Tin dioxide / carbon composite negative electrode material and preparation method thereof

By adopting a three-layer structure of tin dioxide/carbon composite material and using the combination of hollow tin dioxide layer and carbon layer, the problem of volume expansion of tin dioxide in lithium-ion batteries is solved, the cycle performance and gram capacity are improved, and the Competitiveness of sodium-ion batteries.

CN118867167APending Publication Date: 2024-10-29WANXIANG 123 CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410847674.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing tin dioxide anode materials have serious volume expansion in lithium-ion batteries, resulting in poor cycle performance and difficulty in mass production. Compared with hard carbon materials, they have low operating voltage and low theoretical specific capacity, which limits their use. Applications in high energy density scenarios.

Method used

It adopts a three-layer structure of tin dioxide/carbon composite material, including the innermost layer of nano-tin dioxide balls, the second layer of hollow tin dioxide layer, the third layer of carbon layer, hollow tin dioxide layer and tin dioxide layer. The gaps between the balls mitigate volume expansion, and the outer carbon layer improves conductivity and prevents direct contact between the electrolyte and tin dioxide.

Benefits of technology

The cycle performance and gram capacity of the material are significantly improved. Compared with tin dioxide materials, the volume effect is alleviated. The gram capacity is higher than that of hard carbon materials, which enhances the competitiveness of tin dioxide anodes and the market competitiveness of sodium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867167A_ABST
    Figure CN118867167A_ABST
Patent Text Reader

Abstract

The invention discloses a tin dioxide / carbon composite negative electrode material and a preparation method thereof. The innermost layer is a nano tin dioxide ball, the second layer is a hollow tin dioxide layer, and the outermost layer is a carbon layer. The gap between the hollow tin dioxide layer and the tin dioxide ball provides a buffer space for the volume expansion of the tin dioxide ball, the volume effect in the material circulation process is reduced, and the circulation performance is improved. And the carbon layer coated on the outermost layer can avoid direct contact between the electrolyte and the tin dioxide to a certain extent, so that the first effect is improved, the expansion of the hollow tin dioxide layer can be inhibited, and the conductivity of the material can also be improved. The three-layer-structure tin dioxide / carbon composite negative electrode material is high in gram capacity, the volume effect is relieved compared with a tin dioxide material, and the cycle performance of the material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium batteries, and in particular to a tin dioxide / carbon composite negative electrode material and a preparation method thereof. Background Art

[0002] As a supplement to lithium batteries, sodium-ion batteries have developed rapidly in recent years, and many companies have officially announced the installation of sodium batteries for use. At present, the negative electrode material used in sodium-ion batteries is basically hard carbon, which has a large interlayer spacing, stable structure, good volume expansion and cycle performance, but the working voltage of hard carbon is low, the theoretical specific capacity is low, and its use in high energy density scenarios is limited. Transition metal oxides, such as tin dioxide, have a high theoretical capacity of more than 700mAh / g, and are the preferred solution for improving the energy density of sodium-ion batteries. However, at present, this type of material has a large volume effect during charging and discharging, resulting in low first efficiency and poor cycle, and is difficult to mass produce. This type of material can be improved by nano-sizing, carbon composite and element doping, and there are currently a large number of studies of this type. For example, patent CN114014354B discloses a method and application for preparing nano-tin dioxide @ nitrogen-doped carbon composite materials: coal or petroleum-based heavy organic matter, nitrobenzene, anhydrous tin tetrachloride and solvent are added to the reactor, and reacted for a certain time under certain conditions; after the reaction is completed, washing liquid is added to the reaction system, and the mixture is filtered, washed and dried to obtain product A. The product A is carbonized under an inert atmosphere to obtain a nano-tin dioxide@nitrogen-doped carbon composite material. The prepared composite material can be used as a negative electrode material for a battery.

[0003] Patent CN115377396A relates to a core-shell structured sodium ion battery negative electrode material and a preparation method thereof; the method utilizes polythiophene polymer to coat the surface of graphene oxide, thereby improving the dispersibility of graphene oxide and avoiding its agglomeration, so that it can be evenly dispersed in the negative electrode and exhibit good electrochemical properties; by compounding nano-tin dioxide with graphene oxide, graphene can improve the conductivity of the tin dioxide material, thereby improving the rate performance of the material; on the other hand, the flexible and porous graphene can accommodate the volume expansion of tin dioxide during the process of extracting and embedding sodium ions, thereby improving its cycle performance.

