Metal negative electrode protective film, secondary battery, and electric device
By using an A-based protective film in a metal lithium battery, the fluoride of the A element reacts with the electrolyte to form a stable interface layer, which solves the problem of the negative electrode protective film consuming active lithium, improves the cycle life and safety of the battery, and inhibits dendrites. The formation of crystals.
Patent Information
- Application Number
- CN202310414201.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-29
AI Technical Summary
In existing metal lithium batteries, the formation and regeneration of the negative electrode protective film consumes active lithium, resulting in reduced battery capacity and short service life, and it is easy for dendrites to pierce the separator, causing short circuits and safety hazards.
A-based protective film is used, containing fluoride of A element (such as sodium, potassium, rubidium, cesium, magnesium, calcium), as the inactive layer of the metal negative electrode, forming a stable solid electrolyte interface layer through a self-limiting reaction with the electrolyte , reduce the consumption of active substances and inhibit the formation of dendrites.
It improves the electrochemical performance of the battery, extends the cycle life, reduces the impedance of the battery, enhances safety, and avoids the risk of dendrites piercing the separator.
Smart Images

Figure CN118867421A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of secondary batteries, and in particular to a metal negative electrode protective film, a secondary battery and an electrical device. Background Art
[0002] Secondary batteries are important materials for electric energy transfer and are widely used in new energy vehicles, portable electronic products, energy storage, etc. In recent years, the application of batteries in the field of electric vehicles has further increased our demand for high energy density and low-cost batteries, which has forced researchers to develop new high energy density battery systems.
[0003] Negative electrode materials are one of the key factors limiting the improvement of secondary battery energy density. Metal negative electrodes can significantly improve the energy density of secondary batteries due to their extremely high specific capacity and low electrode potential. However, most metal negative electrodes have problems such as dendrite growth, fast consumption of active materials, and high reactivity with electrolytes, which limit the application of metal negative electrodes. Taking lithium secondary batteries as an example, graphite negative electrodes are the key factor limiting the improvement of existing lithium-ion battery energy density. As a high energy density negative electrode material, metallic lithium can greatly improve the energy density of lithium batteries. Metallic lithium has extremely high reactivity, will react chemically / electrochemically with most electrolytes and cause rapid consumption of metallic lithium and electrolytes, reducing the coulombic efficiency of the battery. Lithium atoms have an oriented growth trend during the deposition process, so that metallic lithium tends to be deposited in a dendritic manner, which leads to huge volume deformation of metallic lithium during the cycle, making it difficult to form a stable solid electrolyte interface layer (Solid-Electrolyte Interphase, SEI) on the surface of metallic lithium, and there is a risk of lithium dendrites piercing the diaphragm and causing battery short circuit. At present, there are still some technical problems in directly using metallic lithium as a negative electrode in commercial applications.
[0004] The uneven deposition / stripping of lithium ions causes lithium dendrites to easily peel off from the main body of metal lithium and generate dead lithium, resulting in battery short circuit, which is very likely to cause battery explosion and cause safety hazards. The SEI formed by metal lithium during the cycle process is conducive to blocking the mutual consumption between metal lithium and electrolyte. However, conventional electrolytes either cannot generate a stable SEI on the metal lithium electrode, thereby failing to provide long-term, high-efficiency protection for metal lithium batteries, or cause the passage of solvent molecules and other ions other than lithium ions in the electrolyte, causing them to react with the metal lithium negative electrode to generate by-products, consuming the active substances in the battery, or the generated SEI has a weak conductivity for lithium ions, increasing the impedance of the battery and reducing the rate performance of the battery. Therefore, constructing a negative electrode protective film (SEI) with high stability, strong lithium conductivity, and strong ability to inhibit side reactions is a key factor in improving the electrochemical performance of metal lithium batteries.
[0005] In traditional lithium metal batteries, the formation and / or regeneration of the negative electrode protection film (SEI) on the surface of lithium metal consumes lithium ions, which leads to the following problems: (1) the content of active lithium in the battery is reduced, and the battery capacity is reduced; (2) the lithium ions consumed by the formation and / or regeneration of the traditional lithium metal negative electrode protection film come from the electrolyte and / or the positive electrode. Since the lithium content in the electrolyte and the positive electrode is very limited, the regeneration of SEI will quickly consume the active lithium in the battery, thereby reducing the battery life. The research papers "Electroless Formation of a Fluorinated Li / Na Hybrid Interphase for Robust Lithium Anodes" and "Improving metallic lithium anode with NaPF6 additive in LiPF6-carbonate electrolyte" reported that the negative electrode protection film (SEI) containing sodium can improve the electrochemical performance of the negative electrode, but the sodium element in the SEI comes from the electrolyte or the positive electrode, making it difficult to maintain the long-term stability of the SEI structure, limiting the long-term cycle performance of the battery.
