PY14 < + > intercalated VS4 material as well as preparation method and application thereof
By inserting PY14+ in situ into the VS4 material, the VS4@PY14+ material is formed, which solves the problems of low conductivity and slow diffusion kinetics of VS4, achieves high capacity and high cycle stability of magnesium ion batteries, simplifies the preparation process and reduces the cost cost.
Patent Information
- Application Number
- CN202411212063.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-10-29
AI Technical Summary
The existing VS4 used as a cathode material for magnesium ion batteries has low conductivity and slow solid-state diffusion kinetics, which limits the performance improvement of magnesium ion batteries.
By inserting PY14+ in situ into the VS4 material, the VS4@PY14+ material is formed, which broadens the layer spacing, reduces the Mg2+ diffusion energy barrier, and improves the conductivity and capacity. The cross-petal-shaped nanosheets are prepared using the solvothermal method and the electrochemical in-situ intercalation method. Descriptive VS4@PY14+.
The electrochemical performance of magnesium ion batteries is significantly improved, including high capacity, high rate and high cycle stability, and the preparation process is simple and low cost.
Smart Images

Figure CN118867201A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, and in particular to a PY 14 + Intercalated VS4 material, preparation method and application thereof. Background Art
[0002] With the continuous development of economy and technology, human demand for energy is increasing day by day, and renewable energy has great development prospects in the future. At present, secondary batteries are widely concerned as a new generation of energy storage devices. Among them, magnesium batteries are expected to replace lithium batteries and become the next generation of ion batteries due to the advantages of low reduction potential of magnesium metal, high theoretical volume capacity, low cost and environmental friendliness. However, in practical applications, due to the large charge density of divalent magnesium ions, the diffusion in the positive electrode material is very slow, and there is a relatively serious polarization phenomenon when magnesium metal is used as a positive electrode material. The further development of magnesium ion batteries is limited. Therefore, it is still a very challenging task to develop suitable magnesium battery positive electrode materials to obtain magnesium batteries with better electrochemical performance.
[0003] Among the existing cathode materials, VS4 has attracted extensive attention in the field of energy storage due to its unique "linear chain" quasi-two-dimensional structure and large interchain distance that is conducive to the deintercalation of magnesium ions. 2+ The slow reaction kinetics limits the application of VS4 in magnesium ion batteries. Therefore, it is a very meaningful work to modify VS4 and apply it in magnesium ion batteries. For example, the patent with publication number CN112242526A discloses a Mo-doped VS4 magnesium ion battery positive electrode material. Mo is added as a dopant into the VS4 electrode material, which helps to improve the conductivity of the material itself, provide more active sites, and shorten the diffusion path of magnesium ions, thereby improving the reaction kinetics and maintaining its specific capacity at 120 mAh g -1 The patent with publication number CN112490438A discloses a Mo-VS4 / N-GNTs positive electrode material, in which a Mo-doped VS4 nanosheet array is in-situ grown on an N-GNTs skeleton material by a solvothermal method. The introduction of N-GNTs improves the conductivity of the composite material and enables the active material to grow evenly on the surface of the N-GNTs, avoiding the agglomeration of the active material, which helps to closely combine the active material with the conductive skeleton material, thereby improving the electrochemical performance of the magnesium ion battery.
[0004] Nevertheless, there is still much room for improvement in the performance of VS4 as a positive electrode material for magnesium-ion batteries and the current performance requirements for renewable energy batteries. Summary of the invention
[0005] The present invention is intended to provide a PY 14 + Intercalated VS4 material and its preparation method and application are used to solve the problems of low conductivity and slow solid-state diffusion kinetics when VS4 is used as a positive electrode material in the prior art.
[0006] In order to achieve the above object, the present invention adopts the following technical scheme: a PY 14 + Intercalated VS4 material, the material is VS4@PY 14 + , where PY 14 + This is the in situ intercalation modification of VS4.
[0007] The beneficial effect of this solution is: then by mixing PY into the battery liquid 14 + , PY14+ was in situ intercalated with VS4 through electrochemical reaction to obtain VS4@PY 14 + , widening the interlayer spacing of the material, providing a fast insertion / extraction channel for magnesium ions, and also reducing the Mg 2+ Diffusion energy barrier, that is, through PY 14 + In-situ intercalation further improves the capacity of VS4 as a positive electrode material, increases conductivity, and solves the problem of slow solid-state diffusion kinetics of existing VS4 positive electrode materials.
