LiNbO3 modified composite sulfur solid-state positive electrode material, preparation method thereof and all-solid-state lithium-sulfur battery
By adding LiNbO3 to the cathode material of all-solid-state lithium-sulfur batteries, the problems of electrolyte degradation and interface impedance are solved, the charge-discharge specific capacity and cycle stability of the battery are improved, and higher battery performance is achieved.
Patent Information
- Application Number
- CN202410851855.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
Due to the low electronic conductivity of elemental sulfur and the volume expansion of the positive active material caused by electrochemical reactions in all-solid-state lithium-sulfur batteries, the charge and discharge capacity and cycle stability of the battery are affected, and the interface impedance of solid powder assembly is large, leading to electrochemical reactions. slow.
LiNbO3 is added to the cathode material to generate a built-in electric field through the polarization of LiNbO3, which slows down the degradation of the electrolyte and inhibits the formation of a space charge layer at the interface between the cathode and the solid electrolyte. A specific raw material ratio and preparation method are used to prepare LiNbO3-modified composite sulfur. Solid cathode materials.
It improves the charge-discharge specific capacity and cycle stability of the battery, and improves the overall performance of the battery by inhibiting electrolyte degradation and the formation of the interface space charge layer.
Smart Images

Figure CN118867243A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of functional materials, and relates to a composite sulfur solid positive electrode material, and specifically relates to a LiNbO3-modified composite sulfur solid positive electrode material, a preparation method thereof, and an all-solid-state lithium-sulfur battery. Background Art
[0002] High energy density batteries are essential for modern portable electronic products and electric vehicles. Lithium-sulfur batteries have a high theoretical specific capacity (1675 mAh g -1 ), high theoretical energy density (2600wh kg -1 ), rich sulfur resources, low electrode cost, and environmental friendliness have made it one of the ideal choices for the new generation of energy storage devices. Although people have made a lot of efforts in the positive and negative electrodes, separators, and electrolytes of liquid lithium-sulfur batteries in recent years, liquid lithium-sulfur batteries have caused worrying safety issues due to the inherent shuttle effect. Among the many modification methods, the use of solid electrolytes instead of traditional liquid electrolytes has been favored by more researchers because it avoids the shuttle effect.
[0003] As a new type of battery technology, all-solid-state lithium-sulfur batteries use solid electrolytes instead of liquid electrolytes. First, all-solid-state lithium-sulfur batteries avoid leakage and combustion of electrolytes, reducing the risk of thermal runaway. Second, all-solid-state lithium-sulfur batteries do not have capacity reduction and safety issues caused by the shuttle effect. Finally, all-solid-state lithium-sulfur batteries can further optimize volume and weight, thereby improving the overall energy density of the battery.
[0004] However, all-solid-state lithium-sulfur batteries still face many challenges. First, due to the low electronic conductivity of elemental sulfur, it is usually necessary to add a conductive agent to the positive electrode. The addition of the conductive agent will induce electrolyte decomposition, thus threatening the capacity. In addition, due to the continuous electrochemical reaction, the positive electrode active material will undergo volume expansion, resulting in the disconnection of some ion and electron pathways, thereby producing inactive lithium (dead lithium), which ultimately affects the charge and discharge capacity and cycle stability of the battery. Finally, since all-solid-state lithium-sulfur batteries are assembled from solid powders, solid-solid contact leads to a large interface impedance, resulting in a slower electrochemical reaction. In particular, at the interface between the positive electrode and the solid electrolyte, due to the different chemical potentials of lithium ions between the electrolyte and the active material, there is a large chemical potential difference at the interface, thereby forming a space charge layer, which ultimately affects the battery's cycle performance. Therefore, the rational design of the positive electrode material of the all-solid-state lithium-sulfur battery has an important impact on the performance of the battery. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a LiNbO3-modified composite sulfur solid-state positive electrode material, a preparation method thereof and an all-solid-state lithium-sulfur battery. By adding LiNbO3 to the positive electrode, the built-in electric field generated by the polarization of LiNbO3 slows down the degradation of the electrolyte in the positive electrode, and at the same time inhibits the formation of a space charge layer at the interface between the positive electrode and the solid electrolyte, so that the battery obtains a higher charge and discharge specific capacity and better cycle stability.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A LiNbO3 modified composite sulfur solid positive electrode material comprises, by mass percentage, 10%-20% active sulfur material, 10%-20% electronic conductor, 60%-70% sulfide electrolyte and 5%-10% LiNbO3.
