Secondary battery and electric device
By designing a specific current collector structure in the secondary battery to optimize electrolyte penetration and lithium ion transmission, the problem of insufficient energy replenishment speed and safety performance of the secondary battery is solved, and higher energy density and cycle performance are achieved.
Patent Information
- Application Number
- CN202410864974.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
The energy replenishment speed of existing secondary batteries is still insufficient compared with the energy replenishment speed of fossil energy, and the endurance rate and safety performance under high-power operation are insufficient.
A current collector is designed, including a base layer, a metal layer and an intermediate layer. By controlling the thickness ratio of the intermediate layer, the metal layer and the second polymer layer, combined with the through-hole structure, the electrolyte penetration and lithium ion transmission path are optimized to improve Rate performance and cycle performance, and prevent burrs from being generated during external impact.
It effectively improves the energy density and cycle performance of secondary batteries, shortens the polarization during charge and discharge, enhances safety and stability, and improves the transmission rate of lithium ions and the storage capacity of electrolyte.
Smart Images

Figure BDA0004921228430000121 
Figure BDA0004921228430000131 
Figure BDA0004921228430000132
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a secondary battery and an electrical device. Background Art
[0002] With the continuous growth of energy demand, the energy crisis and environmental problems caused by traditional fossil fuels can no longer be ignored. The emergence of secondary batteries has successfully replaced the traditional fuel-driven mode with electronic equipment, effectively alleviating the environmental crisis and energy pressure. With the development of new energy vehicles, people's requirements for secondary batteries, its core components, are getting higher and higher.
[0003] Although secondary batteries have achieved good results in terms of high rate, high power, fast charging and discharging, and safety performance, their energy replenishment speed is still difficult to match that of fossil energy, and the actual endurance rate and safety performance under high-power operation are insufficient.
[0004] In view of this, this application is filed. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a secondary battery and an electrical device that can effectively improve the energy density. During the cycle, the rich through-hole structure not only shortens the lithium ion transmission distance, but also enhances the electrolyte infiltration, effectively improving the rate performance and cycle performance.
[0006] To achieve the above object, in a first aspect of the present application, the present application provides a secondary battery, comprising a current collector; the current collector comprises a substrate layer and a metal layer disposed on at least one surface of the substrate layer;
[0007] The base layer includes a first polymer layer and a second polymer layer disposed on at least one surface of the first polymer layer;
[0008] An intermediate layer is included between the base layer and the metal layer; the intermediate layer includes a polymer and a metal.
[0009] As an embodiment of the present application, the thickness of the intermediate layer is A, the thickness of the metal layer is B, and the thickness of the second polymer layer is C, satisfying: 0.25≤A / (B+C)≤0.5.
[0010] As an implementation scheme of the present application, at least one of the following (1) to (3) is satisfied:
[0011] (1) 0.3μm≤A≤1.5μm;
[0012] (2) 0.2μm≤B≤1μm;
[0013] (3)1μm≤C≤5μm.
[0014] As an embodiment of the present application, the current collector has through holes, and the volume of the through holes accounts for 60% to 70% of the total pore volume.
[0015] As an embodiment of the present application, the average pore diameter of the through holes is ≤1.5 μm.
[0016] As an embodiment of the present application, the porosity of the first polymer layer is P 1 The porosity of the second polymer layer is P 2 , satisfying: 1.2≤P 1 / P 2 ≤1.56.
[0017] As an embodiment of the present application, the average pore size of the first polymer layer is N 1 The average pore size of the second polymer layer is N 2 ; Satisfy: 2.5≤N 1 / N 2 ≤5.2.
[0018] As an implementation scheme of the present application, at least one of the following (a) to (d) is satisfied:
[0019] (a) 65% ≤ P 1 ≤85%;
[0020] (b) 45% ≤ P 2 ≤60%;
[0021] (c)2μm≤N 1 ≤3μm
[0022] (d) 0.5 μm ≤ N 2 ≤1μm.
[0023] As an embodiment of the present application, the thickness of the first polymer layer is 5 μm to 15 μm.
[0024] As an embodiment of the present application, the thickness of the current collector is 10 μm to 26 μm.