[0004] Patent CN117352692A provides a negative electrode material and a preparation method thereof, including hollow tin dioxide microspheres and a porous carbon layer coated on the outer surface thereof, the thickness of the porous carbon layer is 0.5 to 3 μm, and the pore size distribution of the porous carbon layer is 10 to 50 nm. The design of porous carbon layer coating and hollow tin dioxide microspheres is adopted, and by regulating the coating thickness of the porous carbon layer and the porous structure of the carbon layer, the negative electrode material can have excellent cycle performance and gram capacity at the same time.

[0005] However, the above technologies all have technical defects. The technical focus of patent CN114014354B and patent CN115377396A is on the composite of tin dioxide and carbon-based materials, which can improve the theoretical capacity of negative electrode materials. However, when tin dioxide is embedded in lithium ions, its volume tends to expand rapidly. Therefore, simply coating the outer layer with carbon has little effect on inhibiting or slowing down the volume expansion of tin dioxide, and cannot effectively improve the cycle performance of the material.

[0006] Patent CN117352692A adopts a hollow tin dioxide structure, which can alleviate the volume expansion of the material and improve the cycle performance. However, in this structure, the thickness ratio of tin dioxide to porous carbon is 1:5-7. The proportion of tin dioxide limits the gram capacity of the material. In addition, by using pore-forming agents to form pores in multiple carbon layers, the electrolyte can easily enter the carbon layer and contact with tin dioxide, increasing the first irreversible capacity loss and reducing the initial effect of the material. Summary of the invention

[0007] In view of the above problems, the present invention proposes a tin dioxide / carbon composite negative electrode material and a preparation method thereof. The three-layer structure of the tin dioxide / carbon composite negative electrode material has a higher gram capacity, and the volume effect is alleviated compared with the tin dioxide material, which greatly improves the cycle performance of the material. Compared with the hard carbon material, this material has a higher gram capacity.

[0008] The technical solution adopted by the present invention is as follows: A method for preparing a tin dioxide / carbon composite negative electrode material comprises the following steps:

[0009] (1) dispersing tin dioxide in a water / ethanol mixture, adding ammonia water and a template, stirring fully at room temperature, centrifuging, washing and drying to obtain a SnO2@ template;

[0010] (2) Adding SnO2@template to a water / ethanol mixture, adding hydrated tin tetrachloride and urea, stirring thoroughly, transferring to a hydrothermal kettle, placing in an oven for reaction, cooling after the reaction, washing and drying, and obtaining SnO2@template@SnO2;

[0011] (3) SnO2@template@SnO2 is fully stirred in a sodium hydroxide solution, and the template is removed to obtain a double-layer hollow tin dioxide material;

[0012] (4) The double-layer hollow tin dioxide material and the carbon source are evenly mixed, carbonized in an inert atmosphere in a tube furnace, and cooled to obtain a tin dioxide / carbon composite negative electrode material.

[0013] Optionally, the particle size of tin dioxide in the tin dioxide / carbon composite negative electrode material is in the range of 5-100 nm.

[0014] Optionally, the template includes any one of silicon dioxide, polystyrene balls, and organic carbon, and the ratio of the thickness of the template to the particle size of the tin dioxide nanospheres is 5 to 1:1.

[0015] Optionally, in step (2), the wall thickness of the hollow tin dioxide layer of SnO2@template@SnO2 is 0.1-1 μm.

[0016] Optionally, the template in step (2) is silicon dioxide, and SnO2@SiO2@SnO2 is obtained, and the mass ratio of silicon dioxide to tin dioxide in SnO2@SiO2@SnO2 is 0.5-3.

[0017] Optionally, the template is silicon dioxide, and an alkaline solution etching method is used to remove the template.

[0018] Optionally, the template is organic carbon, and the template is removed by calcination in air.

[0019] Optionally, the mass fraction of the carbon layer in the tin dioxide / carbon composite negative electrode material is 1-10%.

[0020] Optionally, the carbon source in step (4) is biomass or resin, and the carbonization temperature is 500-1000°C.

[0021] The present invention also discloses a tin dioxide / carbon composite negative electrode material prepared by the preparation method described above, comprising a carbon layer, a hollow tin dioxide layer and a tin dioxide ball sequentially coated from the outside to the inside, wherein there is a gap between the tin dioxide ball and the inner wall of the hollow tin dioxide layer.