[0008] Preferably, the active sulfur material includes any one of elemental sulfur and lithium sulfide.
[0009] Preferably, the electronic conductor includes any one of BP2000, Super P and CNTs.
[0010] Preferably, the sulfide electrolyte includes Li 10 GeP2S 12 Or any one of Li6PS5Cl.
[0011] The present invention also protects a method for preparing the LiNbO3-modified composite sulfur solid positive electrode material as described above, comprising the following steps:
[0012] Step 1: ball-milling the active sulfur material and the electronic conductor according to the mass ratio to obtain powder A, and calcining and melting the powder A at high temperature to obtain powder B;
[0013] Step 2: Take the sulfide electrolyte and LiNbO3 according to the mass ratio and grind them together with the composite material B manually to obtain the composite positive electrode material C;
[0014] The above steps are all carried out in an environment filled with inert gas Ar.
[0015] Preferably, the ball-to-material ratio of the ball mill is 50:1, the ball mill speed is 300 rpm / min, and the ball mill time is 12 h.
[0016] Preferably, the high temperature calcination temperature is 155° C. and the calcination time is 12 hours.
[0017] Preferably, the manual grinding time is 30 minutes.
[0018] The present invention also protects a LiNbO3-modified composite sulfur solid-state positive electrode material prepared by the method as described above and its application in an all-solid-state lithium-sulfur battery.
[0019] Compared with the prior art, the present invention has the following technical effects:
[0020] The present invention adds LiNbO3 to the positive electrode material. The built-in electric field generated by the polarization of LiNbO3 slows down the degradation of the electrolyte in the positive electrode, and inhibits the formation of a space charge layer at the interface between the positive electrode and the solid electrolyte, so that the battery has a higher charge and discharge specific capacity and better cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 X-ray diffraction analysis patterns of the composite positive electrode materials of Example 1 and Comparative Example 1;
[0022] Figure 2 This is a SEM image of the composite cathode material of Example 1 before cycling;
[0023] Figure 3 This is a SEM image of the composite positive electrode material of Comparative Example 1 before cycling;
[0024] Figure 4 This is a SEM image of the composite cathode material of Example 1 after cycling;
[0025] Figure 5 This is a SEM image of the composite positive electrode material of Comparative Example 1 after cycling;
[0026] Figure 6 This is the first cycle GITT curve of the all-solid-state lithium-sulfur battery of Comparative Example 1;
[0027] Figure 7 is the first cycle GITT curve of the all-solid-state lithium-sulfur battery of Example 1;
[0028] Figure 8 The figure is a comparison chart of the cycle performance of the all-solid-state lithium-sulfur battery of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0029] The specific contents of the present invention are further explained in detail below in conjunction with embodiments.
[0030] The raw materials used in the present invention can be prepared by those skilled in the art through published literature or purchased;
[0031] In the following examples, the manufacturer of BP2000 (BLACK PEARLS2000) and Super P (Timcal) is Guangdong Candlelight New Energy Technology Co., Ltd.; the manufacturer of CNTs (99%, hexagonal system) is Shenzhen Deheng Technology Co., Ltd.;
[0032] Li 10 GeP2S 12 The manufacturer of (LGPS) and Li6PS5Cl is Hubei Solid New Energy Technology Co., Ltd.