[0025] As an embodiment of the present application, the mass percentage of the metal in the intermediate layer is 10% to 30%.
[0026] In the second aspect of the present application, the present application provides an electrical device, including the secondary battery described above. The beneficial effect of the present invention is that the current collector described in the present application contains a metal layer, a first polymer layer, a second polymer layer, and an intermediate layer. The rich pore structure of the current collector can effectively promote the penetration of the electrolyte, shorten the infiltration time of the pole piece, improve the infiltration effect, shorten the transmission path of lithium ions during the charging and discharging process, increase the transmission rate of lithium ions, and reduce the polarization of the secondary battery during the charging and discharging process. Compared with the traditional metal current collector, the current collector avoids the generation of burrs when it is impacted by external forces, effectively prevents thermal runaway caused by short circuit of the positive and negative electrodes, adopts the first polymer layer and the second polymer layer, effectively improves the energy density, and during the cycle process, the electrolyte stored in the pore structure can replenish the electrolyte on the electrode surface consumed in the cycle process in time, effectively improving the rate performance and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a schematic diagram of the stacking structure of the secondary battery of the present application.
[0028] Figure 2 Schematic diagram of the structure of the current collector described in this application.
[0029] Figure 3 Schematic diagram of the through hole in the cross section of the current collector of the present application.
[0030] Figure 4 This is a SEM image of the second polymer layer of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the embodiments of the present application clearer, the technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0032] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0033] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0034] like Figure 1 As shown, an embodiment of the present application provides a secondary battery, including a stacked composite electrode sheet, wherein the composite electrode sheet includes a positive electrode 1, a negative electrode 2, and a current collector 3 located between the positive electrode and the negative electrode, and the separator 4 is arranged between adjacent composite electrode sheets.
[0035] In one embodiment, the current collector includes a base layer and a metal layer 34 disposed on at least one surface of the base layer;
[0036] The base layer includes a first polymer layer 31 and a second polymer layer 32 disposed on at least one surface of the first polymer layer;
[0037] An intermediate layer 33 is included between the base layer and the metal layer; the intermediate layer includes polymer and metal.
[0038] The present application creatively designs the structure of the current collector, which contains a first polymer layer, a second polymer layer, and a middle layer also containing a polymer, which can effectively promote the penetration of the electrolyte, shorten the wetting time of the electrode, improve the wetting effect, shorten the transmission path of lithium ions during the charging and discharging process, increase the transmission rate of lithium ions, reduce the polarization of the secondary battery during the charging and discharging process, avoid burrs when impacted by external forces, effectively prevent thermal runaway caused by short circuit of the positive and negative electrodes, and use the first polymer layer and the second polymer layer to effectively improve the energy density, inhibit the attenuation of the electrolyte during the cycle, and effectively improve the rate performance and cycle performance.
[0039] In one embodiment, the thickness of the intermediate layer is A, the thickness of the metal layer is B, and the thickness of the second polymer layer is C, satisfying: 0.25≤A / (B+C)≤0.5, for example, it can be 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or a range consisting of any two of these values. The present application satisfies this relationship by controlling the thickness of the intermediate layer, the metal layer, and the second polymer layer. The metal layer and the polymer have sufficiently high peel strength, and the electronic insulation of the upper and lower layers of the metal layer and the mechanical strength of the current collector are ensured, thereby improving the stability of the secondary battery during the cycle and the low self-discharge during storage.
[0040] In one embodiment, it satisfies: 0.3μm≤A≤1.5μm, for example, it can be 0.3μm, 0.4μm, 0.5μm, 0.6μm, 0.8μm, 1.0μm, 1.2μm, 1.5μm or a range consisting of any two of these values. The present application controls the thickness of the intermediate layer within this range, and on the premise of ensuring that the metal layer and the polymer have sufficiently high peel strength, ensures the electronic insulation of the upper and lower layers of the secondary battery electrode, thereby improving the cycle stability and storage stability.