[0006] Therefore, there is an urgent need in the art to develop a new type of metal negative electrode protective film that can overcome the above-mentioned technical defects. Summary of the invention
[0007] In order to solve the problems existing in the prior art, including: 1. The side reaction between the metal negative electrode and the electrolyte continues to occur, and the formation and regeneration of the metal negative electrode SEI consumes a large amount of active substances; 2. The electrolyte cannot generate a stable SEI on the metal negative electrode, thereby failing to provide long-term, high-efficiency protection for the negative electrode; 3. The SEI of the metal negative electrode has a weak conductivity to the active material elements, which increases the impedance of the battery, reduces the rate performance of the battery, and the negative electrode is prone to dendrite growth. On the one hand, the present disclosure provides an A-based protective film for the metal negative electrode of a secondary battery, wherein the A-based protective film conducts the B element as an active substance in the electrolyte of the secondary battery;
[0008] The metal negative electrode comprises a negative electrode base layer, the negative electrode base layer comprises at least one inactive layer containing element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium.
[0009] The B element is different from the A element and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the B element is lower than that of the A element.
[0010] Wherein, the A-based protective film contains fluoride of element A and is located on at least part of the surface of the negative electrode substrate layer of the metal negative electrode. The formation and regeneration of the A-based protective film consumes the inactive substances of the negative electrode substrate layer, thereby reducing the consumption of the active substance element B, which is one of the core innovations of the present invention. In the present invention, the active material undergoes a valence change in a reversible manner during the battery charging and discharging process, and a reversible electrochemical reaction occurs. The inactive layer is a functional auxiliary layer for achieving uniform deposition of active materials. The functional auxiliary layer is a key material for forming a negative electrode protective film (SEI) and dynamically repairing the negative electrode protective film. The B element ions are reduced in the form of B element metal during charging, and the B element metal is oxidized to B element ions during discharging, so the active material is B element metal. Specifically, the A element is not embedded in the positive electrode material or the positive electrode material is preferentially embedded in the B element, so the A element ions cannot be reversibly embedded and removed in the positive electrode material, that is, the A element ions cannot reversibly gain and lose electrons during the battery charging and discharging process, that is, they cannot reversibly participate in the battery charging and discharging.
[0011] In some embodiments of the present disclosure, the A-based protective film includes a solid electrolyte interface (SEI) film constructed on the surface of the negative electrode substrate layer, a SEI film formed in situ by the electrolyte and the negative electrode substrate layer, or a combination thereof.
[0012] In some embodiments of the present disclosure, the A-based protective film further comprises a fluoride of the B element.
[0013] In some embodiments of the present disclosure, the electrolyte contains fluorine-containing anions. Preferably, the fluorine-containing anions contained in the electrolyte are selected from at least one of bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate.
[0014] In some embodiments of the present disclosure, the in-situ formation of the SEI film includes formation through a self-limiting reaction between the negative electrode substrate layer and the electrolyte under battery charge and discharge or non-charge and discharge conditions.
[0015] In another aspect, the present disclosure provides a method for preparing the A-based protective film, the method comprising:
[0016] (1) melting an A element metal and an optional auxiliary metal under the protection of an inert gas, and obtaining a negative electrode substrate layer including at least one inactive layer containing the A element after cooling;
[0017] (2) compounding the negative electrode substrate layer onto the current collector surface to obtain a metal negative electrode; and
[0018] (3) Under the protection of an inert gas, the metal negative electrode is brought into contact with an electrolyte to form an A-based protective film on at least a portion of the surface of the negative electrode base layer.
[0019] In some embodiments of the present disclosure, the electrolyte comprises fluoride.
[0020] In some embodiments of the present disclosure, the inert gas includes at least one of nitrogen, argon and neon.
[0021] In some embodiments of the present disclosure, the concentration of the electrolyte is between 0.5 mol / L and 7 mol / L.
[0022] In another aspect, the present disclosure provides a secondary battery, comprising a positive electrode plate, an electrolyte, a metal negative electrode plate, and the A-based protective film, wherein the metal negative electrode comprises a negative electrode base layer, the negative electrode base layer comprises at least one inactive layer containing an A element, and the A element is at least one of sodium, potassium, rubidium, cesium, magnesium, and calcium,
[0023] The electrolyte includes a B element as an active material;
[0024] The B element is different from the A element and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the B element is lower than that of the A element.