[0033] Example 1
[0034] A LiNbO3-modified composite sulfur solid positive electrode material, the raw material components and their mass percentages are S: BP2000: LGPS: LiNbO3 = 20: 15: 60: 5, and the preparation method steps are as follows:
[0035] Step 1: Take active sulfur material and electronic conductor BP2000 and perform ball milling to obtain powder A, the ball-to-material ratio is 50:1, the ball milling speed is 300 rpm / min, and the ball milling time is 12 hours; the powder A is calcined and melted at high temperature to obtain powder B; the calcination temperature is 155°C, and the calcination time is 12 hours;
[0036] Step 2: Take the sulfide electrolyte LGPS and LiNbO3 according to the mass ratio and grind them together with the composite material B by hand to obtain the composite positive electrode material C. The grinding time is 30 minutes.
[0037] The preparation process was carried out in an argon atmosphere.
[0038] The preparation method of all-solid-state lithium-sulfur battery is as follows:
[0039] Use a scraper to repeatedly remove the black uneven areas on the surface of the lithium sheet to make it smooth and shiny, and use a punching pliers to cut it into lithium sheets with a diameter of 10 mm;
[0040] Weigh 60-80 mg of LGPS electrolyte and place it in a polytetrafluoroethylene solid-state battery mold, apply a force of 2.5 Tons and maintain it for 3 minutes; then weigh 2-3 mg of composite positive electrode material C and place it on top of LGPS, apply a force of 3.5 Tons and maintain it for 3 minutes; finally, place the surface-treated lithium sheet under LGPS, apply 0.3 Tons and maintain it for about 30 seconds to obtain an all-solid-state lithium-sulfur battery; in order to achieve the effect of applying constant pressure to the battery, a constant pressure of 1.0 Tons needs to be applied to the assembled battery.
[0041] The preparation process of all-solid-state lithium-sulfur batteries is carried out in an environment filled with inert gas Ar;
[0042] The assembled all-solid-state lithium-sulfur battery was left at room temperature for more than 2 hours and then tested.
[0043] Test method:
[0044] (1) The battery was tested by constant current gap titration method using a blue electric test system, with a current intensity of 0.1C and a relaxation time of 10 min;
[0045] (2) The battery cycle performance was tested using a blue power test system, with the discharge voltage at 1.7 V, the charge voltage at 2.8 V, the charge and discharge current at 0.1 C, and the cycle duration at 20 cycles.
[0046] Example 2
[0047] The LiNbO3-modified composite sulfur solid positive electrode material of Example 2 has raw material components and their mass percentages of S: BP2000: LGPS: LiNbO3 = 10: 20: 65: 5, and the preparation steps are consistent with those of Example 1.
[0048] Example 3
[0049] The LiNbO3-modified composite sulfur solid positive electrode material of Example 3 has raw material components and their mass percentages of S: BP2000: LGPS: LiNbO3 = 15: 10: 65: 10, and the preparation steps are consistent with those of Example 1.
[0050] Example 4
[0051] The LiNbO3-modified composite sulfur solid positive electrode material of Example 4 has raw material components and their mass percentages of S: BP2000: LGPS: LiNbO3 = 10: 13: 70: 7, and the preparation steps are consistent with those of Example 1.
[0052] Comparative Example 1
[0053] The LiNbO3-modified composite sulfur solid positive electrode material of Comparative Example 1 has raw material components and their mass percentages of S:BP2000:LGPS=30:10:60, and the preparation steps are consistent with those of Example 1.
[0054] Comparative Example 2
[0055] The LiNbO3-modified composite sulfur solid positive electrode material of Comparative Example 2 has raw material components and their mass percentages of S:BP2000:LGPS=20:20:60, and the preparation steps are consistent with those of Example 1.
[0056] Figure 1 Attached is the X-ray diffraction analysis spectrum of the composite positive electrode material of Example 1 and Comparative Example 1; Figure 1 It can be seen that the composite cathode material of Example 1 has typical characteristic peaks of elemental sulfur, LiNbO3 and LGPS, indicating that the preparation method of the composite cathode material is feasible.
[0057] Figure 2This is a SEM image of the composite cathode material of Example 1 before cycling; Figure 3 is a SEM image of the composite positive electrode material of Comparative Example 1 before cycling; Figure 2 and attached Figure 3 The particle sizes of the positive electrode materials in the comparative example 1 are relatively uniform, and the composite positive electrode material in the comparative example 1 retains a particle structure similar to that of the composite positive electrode material in the exemplary embodiment 1.