[0022] The beneficial effects of the present invention are as follows: the prepared tin dioxide / carbon composite negative electrode material is divided into three layers, the innermost layer is nano tin dioxide balls with a particle size between 5-100nm, the second layer is a hollow tin dioxide layer, and the outermost layer is a carbon layer. The gap between the hollow tin dioxide layer and the tin dioxide balls provides a buffer space for the expansion of the volume of the tin dioxide balls, reduces the volume effect during the material cycle, and improves the cycle performance. The carbon layer coated on the outermost layer can avoid direct contact between the electrolyte and tin dioxide to a certain extent, improve the first effect, inhibit the expansion of the hollow tin dioxide layer, and improve the conductivity of the material. The tin dioxide / carbon composite negative electrode material with a three-layer structure has a higher gram capacity, and the volume effect is alleviated compared to the tin dioxide material, and compared to the hard carbon material, the material has a higher gram capacity, which greatly improves the cycle performance of the material, increases the competitiveness of the tin dioxide negative electrode as a sodium negative electrode, and also increases the competitiveness of sodium ion batteries in the market. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 A schematic diagram of the structure of a tin dioxide / carbon composite negative electrode material proposed in an embodiment of the present invention;

[0024] The marks in the drawings are: 1, tin dioxide ball; 2, hollow tin dioxide; 3, carbon layer; 4, void. DETAILED DESCRIPTION

[0025] The present invention is described in detail below in conjunction with the accompanying drawings.

[0026] like Figure 1 As shown, the present invention discloses a tin dioxide / carbon composite negative electrode material, including a carbon layer 3, a hollow tin dioxide layer 2 and a tin dioxide ball 1 coated in sequence from the outside to the inside, the tin dioxide ball 1 is a solid small ball, the number can be multiple, and there is a gap 4 between the tin dioxide ball 1 and the inner wall of the hollow tin dioxide layer, the innermost layer is a nano tin dioxide ball with a particle size between 5-100nm, the second layer is a hollow tin dioxide layer, and the outermost layer is a carbon layer. The tin dioxide is divided into two parts, one part is a core with a smaller particle size, and the volume effect of the particles in charging and discharging is reduced by reducing the size. The other part is a hollow tin dioxide layer, which is made by a template method, has a controllable wall thickness, is in direct contact with the internal tin dioxide ball and the external carbon layer, provides an electron transfer site, and the layer can also play a role in isolating the inner core tin dioxide from contacting the electrolyte. The gap between the hollow tin dioxide layer and the tin dioxide ball provides a buffer space for the expansion of the volume of the tin dioxide ball, reducing the volume effect during the material cycle and improving the cycle performance. The carbon layer coated on the outermost layer can avoid direct contact between the electrolyte and tin dioxide to a certain extent, improve the first effect, inhibit the expansion of the hollow tin dioxide layer, and improve the conductivity of the material. The three-layer structure of tin dioxide / carbon composite negative electrode material has a higher gram capacity, and the volume effect is alleviated compared to the tin dioxide material, which greatly improves the cycle performance of the material, increases the competitiveness of the tin dioxide negative electrode as a sodium negative electrode, and also increases the competitiveness of sodium-ion batteries in the market.

[0027] The present invention also discloses a method for preparing a tin dioxide / carbon composite negative electrode material, comprising the following steps:

[0028] (1) Disperse tin dioxide in a water / ethanol mixture, add ammonia water and a template, stir thoroughly at room temperature, centrifuge, wash and dry to obtain a SnO2@ template; the template includes any one of silicon dioxide, polystyrene balls, and organic carbon, and the ratio of the template thickness to the particle size of the tin dioxide nanospheres is 5 to 1:1. If the ratio of the template thickness to the particle size of the tin dioxide nanospheres is greater than 5, the pore structure is too large, the overall vibration of the material is too small, and the processing performance is poor. If the ratio of the template thickness to the particle size of the tin dioxide nanospheres is less than 1, the void structure is too small to safely accommodate the expansion of tin dioxide, and the advantages of the structure cannot be reflected. The ratio of the template thickness to the particle size of the tin dioxide nanospheres can be 5:1, 3:1, 2:1 or 1:1.