[0025] Wherein, the A-based protective film contains fluoride of element A and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
[0026] In some embodiments of the present disclosure, the metal negative electrode further includes a negative electrode enhancement film located on at least a portion of the surface of the A-based protective film.
[0027] In some embodiments of the present disclosure, the A element and the B element are combined in any of the following ways: a combination of magnesium element and sodium element, a combination of magnesium element and lithium element, a combination of magnesium element and potassium element, a combination of magnesium element and calcium element, a combination of sodium element and potassium element, a combination of sodium element and lithium element, a combination of sodium element and calcium element, a combination of calcium element and potassium element, a combination of calcium element and lithium element, or a combination of potassium element and lithium element.
[0028] In some embodiments of the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound.
[0029] On the other hand, the present disclosure provides an electrical device including the secondary battery.
[0030] The surface of the metal negative electrode plate of the secondary battery in the present invention can form a stable A-based protective film (such as a sodium-based protective film), which is generated by a self-limiting reaction between the negative electrode substrate layer and the electrolyte. The composition is mainly inorganic fluoride, the structure is stable, and it is difficult to dissolve in the electrolyte. The formation and regeneration of the A-based protective film consumes the inactive substances in the negative electrode substrate layer, thereby reducing the consumption of active substances. It has a strong ion (for example, lithium ion) conduction ability, promotes ions to obtain electrons and reduce on the surface of the negative electrode substrate layer, and inhibits the generation of dendrites. At the same time, the conduction ability of the solvent molecules in the electrolyte is weak, avoiding adverse side reactions at the negative electrode, thereby inhibiting the decomposition of the electrolyte and the loss of active substances, maintaining the stability of the metal negative electrode plate structure, and improving the electrochemical performance of the battery.
[0031] The negative electrode substrate layer of the present invention is selected from single substances of sodium, potassium, rubidium, cesium, magnesium and calcium or alloys of sodium, potassium, rubidium, cesium, magnesium and calcium as an inactive layer. When the B element metal is deposited on the surface of the negative electrode substrate layer in the form of dendrites, the B element metal and the A element metal in the negative electrode substrate layer form a primary battery in a local range. The A and B elements have different redox reaction potentials. Driven by the redox potential difference, the B atoms in the B element dendrites are dissolved in the form of B element ions, pass through the A-based protective film, and re-obtain electrons on the negative electrode surface to be reduced and deposited. After the B element ions that pass through the A-based protective film are deposited again on the negative electrode surface, they can quickly diffuse and dissolve with the negative electrode substrate layer, thereby eliminating the B element dendrites.
[0032] In the present invention, element B is used as an active material, which reversibly gains and loses electrons and reversibly changes valence during the battery charge and discharge process. The negative electrode substrate layer containing the inactive substance element A is a functional auxiliary material for achieving uniform deposition of element B metal and eliminating dendrite growth. This functional auxiliary material is a key material for forming a negative electrode protective film (ie, SEI) and dynamically repairing the negative electrode protective film, and is also one of the core points of the present invention.
[0033] These and other features and advantages will become apparent by reading the following detailed description and by reference to the associated drawings.It is to be understood that the foregoing general description and the following detailed description are illustrative only and are not restrictive of the aspects of what is claimed. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a schematic diagram of the structure of a metal negative electrode plate with an A-based protective film in a specific embodiment of the present application.
[0035] Figure 2 This is a SEM image of the negative electrode base layer in Example 7 of the present application after the battery cycle is completed.
[0036] Figure 3This is a SEM image of the negative electrode substrate layer in Comparative Example 6 of the present application after the battery cycle is completed. DETAILED DESCRIPTION
[0037] The present application is described in detail below in conjunction with the accompanying drawings, and the features of the present application will be further revealed in the following specific description.