[0008] Preferably, VS4@PY 14 + The petal-like microstructure is formed by the cross-section of nanosheets, with a size of 1-2 μm, and VS4@PY 14 + There is a gap in the center.
[0009] The beneficial effects of this solution are as follows: the VS4 material is a petal-shaped microstructure formed by the intersection of nanosheets, with a size of 1-2μm and a void in the center, which provides a large specific surface area and shortens the Mg 2+ The diffusion distance provides more active sites, which is beneficial to improve the electrochemical performance of the petal-shaped VS4 positive electrode. The petal-shaped VS4 has a specific surface area of up to 110.31m 2 g -1 , superior to the same type of materials.
[0010] Preferably, a PY 14 + The preparation method of intercalated VS4 material comprises the following steps:
[0011] S1, preparing petal-shaped VS4 material;
[0012] S2, preparation of a formulation containing PY 14 + Cl electrolyte, and this step also includes the following:
[0013] S201, formulated with PY 14 + PY in Cl electrolyte 14 + Cl concentration is 0.05-0.2M;
[0014] S202, the obtained PY 14 + The Cl electrolyte is stirred for 10-12h;
[0015] S203, containing PY 14 + Cl electrolyte, VS4 material as the positive electrode, magnesium metal as the negative electrode to assemble the battery;
[0016] S204, after the assembled battery is left to stand for a set time, an electrochemical performance test of the battery is performed;
[0017] S205, the tested battery is disassembled, the positive electrode sheet is taken out and placed in a solvent for ultrasonic treatment to obtain VS4@PY 14 + Material.
[0018] The beneficial effects of this scheme are: VS4@PY was synthesized by solvothermal method and electrochemical in-situ intercalation method. 14 + Nanomaterials provide a PY 14 + In-situ intercalation of VS4 cathode material provides a fast insertion and extraction channel for magnesium ions by widening the interlayer spacing, while also reducing the Mg 2+ Diffusion energy barrier effectively improves the capacity of positive electrode materials. 14 + This higher capacity and excellent cycle stability enable it to achieve excellent electrochemical properties such as high capacity, high rate and high cycle stability when used to prepare magnesium ion batteries. The entire preparation process is simple, the raw materials are abundant and the cost is low.
[0019] Preferably, in S204, the electrochemical performance test of the battery includes a cyclic voltammetry test, a constant current charge and discharge test, and a rate performance test, and the low potential range of the cyclic voltammetry test is 0.2-0.4V, the high potential range is 1.9-2.2V, and the scanning rate is 0.1-10mV s-1; the current density of the constant current charge and discharge test is 20-100mA g-1; the current density of the rate performance test is 0.05-2A g-1.
[0020] Preferably, in S205, the solvent for ultrasonic treatment is acetonitrile solvent or tetrahydrofuran solvent, and the time of ultrasonic treatment is 5-30 min.
[0021] Preferably, in S203, the battery is assembled in an environment where the water oxygen concentration is less than 0.01 ppm.
[0022] Preferably, preparing the petal-shaped VS4 material comprises the following steps:
[0023] S101, adding NH4VO3 to deionized water, and then stirring the deionized water solution mixed with NH4VO3 in the dark to obtain solution A;
[0024] S102, adding thioacetamide to ethylene glycol to obtain a thioacetamide solution, mixing the thioacetamide solution with solution A and stirring to obtain solution B;
[0025] S103, performing a solvothermal reaction on solution B to obtain a reaction product;
[0026] S104, drying the precipitated reaction product to obtain a petal-shaped VS4 material.
[0027] Preferably, in S01, in solution A, the amount of NH4VO3 substance is 8-11 mmol, the temperature for stirring in the dark is set to 60-80°C, and the stirring time is 30 min.
[0028] Preferably, in S102, in solution B, the amount of thioacetamide is 3 times the amount of NH4VO3, and the stirring temperature of solution B is 60-80°C, and the stirring time is 30 min.