[0029] (2) Take SnO2@template and add it to a water / ethanol mixture, add hydrated tin tetrachloride and urea, stir thoroughly, transfer to a hydrothermal kettle, place in an oven for reaction, cool after the reaction, wash and dry to obtain SnO2@template@SnO2, the wall thickness of the hollow tin dioxide layer of SnO2@template@SnO2 is 0.1-1μm. The template can be selected from silicon dioxide to obtain SnO2@SiO2@SnO2, the mass ratio of silicon dioxide to tin dioxide in SnO2@SiO2@SnO2 is 0.5-3

[0030] (3) SnO2@template@SnO2 is fully stirred in a sodium hydroxide solution, and the template is removed to obtain a double-layer hollow tin dioxide material; if the template is silicon dioxide, the template is removed by alkaline etching; if the template is organic carbon, the template is removed by calcination in air.

[0031] (4) The double-layer hollow tin dioxide material and the carbon source are mixed evenly, carbonized in an inert atmosphere in a tubular furnace, and cooled to obtain a tin dioxide / carbon composite negative electrode material. The carbon source can be biomass or resin, and the carbonization temperature is 500-1000°C. The mass fraction of the carbon layer in the tin dioxide / carbon composite negative electrode material is 1-10%. The particle size range of tin dioxide in the tin dioxide / carbon composite negative electrode material is 5-100nm. The carbon layer is a hard carbon layer. As a coating layer, if the carbon layer is added in too little amount, it is easy to cause uneven coating and the inhibitory effect on the volume effect of the material is not obvious. If the amount added is too much, it will lead to a decrease in the overall gram capacity of the material, and the advantages of the tin dioxide material will not be reflected.

[0032] Comparative Example 1

[0033] 0.5 g of tin dioxide material with a particle size of 20 nm and 0.1 g of resin were evenly mixed and carbonized in a tubular furnace in an argon atmosphere; the heating rate was controlled at 5°C / min, and after heating to 1000°C, the temperature was kept for 2 hours, and the tin dioxide material coated with a carbon layer was obtained by cooling.

[0034] Comparative Example 2

[0035] (1) 0.5 g of commercial tin dioxide with a particle size of 200 nm was dispersed in 300 ml of a water / ethanol mixture with a mass ratio of 3:1, 5 ml of ammonia water and 2 ml of TEOS were added, stirred at room temperature for 8 h, centrifuged and washed and dried to obtain SnO2@SiO2;

[0036] (2) 0.5 g of the above SnO2@SiO2 material was added to 300 ml of a water / ethanol mixture, and 2 g of hydrated tin tetrachloride and urea were added. The mixture was stirred for 0.5 h, transferred to a hydrothermal kettle, and placed in an oven at 180°C for reaction for 12 h. After cooling, the mixture was washed and dried to obtain SnO2@SiO2@SnO2;

[0037] (3) The SnO2@SiO2@SnO2 was stirred in a 2 mol / L sodium hydroxide solution for 10 h, and the silicon dioxide layer was etched away to obtain a double-layer hollow tin dioxide material.

[0038] Example 1

[0039] (1) 0.5 g of commercial tin dioxide with a particle size of 20 nm was dispersed in 300 ml of a water / ethanol mixture with a mass ratio of 3:1, 3 ml of ammonia water and 2 ml of TEOS were added, stirred at room temperature for 8 h, centrifuged and washed and dried to obtain SnO2@SiO2;

[0040] (2) 0.5 g of the above SnO2@SiO2 material was added to 300 ml of a water / ethanol mixture, 2 g of hydrated tin tetrachloride and 10 g of urea were added, and the mixture was stirred for 0.5 h. The mixture was transferred to a hydrothermal kettle and placed in an oven at 180°C for reaction for 12 h. After cooling, the mixture was washed and dried to obtain SnO2@SiO2@SnO2.

[0041] (3) The SnO2@SiO2@SnO2 was stirred in a 2 mol / L sodium hydroxide solution for 10 h, and the silicon dioxide layer was etched away to obtain a double-layer hollow tin dioxide material.

[0042] (4) 0.5 g of the above hollow tin dioxide material and 0.1 g of resin were mixed evenly and carbonized in a tube furnace in an argon atmosphere; the heating rate was controlled at 5°C / min, and the temperature was increased to 1000°C and kept at that temperature for 2 h, and then cooled to obtain a double-layer hollow tin dioxide / carbon composite negative electrode material.