[0038] "Scope" disclosed herein is defined in the form of lower limit and upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a particular range. The scope defined in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a particular parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0039] In this application, if there is no special description, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution. In this application, if there is no special description, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0040] In this application, unless otherwise specified, the terms "include" and "comprising" mentioned herein may be open-ended or closed-ended. For example, the terms "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0041] In the description herein, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0042] It should be understood that, in the description of the present invention, the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0043] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0044] In order to solve the problems of dendrite formation and active material consumption in the metal negative electrode of the prior art during the charge and discharge cycle, while maintaining the high energy density of the battery, the present disclosure provides an A-based protective film for the metal negative electrode of a secondary battery, by constructing the A-based protective film on a metal negative electrode sheet containing a metal single substance of sodium, potassium, rubidium, cesium, magnesium, calcium or an alloy of sodium, potassium, rubidium, cesium, magnesium, and calcium as the negative electrode substrate layer, thereby inhibiting the reaction between the electrolyte and the negative electrode, reducing the loss of active metals and electrolytes, promoting the migration and diffusion of ions, and inhibiting the formation of dendrites to improve the electrochemical performance of the battery. In the secondary battery, the A metal or A alloy inactive layer serves as the negative electrode substrate layer of the negative electrode sheet. When the redox reaction potential of the B element is lower than that of the A element, the A metal or A alloy negative electrode substrate layer can eliminate the B metal dendrites deposited on its surface. In addition, the negative electrode base layer containing element A can be used as the source of element A in the negative electrode protective film. The negative electrode base layer is an inactive layer. By consuming inactive substances, it provides element A for the formation and regeneration of the A-based protective film, which can reduce the consumption of active substance element B and has the function of protecting element B. As mentioned above, active substance elements have a direct impact on battery capacity, reversibly gain and lose electrons during battery charging and discharging, and participate in charge transfer. Inactive substance elements have no direct impact on battery capacity and cannot participate in charge transfer during battery charging and discharging in a reversible form.
[0045] In the present disclosure, metal dendrites are eliminated through the principle of galvanic cell, providing the possibility of eliminating the formation of metal dendrites from the principle level. The present disclosure adopts an inactive layer containing A element metal or A alloy as the negative electrode substrate layer, and adopts B element as the active material. When B element ions are deposited on the surface of the A-containing inactive layer in the form of dendrites, B element metal dendrites and A-containing inactive layer form a galvanic cell in a local area. The redox potential of B element is lower than that of A element. Driven by the redox potential difference between A element and B element, B metal dendrites are dissolved in the form of B element ions and obtain electrons on the surface of the A-containing inactive layer to reduce and deposit. A element metal and B element metal fuse with each other, and B element metal deposited on the surface of A element metal can diffuse rapidly with A element metal, thereby avoiding the formation of B element metal dendrites. The present disclosure is different from the mechanism of suppressing the formation of metal dendrites by two or more cations acting as carriers in the prior art. The A element ions in the present disclosure do not act as carriers and reversibly participate in the charge transfer during the battery charging and discharging process, but eliminate B metal dendrites through the mechanism of galvanic cell and the formation of BA alloy. The present invention uses cations of a single metal as carriers, which is beneficial to reducing the manufacturing, use and management costs of the battery.
[0046] In order to inhibit the reaction between the electrolyte and the negative electrode, reduce the loss of active materials and electrolytes, and promote the migration and diffusion of ions, the A-based protective film for the metal negative electrode of the secondary battery of the present invention can conduct the B element as the active material in the electrolyte of the secondary battery. Preferably, the A-based protective film can hinder the passage of solvent molecules, thereby avoiding their contact with the negative electrode base layer in the metal negative electrode; wherein the metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing the A element, and the A element is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium, the B element is different from the A element, and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the B element is lower than that of the A element, wherein the A-based protective film contains the fluoride of the A element and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
[0047] In a specific embodiment, the A element and the B element are combined in any of the following ways: a combination of magnesium element and sodium element, a combination of magnesium element and lithium element, a combination of magnesium element and potassium element, a combination of magnesium element and calcium element, a combination of sodium element and potassium element, a combination of sodium element and lithium element, a combination of sodium element and calcium element, a combination of calcium element and potassium element, a combination of calcium element and lithium element, or a combination of potassium element and lithium element.
[0048] In a specific embodiment, the A-based protective film may include at least one layer, wherein the A-based protective film includes a solid electrolyte interface (SEI) film (artificially) constructed on the surface of the negative electrode substrate layer, an SEI film formed in situ by the electrolyte and the negative electrode substrate layer, or a combination thereof, for example, a single-layer or multi-layer SEI film formed by a mixed combination of artificial construction and in situ reaction.
[0049] In a specific embodiment, for the case where the A-based protective film is formed by the in-situ reaction of the sodium negative electrode substrate layer with the electrolyte, the main component of the A-based protective film is an inorganic salt containing cations of the element A. The A-based protective film with the inorganic salt as the main component has high structural stability and is difficult to dissolve in the electrolyte, which is beneficial to improving the long-cycle stability of the battery and inhibiting the formation of metal dendrites.