[0041] In one embodiment, 0.2μm≤B≤1μm is satisfied, for example, it can be 0.2μm, 0.3m, 0.4μm, 0.5μm, 0.6μm, 0.8μm, 1.0μm or a range consisting of any two values therein. By controlling the thickness of the metal layer within this range, the present application can take into account the ohmic resistance and mass energy density of the current collector, thereby ensuring the rate charge and discharge performance and high energy density of the secondary battery. .
[0042] In one embodiment, the following is satisfied: 1 μm ≤ C ≤ 5 μm, for example, it can be 1 μm, 2 μm, 3 μm, 4 μm, 5 μm or a range consisting of any two values thereof. The present application controls the thickness of the second polymer layer within this range to ensure the mechanical strength of the current collector and the appropriate lithium ion diffusion distance, taking into account the safety performance and rate performance of the secondary battery.
[0043] In one embodiment, the current collector has through holes, and the volume of the through holes accounts for 60% to 70% of the total pore volume, for example, it can be 60%, 62%, 64%, 65%, 66%, 68%, 70% or a range consisting of any two of these values. The present application sets through holes and controls the proportion of the through hole volume to the total pore volume, so that the electrolyte passes through the current collector quickly, improves the wetting effect, shortens the wetting time, increases the transmission rate of lithium ions, and effectively improves the cycle performance and rate performance.
[0044] like Figure 3 As shown, the current collector has a cross section, and the cross section has through holes, half holes and closed holes. The through holes penetrate from the uppermost metal layer to the lowermost metal layer. Sufficient surfaces are cut along the current collector (generally 10 to 20 cross sections are required), and the volume of the through holes and the volume of the total holes (the sum of the pore volumes of the through holes, half holes and closed holes) are calculated. The average value is calculated to obtain the ratio of the through hole volume to the total pore volume.
[0045] like Figure 3 As shown, the present application does not limit the shape of the through hole, which can be tortuous or linear, as long as the through hole volume accounts for 60% to 70% of the total pore volume.
[0046] In one embodiment, the tortuosity of the current collector is 1.4 to 1.8, for example, it can be 1.4, 1.5, 1.6, 1.7, 1.8 or a range consisting of any two values therein, and the ratio of the resistance (Rb) of the porous medium in the saturated electrolyte to the resistance Re of the same volume of saturated electrolyte is calculated to obtain Nm=Rb / Re. It is calculated according to the formula tortuosity=(Nm*ε)1 / 2, where ε is the porosity.
[0047] In one embodiment, the average pore size of the through holes is ≤1.5 μm.
[0048] In one embodiment, the average pore size of the through hole is 0.5-1.5 μm, for example, it can be 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm, 1.1 μm, 1.2 μm, 1.3 μm, 1.4 μm, 1.5 μm or a range consisting of any two of these values.
[0049] In one embodiment, the porosity of the first polymer layer is P 1 The porosity of the second polymer layer is P 2 , satisfying: 1.2≤P 1 / P 2 ≤1.56, for example, it can be 1.2, 1.3, 1.4, 1.5, 1.56 or a range consisting of any two of these values. By controlling the porosity of the first polymer layer and the second polymer layer to satisfy this relationship, it is possible to promote rapid penetration and wetting of the electrolyte, increase the transmission rate of lithium ions, reduce the polarization of the secondary battery during the charge and discharge process, provide sufficient electrolyte storage space, and increase the cycle life.
[0050] In one embodiment, the average pore size of the first polymer layer is N 1 The average pore size of the second polymer layer is N 2 ; Satisfy: 2.5≤N 1 / N 2 ≤5.2, for example, it can be 2.5, 2.8, 3.0, 3.2, 3.5, 4, 4.2, 4.5, 5.0, 5.2 or a range consisting of any two of the values. By controlling the average pore size of the first polymer layer and the second polymer layer within this range, the current collector has a graded pore size, thereby ensuring the uniformity of the first polymer layer and the second polymer layer, improving the consistency and stability of the current collector, ensuring the peel strength between the two, promoting rapid penetration and wetting of the electrolyte, providing sufficient electrolyte storage space, and improving the cycle life.
[0051] Wherein, the SEM image of the second polymer layer is as follows Figure 4 As shown, through the SEM image, the porosity and average pore size of the second polymer layer can be statistically analyzed.