[0043] Example 2

[0044] (1) 0.5 g of commercial tin dioxide with a particle size of 20 nm was dispersed in 300 ml of a water / ethanol mixture with a mass ratio of 3:1, 5 ml of ammonia water and 3 ml of TEOS were added, stirred at room temperature for 8 h, centrifuged and washed and dried to obtain SnO2@SiO2;

[0045] (2) 0.5 g of the above SnO2@SiO2 material was added to 300 ml of a water / ethanol mixture, and 2 g of hydrated tin tetrachloride and urea were added. The mixture was stirred for 0.5 h, transferred to a hydrothermal kettle, and placed in an oven at 180°C for reaction for 12 h. After cooling, the mixture was washed and dried to obtain SnO2@SiO2@SnO2;

[0046] (3) stirring the above SnO2@SiO2@SnO2 in a 2 mol / L sodium hydroxide solution for 10 h, and etching away the silicon dioxide layer to obtain a double-layer hollow tin dioxide material;

[0047] (4) 0.5 g of the above-mentioned double-layer hollow tin dioxide material and 0.1 g of resin were mixed evenly and carbonized in a tube furnace in an argon atmosphere; the heating rate was controlled at 5°C / min, and the temperature was increased to 1000°C and kept at this temperature for 2 h, and then cooled to obtain a double-layer hollow tin dioxide / carbon composite negative electrode material.

[0048] Example 3

[0049] (1) 0.5 g of commercial tin dioxide with a particle size of 20 nm was dispersed in 300 ml of a water / ethanol mixture with a mass ratio of 3:1, 5 ml of ammonia water and 1 ml of TEOS were added, stirred at room temperature for 8 h, centrifuged and washed and dried to obtain SnO2@SiO2;

[0050] (2) 0.5 g of the above SnO2@SiO2 material was added to 300 ml of a water / ethanol mixture, and 2 g of hydrated tin tetrachloride and urea were added. The mixture was stirred for 0.5 h, transferred to a hydrothermal kettle, and placed in an oven at 180°C for reaction for 12 h. After cooling, the mixture was washed and dried to obtain SnO2@SiO2@SnO2;

[0051] (3) stirring the above SnO2@SiO2@SnO2 in a 2 mol / L sodium hydroxide solution for 10 h, and etching away the silicon dioxide layer to obtain a double-layer hollow tin dioxide material;

[0052] (4) 0.5 g of the above-mentioned double-layer hollow tin dioxide material and 0.1 g of resin were mixed evenly and carbonized in a tube furnace in an argon atmosphere; the heating rate was controlled at 5°C / min, and the temperature was increased to 1000°C and kept at this temperature for 2 h, and then cooled to obtain a double-layer hollow tin dioxide / carbon composite negative electrode material.

[0053] Example 4

[0054] (1) 0.5 g of commercial tin dioxide with a particle size of 200 nm was dispersed in 300 ml of a water / ethanol mixture with a mass ratio of 3:1, 5 ml of ammonia water and 2 ml of TEOS were added, stirred at room temperature for 8 h, centrifuged and washed and dried to obtain SnO2@SiO2;

[0055] (2) 0.5 g of the above SnO2@SiO2 material was added to 300 ml of a water / ethanol mixture, and 2 g of hydrated tin tetrachloride and urea were added. The mixture was stirred for 0.5 h, transferred to a hydrothermal kettle, and placed in an oven at 180°C for reaction for 12 h. After cooling, the mixture was washed and dried to obtain SnO2@SiO2@SnO2;

[0056] (3) stirring the above SnO2@SiO2@SnO2 in a 2 mol / L sodium hydroxide solution for 10 h, and etching away the silicon dioxide layer to obtain a double-layer hollow tin dioxide material;

[0057] (4) 0.5 g of the above-mentioned double-layer hollow tin dioxide material and 0.1 g of resin were evenly mixed and carbonized in a tubular furnace in an argon atmosphere; the heating rate was controlled at 5°C / min, and the temperature was increased to 1000°C and then kept at this temperature for 2 h, and then cooled to obtain a double-layer hollow tin dioxide / carbon composite sodium storage negative electrode material.