[0050] In a specific embodiment, the electrolyte contains fluorine-containing anions, preferably, the fluorine-containing anions contained in the electrolyte are selected from at least one of bisfluorosulfonyl imide, hexafluorophosphate, bistrifluoromethanesulfonyl imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate. In a preferred embodiment, the electrolyte contains hexafluorophosphate of B element cations. In a preferred embodiment, the anion that undergoes a self-limiting reaction with the negative electrode substrate is hexafluorophosphate. The reaction of the fluorine-containing anions with the negative electrode substrate can form an A-based protective film with higher ionic conductivity, improve the stability of the A-based protective film, and limit the adverse side reactions of the electrolyte with the negative electrode substrate.
[0051] In a specific embodiment, the in-situ formation of the SEI film includes formation through a self-limiting reaction between the negative electrode substrate layer and the electrolyte under battery charge-discharge or non-charge-discharge conditions.
[0052] like Figure 1 As shown, the negative electrode plate 1 includes a current collector 11, at least one layer of inactive material containing element A metal or element A alloy formed on the surface of the current collector 11 as a negative electrode base layer 12, an A-based negative electrode protection film 13 formed on at least a portion of the surface of the negative electrode base layer 12, and a negative electrode reinforcement film 14 formed on at least a portion of the surface of the A-based negative electrode protection film 13.
[0053] In one embodiment of the present disclosure, a method for preparing the A-based protective film includes:
[0054] (1) Under the protection of an inert gas, melt the A element metal, or the A element and any other optional alloy material, and after cooling, obtain a negative electrode substrate layer including at least one inactive layer containing the A element; in a specific embodiment, under the protection of an inert gas, heat a metal single substance of sodium, potassium, magnesium, or calcium, or a mixture of a metal single substance of sodium, potassium, magnesium, or calcium and a certain proportion of other alloy materials to completely melt and fully and evenly stir, and after cooling, obtain a negative electrode substrate layer composed of a metal single substance of sodium, potassium, magnesium, or calcium, or an alloy of sodium, potassium, magnesium, and calcium;
[0055] (2) compounding the negative electrode base layer onto the surface of the current collector to obtain a metal negative electrode; in a specific embodiment, the negative electrode base layer is heated under the protection of an inert gas, and a conductive carrier (current collector) is brought into contact with the negative electrode base layer to obtain a metal negative electrode loaded with the negative electrode base layer and the conductive carrier; and
[0056] (3) Under the protection of an inert gas, the metal negative electrode is brought into contact with the electrolyte to form an A-based protective film on at least a portion of the surface of the negative electrode base layer. In a specific embodiment, under the protection of an inert gas, the metal negative electrode that has not been cooled is inserted into the electrolyte for quenching to obtain a metal negative electrode having an A-based protective film.
[0057] In a specific embodiment, the electrolyte contains fluoride, and the time for the negative electrode substrate layer to contact and react with the electrolyte to generate the A-based protective film is 0.1-20 hours, 0.5-15 hours, 1-10 hours, 3-8 hours, or any numerical range consisting of the end values of the above ranges. When the reaction time for generating the A-based protective film is within the above range, the A-based protective film has a high ionic conductivity, can effectively block the adverse side reactions between the negative electrode substrate layer and the electrolyte, inhibit the formation of dendrites, improve the battery production efficiency, and reduce the battery manufacturing cost.
[0058] In some embodiments of the present disclosure, the inert gas includes at least one of nitrogen, argon and neon.
[0059] In some embodiments of the present disclosure, the concentration of the electrolyte is between 0.5mol / L and 7mol / L, between 1mol / L and 6mol / L, between 3mol / L and 5mol / L, or any numerical range formed by the end values of the above ranges. When the concentration of the electrolyte is within the above range, the electrolyte has high ionic conductivity, strong operability, good wettability, and can efficiently form an A-based protective film with high ionic conductivity and stable structure on the surface of the negative electrode base layer to inhibit the formation of dendrites.
[0060] In the present disclosure, a secondary battery includes a positive electrode plate, an electrolyte, a metal negative electrode plate and the A-based protective film, wherein the metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium, the electrolyte includes element B as an active substance, which is at least one of lithium, sodium, potassium, magnesium and calcium, the element B is a different element from A, and the redox reaction potential of B is lower than that of element A, wherein the A-based protective film contains a fluoride of element A and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
[0061] In some embodiments of the present disclosure, the metal negative electrode further includes a negative electrode enhancement film located on at least a portion of the surface of the A-based protective film.