[0052] In one embodiment, 65%≤P 1 ≤85%, for example, it can be 65%, 68%, 70%, 72%, 75%, 76%, 78%, 80%, 82%, 85% or a range consisting of any two of these values.
[0053] In one embodiment, 45%≤P2 ≤60%, for example, it can be 45%, 48%, 50%, 52%, 55%, 56%, 58%, 60% or a range consisting of any two values therein.
[0054] In one embodiment, 2 μm ≤ N 1 ≤3μm, for example, it can be 2μm, 2.1μm, 2.2μm, 2.4μm, 2.5μm, 2.6μm, 2.8μm, 3μm or a range consisting of any two of these values.
[0055] In one embodiment, 0.5 μm ≤ N 2 ≤1 μm, for example, it may be 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1 μm or a range consisting of any two of these values.
[0056] In one embodiment, the thickness of the first polymer layer is 5 μm to 15 μm, for example, it can be 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm or a range consisting of any two of these values. Controlling the thickness of the first polymer layer within this range can effectively improve the mechanical strength of the current collector, avoid burrs when subjected to external impact, effectively prevent thermal runaway caused by short circuit of the positive and negative electrodes, and effectively improve the energy density.
[0057] In one embodiment, the first polymer layer can be made of synthetic fibers, natural cellulose and cellulose derivatives, wherein, exemplarily, the first polymer layer can be made of at least one of the following materials: bacterial cellulose (BC), polyethylene terephthalate (PET), PI, PVDF, polytetrafluoroethylene (PTFE).
[0058] More specifically, the first polymer layer is prepared by electrospinning.
[0059] In one embodiment, the first polymer layer is composed of nanowires of 100nm to 800nm interwoven to form a three-dimensional 3D film.
[0060] In one embodiment, the porosity of the first polymer layer is 65% to 85%, for example, 65%, 68%, 70%, 72%, 75%, 80%, 85% or a range consisting of any two values therein.
[0061] In one embodiment, the thickness of the current collector is 10 μm to 26 μm. For example, it can be 10 μm, 12 μm, 15 μm, 16 μm, 18 μm, 20 μm, 22 μm, 24 μm, 25 μm, 26 μm, or a range consisting of any two values therein. Controlling the thickness of the current collector within this range can ensure the mechanical strength of the current collector while taking into account excellent energy density.
[0062] In one embodiment, the mass percentage of the metal in the intermediate layer is 10% to 30%. By controlling the mass percentage of the metal in the intermediate layer to be within this range, the ohmic internal resistance can be reduced.
[0063] In one embodiment, the second polymer layer includes at least one of polyvinylidene fluoride-hexafluoropropylene polymer, polyvinylidene fluoride-polyacrylonitrile, polyvinylidene fluoride-trifluoroethylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyvinyl butyral, and polyvinylidene fluoride.
[0064] In one embodiment, the metal layer includes at least one of Au, Ag, Al, Cu, Ni, Ti, V, Cr, Mn, Co, Zn, Cd, Au-based alloy, Ag-based alloy, Al-based alloy, Cu-based alloy, and Ni-based alloy.
[0065] In one embodiment, the metal in the intermediate layer includes at least one of Au, Ag, Al, Cu, Ni, Ti, V, Cr, Mn, Co, Zn, Cd, Au-based alloy, Ag-based alloy, Al-based alloy, Cu-based alloy, and Ni-based alloy.
[0066] In one embodiment, the polymer in the intermediate layer includes at least one of polyvinylidene fluoride-hexafluoropropylene polymer, polyvinylidene fluoride-polyacrylonitrile, polyvinylidene fluoride-trifluoroethylene, polyvinylidene fluoride-chlorotrifluoroethylene, polyvinyl butyral, and polyvinylidene fluoride.