[0029] Preferably, a PY 14 + Application of intercalated VS4 materials, VS4@PY 14 + The material is used in the preparation of magnesium ion batteries, lithium ion batteries, sodium ion batteries, calcium ion batteries or zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is the XRD spectrum of the VS4 material synthesized in Example 1 of the present invention;
[0031] Figure 2 This is a SEM image of the VS4 material synthesized in Example 1 of the present invention;
[0032] Figure 3 VS4@PY is used in Example 1 of the present invention 14 +Cyclic voltammetry curve of the battery when it is the positive electrode;
[0033] Figure 4 VS4@PY is used in Example 1 of the present invention 14 + The rate performance of the battery when it is the positive electrode;
[0034] Figure 5 The present invention is comparative example 1 using un-PY 14 + Battery rate performance with in-situ intercalation of VS4 cathode. DETAILED DESCRIPTION
[0035] The following is further described in detail through specific implementation methods:
[0036] Example 1
[0037] Embodiment 1 is basically as attached Figure 1-4 As shown in the figure, based on the existing problems of low conductivity and slow solid-state diffusion kinetics when VS4 is used as a positive electrode material, the synthesis method and synthesis conditions of VS4 material are improved to give VS4 material a new microstructure morphology and increase its specific surface area, so as to improve the capacity of VS4 as a positive electrode material. Then, by mixing PY 14 + , PY14+ was in situ intercalated with VS4 through electrochemical reaction to obtain VS4@PY 14 + , widening the interlayer spacing of the material, providing a fast insertion / extraction channel for magnesium ions, and also reducing the Mg 2+ Diffusion energy barrier, that is, through PY 14 + In-situ intercalation further improves the capacity of VS4 as a positive electrode material, increases conductivity, and solves the problem of slow solid-state diffusion kinetics of existing VS4 positive electrode materials.
[0038] First, this embodiment provides a novel method for synthesizing VS4 material, which uses a solvothermal method to synthesize a VS4 material with a novel microstructure morphology, specifically comprising the following steps:
[0039] S101, adding NH4VO3 into deionized water, and then stirring the deionized water solution mixed with NH4VO3 in the dark to obtain solution A; in solution A, the amount of NH4VO3 substance is 8-11 mmol, the temperature for stirring in the dark is set to 60-80°C, and the stirring time is 30 min.
[0040] In this step, the amount of NH4VO3 in solution A is preferably 9-10 mmol. The specific operation is to weigh 1.17 g of NH4VO3 powder and add it to 3 ml of deionized water, then transfer the deionized water mixed with NH4VO3 powder to an 80°C water bath and stir for 30 minutes in the dark to obtain a light yellow solution, which is recorded as solution A.
[0041] S102, adding thioacetamide (C2H5NS, hereinafter referred to as TAA) to 30 ml of ethylene glycol to obtain a thioacetamide solution, mixing the thioacetamide solution with solution A and stirring until uniform, to obtain solution B; in solution B, the amount of TAA substance is 3 times the amount of NH4VO3 substance, and the stirring temperature of solution B is 60-80°C, and the stirring time is 30 minutes.
[0042] In this embodiment, the specific operation is: first weigh 2.25g of TAA powder and add it to 30ml of ethylene glycol to mix, and then add the mixed thioacetamide solution to solution A, and then place the mixed solution under electromagnetic stirring at 80°C for 30 minutes to obtain a precursor solution, which is recorded as solution B.
[0043] S103, performing a solvothermal reaction on solution B to obtain a reaction product; the temperature of the solvothermal reaction is 180-240° C., and the reaction time is 2-5 hours.
[0044] In this step, the temperature of the solvent thermal reaction is preferably 190-210°C, and the reaction time is preferably 3-4h. The specific operation of this embodiment is: transfer solution B to a 100mL reactor, and place the reactor in a blast drying oven, and perform a hydrothermal reaction at 200°C for 4h; after the reaction is completed, take out the reactor and cool it at room temperature to obtain a reaction product precipitated in the solution.
[0045] S104, drying the precipitated reaction product to obtain VS4 positive electrode material; the drying temperature is 60-80° C., and the drying time is 8-12 hours.
[0046] In this step, first, the reaction product precipitated in the solution is separated by centrifugation, and then the reaction product is centrifuged and washed three times with deionized water and anhydrous ethanol respectively; finally, it is vacuum dried at 80°C for 12 hours to obtain the final sample, i.e., VS4 material.
[0047] The obtained petal-shaped VS4 material is as follows: Figure 1 As shown, the XRD characterization shows that the diffraction peak of VS4 is relatively sharp and consistent with the standard peak of VS4 monoclinic crystal (JCPDS No.72-1294), which indicates that the VS4 material with high crystallinity is successfully synthesized.