[0062] In some embodiments of the present disclosure, the A element and the B element are combined in any of the following ways: a combination of magnesium element and sodium element, a combination of magnesium element and lithium element, a combination of magnesium element and potassium element, a combination of magnesium element and calcium element, a combination of sodium element and potassium element, a combination of sodium element and lithium element, a combination of sodium element and calcium element, a combination of calcium element and potassium element, a combination of calcium element and lithium element, or a combination of potassium element and lithium element.
[0063] In some embodiments of the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound.
[0064] In another preferred embodiment, the positive electrode plate active material does not undergo a reversible electrochemical reaction with the A element ions or preferentially undergoes a reversible electrochemical reaction with the B element ions; preferably, the positive electrode plate active material is a polyanion salt type, a metal oxide type, or a compound type.
[0065] In some embodiments of the present disclosure, the B element is lithium, the A element is sodium, and the positive electrode plate includes at least one of lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese iron phosphate and lithium manganese phosphate.
[0066] In the present disclosure, the electrolyte comprises a solvent and a fluorine-containing salt. The electrolyte comprises at least one anion selected from fluorine-containing anions; preferably, at least one selected from bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate.
[0067] In the present disclosure, the solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound. In a preferred embodiment, the solvent is an ether solvent. More preferably, the solvent is ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, polyethylene glycol dimethyl ether, ethylene glycol methyl ether ethyl ether, ethylene glycol diethyl ether, diethylene glycol methyl ether ethyl ether, diethylene glycol diethyl ether, triethylene glycol methyl ether ethyl ether, triethylene glycol diethyl ether, tetraethylene glycol methyl ether ethyl ether, tetraethylene glycol diethyl ether, ethylene glycol methyl ether propyl ether, ethylene glycol ethyl ether propyl ether, ethylene glycol dipropyl ether, diethylene glycol methyl ether propyl ether, diethylene glycol dipropyl ether, triethylene glycol methyl ether propyl ether, triethylene glycol ethyl ether At least one of propyl ether, triethylene glycol dipropyl ether, tetraethylene glycol methyl ether propyl ether, tetraethylene glycol ethyl ether propyl ether, tetraethylene glycol dipropyl ether, ethylene glycol methyl ether butyl ether, ethylene glycol ethyl ether butyl ether, ethylene glycol propyl ether butyl ether, ethylene glycol dibutyl ether, diethylene glycol methyl ether butyl ether, diethylene glycol ethyl ether butyl ether, diethylene glycol propyl ether butyl ether, diethylene glycol dibutyl ether, triethylene glycol methyl ether butyl ether, triethylene glycol ethyl ether butyl ether, triethylene glycol propyl ether butyl ether, triethylene glycol dibutyl ether, tetraethylene glycol methyl ether butyl ether, tetraethylene glycol ethyl ether butyl ether, tetraethylene glycol propyl ether butyl ether, and tetraethylene glycol dibutyl ether. When the electrolyte solvent is selected from the above range, the reaction activity of the solvent with the negative electrode substrate layer is low, the structure of the negative electrode substrate layer and the A-based protective film is stable, the ionic conductivity of the electrolyte and the A-based protective film is high, dendrite formation is suppressed, the battery charge and discharge coulomb efficiency is high, and the service life is long.
[0068] In the present disclosure, the concentration of the fluoride salt in the electrolyte is 0.5mol / L-7mol / L, 1mol / L-5mol / L, 2mol / L-4mol / L or any numerical range consisting of the end values of the above ranges. In some embodiments of the present application, the electrolyte also includes additives, and the additives include, but are not limited to: 1,3-dioxolane, 1,4-dioxane, trioxymethylene, lithium nitrate, lithium fluorosulfonate, sulfur dioxide, fluoroethylene carbonate, 12-crown ether-4, 15-crown ether-5 and 18-crown ether-6. In some embodiments, the mass content of the additive in the electrolyte is 0.1% to 20%, 1% to 15% or 5% to 10%.
[0069] Secondary battery
[0070] The secondary battery of the present application includes a positive electrode (pole sheet), a negative electrode (pole sheet), a separator (optional), an electrolyte / liquid or solid electrolyte, etc. During the battery charging and discharging process, active ions are embedded and extracted back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet.
[0071] [Positive electrode]
[0072] In the secondary battery of the present application, the positive electrode plate includes a positive electrode current collector and a positive electrode film layer (or positive electrode active material layer) disposed on at least one surface of the positive electrode current collector and including a positive electrode active material. For example, the positive electrode current collector has two surfaces opposite to each other in the thickness direction of itself, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector. In the secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector, for example, the metal foil may be an aluminum foil, and the composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene PP, polyethylene terephthalate PET, polybutylene terephthalate PBT, polystyrene PS, polyethylene PE and its copolymers, etc.).