[0067] In one embodiment, the positive electrode includes a positive electrode active material, and the positive electrode active material can be selected from sodium iron composite oxide, sodium cobalt composite oxide, sodium manganese composite oxide, sodium nickel composite oxide, sodium nickel titanium composite oxide, sodium nickel manganese composite oxide, sodium iron manganese composite oxide, sodium nickel cobalt manganese composite oxide, sodium iron phosphate compound, sodium manganese phosphate compound, sodium cobalt phosphate compound, etc. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries can also be used. These positive electrode active materials can be used alone or in combination of two or more.
[0068] In one embodiment, the preparation method of the current collector is:
[0069] The spinning solution is electrospinned to form a spinning membrane, and hot-pressed to obtain a first polymer layer;
[0070] A polymer-containing slurry is coated on at least one surface of the first polymer layer, and the solvent in the slurry is quickly evaporated to promote phase separation to form a second polymer layer with through holes, semi-holes and closed holes, and the proportion of through holes is adjusted by controlling the solvent content.
[0071] The second polymer layer on at least one surface of the first polymer layer is plasma treated, and metal is deposited using pulsed DC magnetron sputtering technology to form a metal layer on at least one surface of the second polymer layer. When metal is deposited between the metal layer and the second polymer layer using pulsed DC magnetron sputtering technology, an intermediate layer including a polymer and a metal is formed to obtain the current collector of the present application.
[0072] In one embodiment, the spinning solution includes a polymer and a first solvent, and the solid-to-liquid ratio of the polymer to the first solvent is 1g:(5-15)mL, for example, it can be 1g:5mL, 1g:6mL, 1g:8mL, 1g:10mL, 1g:12mL, 1g:15mL or a range consisting of any two of these values.
[0073] In one embodiment, the evaporation temperature is 40-80°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C or a range consisting of any two of the values.
[0074] In one embodiment, the evaporation time is 24 to 72 hours, for example, it can be 24 hours, 30 hours, 36 hours, 42 hours, 48 hours, 54 hours, 60 hours, 66 hours, 72 hours or a range consisting of any two values therein.
[0075] In one embodiment, the first solvent includes at least one of water, trifluoroacetic acid, DMF, acetone, ethanol, and NMP.
[0076] In one embodiment, during the electrospinning, aluminum foil is used as a collector, and after the spinning is completed, the aluminum foil is separated from the spun material.
[0077] In one embodiment, the voltage of the electrospinning is 13-20 kV, for example, 13 kV, 14 kV, 15 kV, 16 kV, 18 kV, 20 kV or a range consisting of any two values therein.
[0078] In one embodiment, the hot pressing time is 1 to 10 minutes, and the hot pressing temperature is 90-120°C.
[0079] It should be noted that, in the present application, the porosity P of the first polymer layer is adjusted by controlling the hot pressing time and the hot pressing temperature. 1 , thereby adjusting the porosity ratio of the first polymer layer to the second polymer layer.
[0080] It should be noted that, in the present application, the average pore size N of the first polymer layer is adjusted by controlling the concentration of the polymer in the spinning solution or the polymer-containing slurry. 1 and the average pore size N of the second polymer layer 2 .
[0081] In one embodiment, the polymer-containing slurry includes a polymer and a second solvent.
[0082] In one embodiment, the solid-liquid ratio of the polymer to the second solvent is 1g:(4-10)mL, for example, 1g:4mL, 1g:5mL, 1g:6mL, 1g:8mL, 1g:10mL or a range consisting of any two of these values.
[0083] In one embodiment, the second solvent includes at least one of acetone and deionized water.
[0084] In one embodiment, inert gas protection is used during metal deposition for 5 to 30 minutes, for example, 5 minutes, 6 minutes, 8 minutes, 10 minutes, 12 minutes, 15 minutes, 20 minutes, 25 minutes, 30 minutes or a range consisting of any two values therein.
[0085] It should be noted that, in the present application, the metal content of the intermediate layer is adjusted by controlling the deposition time.
[0086] In one embodiment, the positive electrode further includes a conductive agent and a binder.
[0087] In one embodiment, the negative electrode includes a negative electrode active material, and the negative electrode active material can be natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, SiO, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO 2 , spinel structure lithium titanate Li 4 Ti 5 O 12 , at least one of Li-Al alloy and metallic lithium.