[0058] The negative electrode materials obtained in Examples 1 to 4 and Comparative Examples 1 to 2 were used as working electrodes, metallic sodium was used as a counter electrode, glass fiber was used as a diaphragm, 1 mol / L NaPF6 conductive salt and DMC:EC (Vol%) = 1:1 were used as electrolytes, button cells were prepared, 0.1C charge and discharge tests were performed, the cells were fully charged and disassembled after 100 cycles, the thickness of the negative electrode sheets was tested, and the rebound was calculated. The electrochemical properties of the materials are shown in Table 1:

[0059]

[0060] From the test results of Examples 1-4 and Comparative Examples 1-2 in the table, it can be seen that the surface carbon layer has an obvious effect on alleviating volume expansion and improving the cycle performance of the material; and the construction of the double-layer hollow structure further reduces the volume expansion of the pole piece on this basis and improves the cycle performance of the material. The presence of the hollow structure reduces the thickness expansion of the carbon-coated tin dioxide from 69% to 37%, and increases the capacity retention rate from 63.8% to 82.6%, with very significant effects; when the amount of TEOS added is different, the pole piece expansion and capacity retention rate are also different, mainly because the amount of TEOS affects the thickness of the silicon dioxide layer, thereby affecting the thickness of the hollow layer and affecting the alleviating effect on the volume expansion of tin dioxide. When the amount of TEOS added increases from 1ml to 2ml and from 2ml to 3ml, the improvement effect of the former is significantly better than that of the latter, which may be because 3ml TEOS is already in excess.

[0061] The above description is only a preferred embodiment of the present invention, and does not limit the patent protection scope of the present invention. Any equivalent structural transformation made by using the contents of the present invention and the drawings, directly or indirectly used in other related technical fields, is also included in the protection scope of the present invention.

Claims

1. A method for preparing a tin dioxide / carbon composite negative electrode material, characterized in that: The steps include: (1) dispersing tin dioxide in a water / ethanol mixture, adding ammonia water and a template, stirring fully at room temperature, centrifuging, washing and drying to obtain a SnO2@ template; (2) Adding SnO2@template to a water / ethanol mixture, adding hydrated tin tetrachloride and urea, stirring thoroughly, transferring to a hydrothermal kettle, placing in an oven for reaction, cooling after the reaction, washing and drying, and obtaining SnO2@template@SnO2; (3) SnO2@template@SnO2 is fully stirred in a sodium hydroxide solution, and the template is removed to obtain a double-layer hollow tin dioxide material; (4) The double-layer hollow tin dioxide material and the carbon source are evenly mixed, carbonized in an inert atmosphere in a tube furnace, and cooled to obtain a tin dioxide / carbon composite negative electrode material.

2. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The particle size of tin dioxide in the tin dioxide / carbon composite negative electrode material is in the range of 5-100 nm.

3. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The template comprises any one of silicon dioxide, polystyrene balls and organic carbon, and the ratio of the thickness of the template to the particle size of the tin dioxide nanospheres is 5 to 1:

1.

4. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: In the step (2), the wall thickness of the hollow tin dioxide layer of SnO2@template@SnO2 is 0.1-1 μm.

5. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The template in step (2) is silicon dioxide, and SnO2@SiO2@SnO2 is obtained, wherein the mass ratio of silicon dioxide to tin dioxide in SnO2@SiO2@SnO2 is 0.5-3.

6. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The template is silicon dioxide, and an alkali solution etching method is used to remove the template.

7. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The template is organic carbon, and the template is removed by calcining in air.

8. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The mass fraction of the carbon layer in the tin dioxide / carbon composite negative electrode material is 1-10%.

9. The method for preparing the tin dioxide / carbon composite negative electrode material according to claim 1, characterized in that: The carbon source in step (4) is biomass or resin, and the carbonization temperature is 500-1000°C.

10. A tin dioxide / carbon composite negative electrode material prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The invention comprises a carbon layer, a hollow tin dioxide layer and a tin dioxide ball which are sequentially coated from the outside to the inside, and a gap is provided between the tin dioxide ball and the inner wall of the hollow tin dioxide layer.

Citation Information

Patent Citations

  • A method for preparing nano-tin dioxide@nitrogen-doped carbon composite materials and their applications

    CN114014354B

  • Sodium-ion battery negative electrode material with core-shell structure and preparation method of sodium-ion battery negative electrode material

    CN115377396A

  • Negative electrode material, preparation method thereof and sodium ion battery

    CN117352692A