[0048] SEM characterization of VS4 material Figure 2 As shown, Figure 2 Figures a and b show that the VS4 material synthesized in this scheme has a petal-like microstructure formed by the intersection of nanosheets, with a size of 1-2 μm and a void in the center, which provides a large specific surface area to shorten the Mg 2+ The diffusion distance provides more active sites, which is beneficial to improve the electrochemical performance of the petal-shaped VS4 positive electrode. The results show that the specific surface area of VS4 prepared in this example is 110.31 m 2 g -1 , superior to the same type of materials.
[0049] Next, based on the new petal-shaped VS4 as a battery material, a PY 14 + In-situ intercalation of VS4 material specifically includes the following steps:
[0050] S201, formulated with PY 14 + Cl electrolyte, and PY in the electrolyte 14 + The Cl concentration is 0.05-0.2M.
[0051] The electrolyte is one of APC electrolyte or THF electrolyte. Among them, APC electrolyte is an electrolyte based on 1-butyl-1-methylpyrrolidone (NMP) as a base solvent. APC electrolyte is commonly used in the electrolyte of lithium-ion batteries due to its good dissolving ability and stability. It can effectively dissolve the active substances in the positive electrode material and improve the performance of the battery. THF electrolyte is an electrolyte based on tetrahydrofuran (THF) as a base solvent. THF electrolyte can also provide good electrochemical performance in certain specific applications due to its low viscosity and good solubility. However, THF has a low boiling point and may have certain evaporation problems when used under high temperature conditions, which limits its use in certain applications to a certain extent. In this embodiment, the electrolyte is THF electrolyte.
[0052] In this step, 1-butyl-1-methylpyrrolidine chloride (PY 14 + Cl), the specific operation is: first, add phenyl magnesium chloride tetrahydrofuran solution (PhMgCl / THF) into tetrahydrofuran (THF), then slowly add AlCl3 powder to mix, slowly add AlCl3 powder to avoid AlCl3 and tetrahydrofuran solution reacting with heat to produce a lot of white smoke; then, add 0.2M PY 14 + Cl, configure to get THF-PY14 + Cl electrolyte solution, and the electrolyte is prepared in a glove box with a water oxygen concentration of less than 0.01 ppm. 14 + The preferred concentration of Cl is 0.1-0.2M.
[0053] S202, the obtained PY 14 + The Cl electrolyte was stirred for 10-12h.
[0054] The THF-PY 14 The Cl electrolytic solution was stirred for 12 hours to obtain the final product containing PY 14 + Cl in THF electrolyte.
[0055] S203, containing PY 14 + The battery is assembled with VS4 material as the positive electrode and magnesium metal as the negative electrode.
[0056] First, the petal-shaped VS4 synthesized in this embodiment is used as the positive electrode active material, and is uniformly mixed with conductive carbon black (i.e., acetylene black) and binder polyvinylidene fluoride (PVDF) in a mass ratio of 8:1:1, and then N-methylpyrrolidone solvent is added to grind into a uniform slurry; then the slurry is coated on a conductive carbon cloth with a diameter of 14 mm, and then placed in a vacuum oven at 80°C and dried overnight to obtain a positive electrode sheet of a magnesium ion battery, and its loading amount is 1.5-2 mg / cm 3 .
[0057] Next, Whatman GF / C glass fiber with a diameter of 19 mm was used as the separator, and a metal magnesium foil with a diameter of 16 mm and a thickness of 0.1 mm was selected as the negative electrode.
[0058] Finally, the PY 14 + The THF electrolyte of Cl is used as the electrolyte for assembling the battery.
[0059] Likewise, in this step, the battery is assembled in a glove box, and the water-oxygen environment in the glove box is less than 0.01 ppm to prevent oxidation of the positive electrode material and the negative electrode material during the assembly process.
[0060] S204, after the assembled battery is left to stand for a set period of time, an electrochemical performance test is performed on the battery.
[0061] In this step, the electrochemical performance tests of the battery include cyclic voltammetry test, constant current charge and discharge test and rate performance test. The low potential range of the cyclic voltammetry test is 0.2-0.4V, the high potential range is 1.9-2.2V, and the scanning rate is 0.1-10mV s -1 ; The constant current charge and discharge test current density is 20-100mA g -1 ; The current density of the rate performance test is 0.05-2A g -1 .