[0088] In one embodiment, the negative electrode further includes a conductive agent and a binder.
[0089] In one embodiment, the type of the conductive agent mentioned in the present application is not limited, and any known conductive agent can be used.
[0090] In one embodiment, the conductive agent includes at least one of carbon materials such as acetylene black, needle coke, carbon nanotubes, and graphene.
[0091] In one embodiment, the type of adhesive mentioned in the present application is not limited, and known adhesives can be used.
[0092] In one embodiment, the binder includes at least one of polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, nitrocellulose, styrene-butadiene rubber, nitrile rubber, fluororubber, isoprene rubber, polybutadiene rubber, ethylene-propylene rubber, styrene-butadiene-styrene block copolymer or its hydrogenate, ethylene-propylene-diene terpolymer, styrene-ethylene-butadiene-ethylene copolymer, styrene-isoprene-styrene block copolymer, isotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymer, propylene-α-olefin copolymer, polyvinylidene fluoride, polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and polytetrafluoroethylene-ethylene copolymer.
[0093] In one embodiment, the secondary battery may include an outer package, which can be used to encapsulate the electrode assembly and the electrolyte.
[0094] In one embodiment, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0095] In some embodiments, the secondary battery further comprises an electrolyte, and the type of the electrolyte is not subject to specific restrictions. The electrolyte comprises an electrolyte salt and an organic solvent, and the specific types of the electrolyte salt and the organic solvent are not subject to specific restrictions and can be selected according to actual needs. The electrolyte may also include additives, and the types of the additives are not particularly limited, and may be film-forming additives for the positive electrode and / or the negative electrode, or additives that can improve certain properties of the battery, such as additives that improve the high or low temperature performance of the battery.
[0096] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape.
[0097] An embodiment of the present application provides an electric device, comprising the secondary battery described above, wherein the secondary battery serves as a power supply for the electric device.
[0098] Exemplarily, the above-mentioned electrical devices may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0099] The present application is further described below with specific embodiments:
[0100] Example 1
[0101] A method for preparing a secondary battery:
[0102] Preparation of current collector :
[0103] (1) Preparation of base layer:
[0104] Take 1g PET and put it in a 20ml beaker, add 10ml trifluoroacetic acid, ultrasonically oscillate for 10min, stir for 24h to form a uniform, stable and transparent spinning solution, inject the spinning solution into the syringe, install it on the electrospinning machine, push the syringe at a speed of 0.002mm / s, adjust the spinning voltage to 15KV, and collect the electrospun membrane with aluminum foil as the collector. After spinning, remove the aluminum foil covered with the spinning membrane, vacuum dry it at 60℃ overnight, separate the aluminum foil from the spinning membrane, and hot press it at 120℃ for 10min to obtain the first polymer layer.
[0105] 8 g of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) and 2 g of succinonitrile (SN) were dissolved in 50 ml of acetone solution and stirred for 10 h to form a honey-like slurry, 5 ml of deionized water was added, and the mixture was stirred at 50° C. for 30 min. The mixture was evenly coated on both surfaces of the first polymer layer using a coating technology, evaporated at 50° C. for 48 h, and vacuum dried at 80° C. for 12 h to form a second polymer layer on both surfaces of the first polymer layer to obtain a substrate layer;
[0106] (2) Plasma treatment is performed on the substrate obtained in step (1), and metal deposition is performed by pulsed DC magnetron sputtering technology in a vacuum inert gas environment, and the deposition time is controlled to be 15 minutes. A Cu layer is deposited on one surface of the substrate layer, and an Al layer is deposited on the other surface, and an intermediate layer including Al and polyvinylidene fluoride-hexafluoropropylene is formed between the Al layer and the substrate layer, and an intermediate layer including Cu and polyvinylidene fluoride-hexafluoropropylene is formed between the Cu layer and the substrate layer to obtain a current collector.
[0107] Preparation of cathode slurry
[0108] (3) The positive electrode active material lithium iron phosphate, the conductive agent carbon black, and the binder PVDF are mixed in a ratio of 8:1:1, and NMP is added for homogenization to prepare a positive electrode slurry for use.