[0073] In the secondary battery of the present application, the positive electrode active material containing the B metal element may be a positive electrode active material for a secondary battery known in the art. For example, the positive electrode active material may include one or more of the following: a layered oxide containing B element ions, a polyanion material, or a Prussian blue material. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for secondary batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more.
[0074] In some embodiments, the positive electrode film layer may also optionally include a binder. Non-limiting examples of binders that can be used for the positive electrode film layer may include one or more of the following: polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin. In an embodiment of the present application, the first positive electrode active material layer and / or the second positive electrode active material layer each independently contain a binder selected from polyvinylidene fluoride, polyacrylic acid, polytetrafluoroethylene, polyimide and combinations thereof.
[0075] In some embodiments, the positive electrode film layer may also optionally include a conductive agent. Examples of conductive agents for the positive electrode film layer may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers. In an embodiment of the present application, the first positive electrode active material layer and / or the second positive electrode active material layer each independently contain a conductive agent of graphite, carbon black, acetylene black, graphene, carbon nanotubes and a combination of the above substances.
[0076] In one embodiment of the present application, the positive electrode can be prepared in the following manner: the above-mentioned components for preparing the positive electrode, such as the positive electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0077] [Negative electrode]
[0078] In the secondary battery of the present application, the negative electrode plate does not exclude other additional functional layers in addition to the negative electrode base layer. For example, in some embodiments, the negative electrode plate of the present application may also include a conductive primer layer (e.g., composed of a conductive agent and a binder) sandwiched between the negative electrode current collector and the negative electrode base layer and disposed on the surface of the negative electrode current collector. In some other embodiments, the negative electrode plate of the present application may also include a covering protective layer covering the surface of the second negative electrode film layer.
[0079] In the secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector, for example, the metal foil may be a copper foil, a silver foil, an iron foil, or a foil composed of an alloy of the above metals. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer, and may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material base layer (such as a base layer made of materials such as polypropylene PP, polyethylene terephthalate PET, polybutylene terephthalate PBT, polystyrene PS, polyethylene PE and copolymers thereof).
[0080] [Electrolytes]
[0081] The electrolyte plays the role of conducting ions between the positive electrode plate and the negative electrode plate. The electrolyte can be selected from at least one of a solid electrolyte, a semi-solid electrolyte and a liquid electrolyte. In one embodiment of the present application, the electrolyte may also optionally contain additives. For example, the additives may include one or more of the following: negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain properties of the battery, such as additives that improve the overcharge performance of the battery, additives that improve the high temperature performance of the battery, additives that improve the low temperature performance of the battery, etc.
[0082] [Isolation film]
[0083] In one embodiment of the present application, the secondary battery further comprises a separator, which separates the anode side of the secondary battery from the cathode side, and provides selective permeation or blocking for substances of different types, sizes and charges in the system. For example, the separator can insulate electrons, physically isolate the positive and negative electrodes of the secondary battery, prevent internal short circuits and form an electric field in a certain direction, and allow ions in the battery to pass through the separator and move between the positive and negative electrodes. In one embodiment of the present application, the material used to prepare the separator may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer may be the same or different. In an embodiment of the present application, the separator is selected from polyolefin separators, polyester separators, polyimide separators, polyamide separators and cellulose separators.
[0084] In one embodiment of the present application, the positive electrode sheet, the negative electrode sheet and the separator can be made into an electrode assembly / bare cell by a winding process or a lamination process.
[0085] In one embodiment of the present application, the secondary battery may include an outer package, which can be used to encapsulate the above-mentioned electrode assembly and electrolyte. In some embodiments, the outer package of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. In other embodiments, the outer package of the secondary battery can be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.
[0086] The shape of the secondary battery of the present application may be cylindrical, square or any other shape. The outer packaging may include a shell and a cover plate, and the shell may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell has an opening connected to the receiving cavity, and the cover plate can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the separator can form an electrode assembly through a winding process or a lamination process, and the electrode assembly is encapsulated in the receiving cavity, and the electrolyte is impregnated in the electrode assembly. The number of electrode assemblies contained in the secondary battery may be one or more.
[0087] In one embodiment of the present application, a plurality of secondary batteries may be assembled together to form a battery module, wherein the battery module includes two or more secondary batteries, and the specific number depends on the application of the battery module and the parameters of a single battery module.
[0088] In the battery module, the plurality of secondary batteries may be arranged in sequence along the length direction of the battery module. Of course, they may also be arranged in any other manner. The plurality of secondary batteries may further be fixed by fasteners. Optionally, the battery module may further include a housing having a storage space, and the plurality of secondary batteries are stored in the storage space.