[0062] By PY 14 + In-situ intercalation improves the performance of the VS4 cathode, and then the electrochemical performance of the assembled battery is tested. The specific operation of the test is as follows:
[0063] The cyclic voltammetry test was carried out on a Shanghai Chenhua CHI660e electrochemical analyzer with a voltage window of 0.35–2.0 V and a scan rate of 0.5 mV s -1 The results are as follows Figure 3 As shown, using THF-PY 14 + The first three cycles of CV curves of Cl electrolyte show highly consistent redox peak positions and intensities, indicating its excellent electrochemical reversibility.
[0064] Constant current charge and discharge tests and rate performance tests are performed on Neware multi-channel battery measurement devices, such as Figure 4 As shown, PY 14 + The in-situ intercalated VS4 cathode material showed a significant improvement in specific capacity and rate performance. -1 , 0.1A g -1 , 0.2A g -1 , 0.5A g -1 , 1A g -1 , 2A g -1 At a current density of 234 mAh g -1 , 152mAh g -1 , 125mAh g -1 , 107mAh g -1 , 95mAh g -1 , 84mAh g -1 When the current density returned to 50 mA g -1 When the battery capacity is 167 mAh g -1 .
[0065] S205, the tested battery is disassembled, the positive electrode sheet is taken out and placed in a solvent for ultrasonic treatment to obtain VS4@PY 14 + Material.
[0066] The assembled battery was operated during the above test process, and the VS4 positive electrode material underwent electrochemical reaction to generate PY 14 + In-situ intercalated VS4 cathode material, namely VS4@PY 14 + In this step, in order to prevent the VS4 positive electrode material from being oxidized, the ultrasonic treatment solvent is acetonitrile solvent or tetrahydrofuran solvent, and the ultrasonic treatment time is 5-30 minutes.
[0067] Comparative Example 1
[0068] The difference from Example 1 is that the positive electrode material of the battery in Comparative Example 1 is ordinary VS4 material instead of PY 14 + In-situ intercalation of VS4 cathode material, and the battery electrolyte does not contain PY 14 + Cl in THF electrolyte.
[0069] The electrolyte in Comparative Example 1 does not contain PY 14 + The preparation steps of the THF electrolyte containing PYCl are as follows: first, a certain amount of phenylmagnesium chloride tetrahydrofuran solution (PhMgCl / THF) is added to tetrahydrofuran (THF), and then AlCl3 powder is slowly added to obtain a mixed electrolytic cell solution; then, the mixed electrolytic cell solution is stirred for 12 hours to obtain a final solution without PYCl3. 14 + Finally, the same separator and metal magnesium foil as in Example 1 were used as the negative electrode of the battery, and the battery was assembled in a glove box with a water and oxygen concentration of less than 0.01 ppm.
[0070] The obtained battery was subjected to constant current charge and discharge test, and the constant current charge and discharge test was performed on the Neware multi-channel battery measurement device under the same setting conditions. The results are as follows Figure 5 As shown, the cell in Comparative Example 1 is at 0.05Ag -1 , 0.1Ag -1 , 0.2Ag -1 , 0.5Ag -1 , 1Ag -1 , 2Ag -1 At current densities of 141 mAh g -1 , 78mAh g -1, 58mAh g -1 , 50mAh g -1 , 40mAh g -1 , 34mAh g -1 The specific capacity of the battery is much smaller than that of PY in Example 1. 14 + The VS4 positive electrode material assembled after in-situ intercalation obtains the specific capacity exhibited by the battery.
[0071] In summary, the present invention adopts solvothermal method and electrochemical in-situ intercalation method to synthesize VS4@PY 14 + Nanomaterials provide a PY 14 + In-situ intercalation of VS4 cathode material provides a fast insertion and extraction channel for magnesium ions by widening the interlayer spacing, while also reducing the Mg 2+ Diffusion energy barrier effectively improves the capacity of positive electrode materials. 14 + This higher capacity and excellent cycle stability enable it to achieve excellent electrochemical properties such as high capacity, high rate and high cycle stability when used to prepare magnesium ion batteries. The entire preparation process is simple, the raw materials are abundant and the cost is low.
[0072] At the same time, the VS4@PY 14 + The magnesium battery system constructed by the positive electrode material uses VS4 as the positive electrode material of the magnesium ion battery, metal magnesium foil as the negative electrode material, and PY 14 + Cl was added to 0.4 M APC or THF as the electrolyte to assemble the battery. -1 The current density is 250 mAh g -1 High specific capacity, when the current density is expanded 40 times to 2A -1 , it can still provide ~90mAh g -1 The specific capacity has excellent rate performance; and when the current density is restored to 50mAg -1 When the specific capacity is restored to 160 mAh g -1 , showing excellent electrochemical reversibility.