[0058] Figure 4 This is a SEM image of the composite cathode material of Example 1 after cycling; Figure 5 is a SEM image of the composite positive electrode material of Comparative Example 1 after cycling; Figure 4 and attached Figure 5 The positive electrode material after the medium cycle presents a relatively flat surface due to the application of pressure.
[0059] Figure 6 This is the first cycle GITT curve of the all-solid-state lithium-sulfur battery of Comparative Example 1; Figure 7 is the first cycle GITT curve of the all-solid-state lithium-sulfur battery of Example 1; Figure 6 and Figure 7 It can be seen that both the all-solid-state lithium-sulfur battery of Comparative Example 1 and the all-solid-state lithium-sulfur battery of Example 1 have typical charging and discharging platforms. By comparison, the all-solid-state lithium-sulfur battery of Example 1 has a wider charging and discharging platform, and the corresponding charging and discharging specific capacity is also higher.
[0060] Figure 8 The figure is a comparison of the cycle performance of the all-solid-state lithium-sulfur battery of Example 1 and Comparative Example 1. Figure 8 It can be seen that the all-solid-state lithium-sulfur battery of Example 1 has a higher discharge specific capacity and better cycle stability, indicating the feasibility of LiNbO3 as a positive electrode additive.
[0061] Those skilled in the art will appreciate that the above description is only a preferred embodiment of the present invention and does not limit the present invention. Any obvious improvements made to the present invention by those skilled in the art in combination with existing knowledge shall fall within the scope of protection defined by the claims of the present invention.
Claims
1. A LiNbO3-modified composite sulfur solid positive electrode material, characterized in that: The raw materials include, by mass percentage, 10%-20% of active sulfur material, 10%-20% of electronic conductor, 60%-70% of sulfide electrolyte and 5%-10% of LiNbO3.
2. The LiNbO3-modified composite sulfur solid positive electrode material according to claim 1, characterized in that: The active sulfur material includes any one of elemental sulfur and lithium sulfide.
3. The LiNbO3-modified composite sulfur solid positive electrode material according to claim 1, characterized in that: The electronic conductor includes any one of BP2000, Super P and CNTs.
4. The LiNbO3-modified composite sulfur solid positive electrode material according to claim 1, characterized in that: The sulfide electrolyte includes Li 10 GeP2S 12 Or any one of Li6PS5Cl.
5. A method for preparing a LiNbO3-modified composite sulfur solid positive electrode material as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: ball-milling the active sulfur material and the electronic conductor according to the mass ratio to obtain powder A, and calcining and melting the powder A at high temperature to obtain powder B; Step 2: Take the sulfide electrolyte and LiNbO3 according to the mass ratio and grind them together with the composite material B manually to obtain the composite positive electrode material C; The above steps are all carried out in an environment filled with inert gas Ar.
6. The method for preparing the LiNbO3-modified composite sulfur solid positive electrode material according to claim 5, characterized in that: The ball-to-material ratio of the ball mill is 50:1, the ball mill speed is 300 rpm / min, and the ball mill time is 12 hours.
7. The method for preparing the LiNbO3-modified composite sulfur solid positive electrode material according to claim 5, characterized in that: The high temperature calcination temperature is 155° C., and the calcination time is 12 hours.
8. The method for preparing the LiNbO3-modified composite sulfur solid positive electrode material according to claim 5, characterized in that: The manual grinding time is 30 minutes.
9. A LiNbO3-modified composite sulfur solid-state positive electrode material prepared by the method according to any one of claims 5 to 8.
10. An all-solid-state lithium-sulfur battery, characterized in that: A composite sulfur solid-state positive electrode material comprising LiNbO3 modified as claimed in claim 1 or 9.
Citation Information
Cited By
All-solid-state lithium-sulfur battery composite positive electrode and preparation method thereof
CN119725369A
Composite positive electrode for solid-state lithium-sulfur battery and preparation method of composite positive electrode
CN120955081A