wt.% as an oxidant was added dropwise at a constant rate of 12 mL / h, and the hydrogen peroxide concentration of the reaction system was 0.75 M. The oxidant was hydrogen peroxide. After the addition of hydrogen peroxide for 2 hours, the copper-loaded micron silicon powder was separated from the etching solution by centrifugal separation. The copper-loaded porous silicon material was obtained by drying at 60°C in a vacuum drying oven for 10 hours, which was recorded as P-Si / Cu.
[0196] 5) Preparation of porous silicon-carbon composite materials loaded with copper
[0197] Dopamine was used as a carbon source to carbon-coat porous silicon. 100 mg of the copper-loaded porous silicon material powder obtained in (4) and 96 mg of tris(hydroxymethyl)aminomethane (Ttris) powder were weighed and placed in a beaker. 80 mL of deionized water was added and magnetically stirred for 30 min at room temperature. 100 mg of dopamine hydrochloride was weighed and added to the above solution. After stirring for 4 h, centrifugation was performed. The solution was washed with water and ethanol for 3 times and then dried in a vacuum drying oven. The dried powder was calcined in a tube furnace at 550° C. in an argon atmosphere for 3 h to obtain a copper-loaded porous silicon-carbon composite material, which was recorded as a copper-loaded porous silicon-carbon composite material.
[0198] 2. Battery assembly
[0199] Same as Example 1.
[0200] 3. Battery test
[0201] Same as Example 1.
[0202] 4. The experimental results are as follows:
[0203] A 2032-type button-type half-cell was assembled using this porous silicon-carbon composite material as the negative electrode active material. Its first-week discharge capacity was 2100.6 mAh g-1, the charging capacity was 1758.5 mAh g-1, the coulombic efficiency was 70.3%, and the capacity retention rate after 200 cycles was 67.6%.
[0204] The present application aims to solve the problems of poor conductivity and volume expansion of silicon-based negative electrodes. The method of the application includes chemical metal-assisted chemical etching to form pores on micron silicon raw materials, and then carbon coating using a vapor deposition method. The method improves the conductivity and operability of the material by uniformly depositing copper metal particles. The method is simple, controllable, low-cost, and does not require post-processing steps, which is very suitable for industrial production. The prepared porous silicon has a large space that can buffer the volume expansion of silicon during charging and discharging. The copper nano-silicon particles play a conductive role, and the dense carbon layer plays a coating role, preventing the formation of SEI and reducing the occurrence of side reactions. In the invention, we successfully prepared a porous silicon-carbon composite material and evaluated its performance, proving that this type of composite material has broad application prospects in the field of lithium-ion batteries. The porous silicon-carbon composite material can alleviate the particle pulverization and shedding caused by the volume change of the negative electrode material of the lithium-ion battery made of the material, avoid the collapse of the porous structure, and effectively extend the charge and discharge cycle life of the lithium battery.
[0205] Although the embodiments disclosed in the present invention are as above, the contents described are only embodiments adopted to facilitate understanding of the present invention and are not intended to limit the present invention. Any technician in the field to which the present invention belongs can make any modifications and changes in the form and details of implementation without departing from the spirit and scope disclosed in the present invention, but the patent protection scope of the present invention shall still be subject to the scope defined in the attached claims.
Claims
1. A preparation method of a porous silicon-carbon composite material loaded with copper, characterized in that: include: Preparation of copper-loaded micronized silicon; Etching the copper-loaded micron silicon to form porous micron silicon loaded with copper; The copper-loaded porous micron silicon is carbonized to obtain the copper-loaded porous silicon-carbon composite material.
2. The preparation method according to claim 1, characterized in that: The preparation of copper-loaded micron silicon comprises: Adding micron silicon powder into a hydrofluoric acid solution to form a first solution; Prepare a deposition liquid of copper sulfate and disodium ethylenediaminetetraacetate, add the deposition liquid dropwise to the first solution, and obtain a precursor of copper-loaded micron silicon after centrifugation and drying; The precursor is subjected to heat treatment to obtain the copper-loaded micron silicon; Preferably, the molar ratio of the micron silicon powder, copper sulfate and sodium ethylenediaminetetraacetate is 355-357:1-50:10-100.
3. The preparation method according to claim 2, characterized in that: Before the micron silicon powder is added to the hydrofluoric acid solution, it needs to be pretreated, and the pretreatment includes ultrasonic treatment of the micron silicon in a solvent and / or soaking in a hydrofluoric acid solution; and / or the concentration of the hydrofluoric acid solution in the first solution is 1-10M; and / or the concentration of micron silicon powder in the first solution is 5-15 g / L; And / or the concentration of the copper sulfate is 10-500mmol / L; and / or the concentration of the disodium edetate is 100-1000mmol / L; And / or the dropping speed is 0.5mL-3mL / min; And / or the drying conditions are: vacuum drying, temperature 50-120° C., time 8-12 h; And / or the heat treatment conditions are: in an inert gas atmosphere at 2-30°C min -1 After heating to 300-600°C at a heating rate of , an inert gas / H2 mixed gas is used as a carrier gas and kept at 300-600°C for 0.5-3h.
4. The preparation method according to claim 1, characterized in that: Etching the copper-loaded micron silicon to form copper-loaded porous micron silicon comprises: Adding deionized water and an organic solvent to the copper-loaded micron silicon, then adding an etching solution, then dripping an oxidant at a constant rate, separating and drying, to obtain the copper-loaded porous micron silicon; Preferably, the molar ratio of the copper-loaded micron silicon to the etching solution is 1:1-1:9; Preferably, the value of the solution concentration of the etching solution divided by the sum of the solution concentrations of the etching solution and the oxidant in the reaction system is 0.5-0.
95.
5. The preparation method according to claim 4, characterized in that: The etching solution is hydrofluoric acid. Preferably, the concentration of the hydrofluoric acid in the reaction system is 3-6M; and / or the oxidant is hydrogen peroxide; And / or the etching time is 0.5-6h; And / or the drying conditions are: vacuum drying, temperature 50-120° C., time 8-12 h; And / or the dropping speed of the hydrogen peroxide is 6mL-24mL / h.
6. The preparation method according to claim 1, characterized in that: Carrying the copper-loaded porous micron silicon comprises: The copper-loaded porous micron silicon is placed in a tubular heat treatment furnace, and a carbon source gas is introduced to heat the furnace.
7. The preparation method according to claim 6, characterized in that: The carbon source gas is a carbon-containing hydrocarbon gas; And / or the heating conditions are: heating to 600-1000°C at a heating rate of 2-30°C min-1 in an inert gas atmosphere; using an inert gas / carbon source gas mixture as a carrier gas, at 600-1000°C and keeping warm for 1-6h.
8. The preparation method according to claim 7, characterized in that: The volume ratio of the inert gas to the carbon source gas in the mixed gas is 1:1-9:
1.
9. A porous silicon-carbon composite material loaded with copper, characterized in that: Prepared by any one of claims 1 to 8.
10. A battery negative electrode material, characterized in that: The invention comprises the copper-loaded porous silicon-carbon composite material as claimed in claim 9.
Citation Information
Patent Citations
Nano-copper particle in-situ modified micron-sized porous silicon composite structure material and preparation method thereof
CN110993899A
Preparation method of porous silicon / metal / carbon nanomaterial composite negative electrode material of lithium ion battery
CN115472813A