[0073] Finally, it should be noted that the present invention provides a PY 14 + In-situ intercalation VS4 positive electrode material preparation method, this method is not only used in magnesium ion batteries, but also can be used in the preparation of lithium ion batteries, sodium ion batteries, calcium ion batteries and zinc ion batteries. The preparation method thereof refers to the above-mentioned magnesium ion battery preparation method and will not be repeated here.
[0074] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions and / or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the technical solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A PY 14 + Intercalated VS4 material, characterized by: Material: VS4@PY 14 + , where PY 14 + This is the in situ intercalation modification of VS4.
2. A PY according to claim 1 14 + Intercalated VS4 material, characterized by: VS4@PY 14 + The petal-like microstructure is formed by the cross-section of nanosheets, with a size of 1-2 μm, and VS4@PY 14 + There is a gap in the center.
3. A PY 14 + The preparation method of intercalated VS4 material is characterized in that: The following steps are involved: S1, preparing petal-shaped VS4 material; S2, preparation of a formulation containing PY 14 + Cl electrolyte, and this step also includes the following: S201, formulated with PY 14 + PY in Cl electrolyte 14 + Cl concentration is 0.05-0.2M; S202, the obtained PY 14 + The Cl electrolyte is stirred for 10-12h; S203, containing PY 14 + Cl electrolyte, VS4 material as the positive electrode, magnesium metal as the negative electrode to assemble the battery; S204, after the assembled battery is left to stand for a set time, an electrochemical performance test of the battery is performed; S205, the tested battery is disassembled, the positive electrode sheet is taken out and placed in a solvent for ultrasonic treatment to obtain VS4@PY 14 + Material.
4. A PY according to claim 3 14 + The preparation method of intercalated VS4 material is characterized by: In S204, the electrochemical performance tests of the battery include cyclic voltammetry test, constant current charge and discharge test and rate performance test, and the low potential range of the cyclic voltammetry test is 0.2-0.4V, the high potential range is 1.9-2.2V, and the scanning rate is 0.1-10mV s-1; the current density of the constant current charge and discharge test is 20-100mA g-1; the current density of the rate performance test is 0.05-2Ag-1.
5. A PY according to claim 4 14 + The preparation method of intercalated VS4 material is characterized by: In S205, the solvent for ultrasonic treatment is acetonitrile or tetrahydrofuran, and the ultrasonic treatment time is 5-30 min.
6. A PY according to claim 5 14 + The preparation method of intercalated VS4 material is characterized by: In S203 , the battery is assembled in a water-oxygen environment with a concentration of less than 0.01 ppm.
7. A PY according to claim 3 14 + The preparation method of intercalated VS4 material is characterized by: The preparation of petal-shaped VS4 material includes the following steps: S101, adding NH4VO3 to deionized water, and then stirring the deionized water solution mixed with NH4VO3 in the dark to obtain solution A; S102, adding thioacetamide to ethylene glycol to obtain a thioacetamide solution, mixing the thioacetamide solution with solution A and stirring to obtain solution B; S103, performing a solvothermal reaction on solution B to obtain a reaction product; S104, drying the precipitated reaction product to obtain a petal-shaped VS4 material.
8. A PY according to claim 7 14 + The preparation method of intercalated VS4 material is characterized by: In S01, in solution A, the amount of NH4VO3 substance is 8-11 mmol, the temperature for stirring in the dark is set to 60-80°C, and the stirring time is 30 min.
9. A PY according to claim 8 14 +The preparation method of intercalated VS4 material is characterized by: In S102, in solution B, the amount of thioacetamide is three times the amount of NH4VO3, and the stirring temperature of solution B is 60-80°C, and the stirring time is 30 minutes.
10. A PY 14 + The application of intercalated VS4 material is characterized by: VS4@PY in claim 1 or 2 14 + The material is used in the preparation of magnesium ion batteries, lithium ion batteries, sodium ion batteries, calcium ion batteries or zinc ion batteries.
Citation Information
Patent Citations
Curly vanadium tetrasulfide nanosheet negative electrode material of sodium-ion battery as well as preparation method and application thereof
CN111646509A
Mg < 2 + > pre-embedded magnesium ion battery positive electrode material MgVS4 / N-TG and application
CN114039034A