[0109] Preparation of negative electrode slurry :
[0110] (4) The negative electrode active material graphite, the conductive agent carbon black, and the binder SBR are mixed in a ratio of 8:1:1, and deionized water is added to mix and homogenize to form a negative electrode slurry for use.
[0111] Composite pole piece preparation:
[0112] (5) The positive electrode slurry is applied to the Al layer of the current collector and dried; the negative electrode slurry is applied to the Cu layer of the current collector and dried; and the composite electrode sheet is obtained by rolling and die-cutting.
[0113] Preparation of secondary batteries
[0114] (6) The composite electrodes are stacked in sequence with the positive electrode side facing the negative electrode side, the electrodes are separated by a diaphragm, and a secondary battery is prepared through steps such as hot pressing, shelling, packaging, liquid injection, formation, degassing, and capacity division.
[0115] The parameters of Example 1 are shown in Table 1 and Table 2.
[0116] Embodiments 2 to 8
[0117] The difference between Examples 2 to 8 and Example 1 is that Examples 2 to 8 adjust the value of A / (B+C) by changing the values of A, B, and C.
[0118] Embodiments 9 to 14
[0119] The difference between Examples 9 to 14 and Example 1 is that Examples 9 to 14 adjust the porosity P of the first polymer layer by controlling the hot pressing time and the hot pressing temperature. 1 and the porosity P of the second polymer layer 2 and P 1 :P 2 .
[0120] Embodiments 15 to 20
[0121] The difference between Examples 15 to 20 and Example 1 is that the concentration of the polymer in the spinning solution and the polymer-containing slurry in Examples 15 to 20 is adjusted to adjust the average pore size N of the first polymer layer. 1 and the average pore size N of the second polymer layer 2 and N 1 :N 2 .
[0122] Examples 21 to 24
[0123] The difference between Examples 21 to 24 and Example 1 is that Examples 21 to 24 adjust the evaporation temperature and time, thereby adjusting the through-hole ratio.
[0124] Examples 25 to 27
[0125] The difference between Examples 25 to 27 and Example 1 is that Examples 25 to 27 adjust the average pore size of the through holes by adjusting the amount of deionized water added in step (2).
[0126] Embodiments 28 to 29
[0127] The difference between Examples 28 and 29 and Example 1 is that Examples 28 and 29 adjust the deposition time and thus adjust the proportion of metal.
[0128] Embodiments 30 to 31
[0129] The difference between Examples 30 and 31 and Example 1 is that Examples 30 and 31 change the thickness of the first polymer layer.
[0130] Comparative Example 1
[0131] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses aluminum foil and copper foil of equal thickness (the thickness ratio of aluminum foil to copper foil is 1:1) to replace the current collector of Example 1.
[0132] Comparative Example 2
[0133] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses an aluminum foil of the same thickness to replace the first polymer layer of Example 1.
[0134] Table 1
[0135]
[0136]
[0137] Table 2
[0138]
[0139]
[0140] Performance Testing
[0141] Rate performance test: The capacity of all secondary batteries after 0.5C capacity division is recorded as C0, and 4C rate performance charge and discharge test is carried out based on C0.
[0142] Charging performance test: Copper wire was used to make three electrodes and they were charged at different rates from large to small at 25°C. The next rate was jumped when the potential of the negative electrode and the copper wire was 0. The capacity of all secondary batteries was adjusted to 20% SOC. The test cell was charged from 20% to 80% SOC to calculate the equivalent rate.
[0143] Energy density test: Weigh the secondary battery, charge it to 3.65V at 0.5C constant current and constant voltage, and then discharge it to 2.5V at 0.5C constant current. Record the discharge energy and calculate the mass energy density.
[0144] K value measurement: The half-charged battery is placed naturally at 25°C for 7 days, and the voltages V1 and V2 before and after discharge are recorded. K = (V1-V2) / (7*24).
[0145] Table 3
[0146]
[0147]
[0148]
[0149] It can be seen from Table 3 that the secondary battery of the present application has excellent mass energy density, rate charge and discharge performance, cycle performance and storage performance. The mass energy density, rate charge and discharge performance, cycle performance and storage performance of the embodiment are better than those of the comparative example.
[0150] By comparing Examples 1 to 5 with Examples 6 to 8, it can be seen that the present application improves the sufficiently high peel strength between the metal layer and the polymer by controlling 0.25≤A / (B+C)≤0.5, and ensures the electronic insulation of the upper and lower layers of the metal layer and the mechanical strength of the current collector, thereby improving the stability of the secondary battery during the cycle process and the low self-discharge during storage.
[0151] Comparing Examples 1, 10 to 13 with Examples 9 and 14, it can be seen that the present invention achieves the desired effect by controlling 1.2≤P 1 / P 2 ≤1.56, which can promote rapid penetration and wetting of electrolyte, increase the transmission rate of lithium ions, reduce the polarization of secondary batteries during charging and discharging, provide sufficient electrolyte storage space, and improve cycle life.
[0152] Comparing Examples 1, 16 to 19 with Examples 15 and 20, it can be seen that the present invention controls 2.5≤N 1 / N 2≤5.2, the current collector has a graded pore size, which ensures the uniformity of the first polymer layer and the second polymer layer, improves the consistency and stability of the current collector, ensures the peel strength between the two, promotes rapid penetration and wetting of the electrolyte, provides sufficient electrolyte storage space, and improves the cycle life.
[0153] By comparing Examples 1, 22 to 23 with Examples 21 and 24, it can be seen that the present application controls the pore volume to account for 60% to 70% of the total pore volume, so that the electrolyte can quickly pass through the current collector, thereby improving the wetting effect, shortening the wetting time, and increasing the lithium ion transmission rate, thereby effectively improving the cycle performance and rate performance.
[0154] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present application rather than to limit the scope of protection of the present application. Although the present application has been described in detail with reference to the preferred embodiments, ordinary technicians in this field should understand that the technical solution of the present application can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present application.
Claims
1. A secondary battery, It is characterized in that A current collector is included; the current collector includes a base layer and a metal layer disposed on at least one surface of the base layer; The base layer includes a first polymer layer and a second polymer layer disposed on at least one surface of the first polymer layer; An intermediate layer is included between the base layer and the metal layer; the intermediate layer includes a polymer and a metal.
2. The secondary battery according to claim 1, It is characterized in that The thickness of the intermediate layer is A, the thickness of the metal layer is B, and the thickness of the second polymer layer is C, satisfying: 0.25≤A / (B+C)≤0.
5.
3. The secondary battery according to claim 2, It is characterized in that Satisfy at least one of the following (1) to (3): (1) 0.3μm≤A≤1.5μm; (2) 0.2μm≤B≤1μm; (3)1μm≤C≤5μm.
4. The secondary battery according to claim 1, It is characterized in that The current collector has through holes, and the volume of the through holes accounts for 60% to 70% of the total pore volume.
5. The secondary battery according to claim 4, It is characterized in that The average pore diameter of the through holes is ≤1.5 μm.
6. The secondary battery according to claim 1, It is characterized in that The porosity of the first polymer layer is P 1 The porosity of the second polymer layer is P 2 , satisfying: 1.2≤P 1 / P 2 ≤1.56; and / or The average pore size of the first polymer layer is N 1 The average pore size of the second polymer layer is N 2 ; Satisfy: 2.5≤N 1 / N 2 ≤5.
2.
7. The secondary battery according to claim 6, It is characterized in that Satisfy at least one of the following (a) to (d): (a)65%≤P 1 ≤85%; (b)45%≤P 2 ≤60%; (c)2μm≤N 1 ≤3μm (d)0.5μm≤N 2 ≤1μm。 8. The secondary battery according to claim 1, It is characterized in that The thickness of the first polymer layer is 5 μm to 15 μm; and / or The thickness of the current collector is 10 μm to 26 μm.
9. The secondary battery according to claim 1, It is characterized in that The mass percentage of the metal in the intermediate layer is 10% to 30%.
10. An electrical device, It is characterized in that A secondary battery comprising any one of claims 1 to 9.
Citation Information
Cited By
Negative current collector and preparation method and application thereof