[0089] In one embodiment of the present application, two or more of the above-mentioned battery modules can be assembled into a battery pack, and the number of battery modules contained in the battery pack depends on the application of the battery pack and the parameters of the individual battery modules. The battery pack may include a battery box and a plurality of battery modules disposed in the battery box, and the battery box includes an upper box body and a lower box body, and the upper box body can cover the lower box body and match well with it to form a closed space for accommodating the battery modules. Two or more battery modules can be arranged in the battery box in a desired manner.
[0090] In one embodiment of the present application, an exemplary battery pack may include a battery box and a plurality of battery modules disposed in the battery box. The battery box includes an upper box body and a lower box body, wherein the upper box body is used to cover the lower box body and form a closed space for accommodating the battery modules. The plurality of battery modules may be arranged in the battery box in any manner.
[0091] Electrical devices
[0092] In one embodiment of the present application, the electric device of the present application includes at least one of the secondary battery, battery module, or battery pack of the present application, and the secondary battery, battery module, or battery pack can be used as a power source of the electric device, and can also be used as an energy storage unit of the electric device. The electric device includes but is not limited to mobile digital devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0093] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0094] In the following, the influence of the secondary battery manufactured according to the embodiment of the present application on the performance of the electrochemical device is characterized based on specific examples, but it should be pointed out that the protection scope of the present application is defined by the claims and is not limited to the above specific embodiments.
[0095] Example
[0096] Unless otherwise specified, all raw materials used in the present invention are analytically pure and all water is deionized water.
[0097] 1. Preparation of positive electrode
[0098] 10 wt% of polyvinylidene fluoride was dissolved in N-methylpyrrolidone as a binder, and 80 wt% of a polyanion salt-type positive electrode active material containing element B (see Table 1-4 for details) and 10 wt% of conductive carbon black were added to prepare a uniformly dispersed positive electrode slurry. The positive electrode slurry was evenly coated on the surface of the aluminum foil current collector and transferred to a vacuum oven for thorough drying. The obtained positive electrode sheet was rolled and punched to obtain the target positive electrode disc.
[0099] 2. Preparation of negative electrode sheet
[0100] In an Ar atmosphere, element A metal (see Table 1-4 for details) or element A metal and other alloy component powders are placed in a stainless steel crucible and heated until completely melted and fully stirred, and then cooled to obtain an inactive layer material containing element A.
[0101] The inactive layer material containing element A is compounded on the surface of the copper foil by cold pressing or hot pressing to obtain a negative electrode substrate layer with a layered structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by atomization spraying or sputtering to obtain a negative electrode substrate layer with a granular structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by extrusion to obtain a negative electrode substrate layer with a strip structure. Alternatively, the inactive layer material containing element A is compounded on the surface of the copper foil by atomization spraying or sputtering to obtain a negative electrode substrate layer with a three-dimensional structure.
[0102] The negative electrode reinforcement film material is compounded on the surface of the negative electrode base layer by cold pressing or hot pressing to obtain a negative electrode plate.
[0103] 3. Preparation of Isolation Membrane
[0104] A polypropylene porous polymer film is used as the isolation membrane.
[0105] 4. Preparation of Electrolyte
[0106] Under an Ar atmosphere, a fully dried fluorine-containing salt (see Table 1-4 for details) or a non-fluorine-containing salt (lithium nitrate) is dissolved in an organic solvent of ethylene glycol dipropyl ether, and the mixture is stirred well to prepare an electrolyte.
[0107] 5. Preparation of button cells
[0108] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and the electrolyte is added to assemble into a button battery.
[0109] According to the above preparation method, button batteries of Examples 1 to 20 and Comparative Examples 1 to 11 were prepared.
[0110] According to the test results of Examples 1 to 4 and Comparative Examples 1 to 5 in Table 1, when the A element is sodium and the B element is lithium (Example 1, Na-Li); the A element is magnesium and the B element is lithium (Example 2, Mg-Li), the A element is calcium and the B element is lithium (Example 3, Ca-Li), or the A element is sodium and the B element is calcium (Example 4, Na-Ca) (all satisfying that the redox potential of the B element is lower than that of the A element), the negative electrode substrate layer containing the A element can effectively inhibit the formation of metal dendrites of the B element, and the ion conduction ability of the A-based protective film is strong, which can effectively inhibit the occurrence of adverse side reactions in the battery. The secondary battery has good cycle performance (expressed in the number of cycles, <500 is "poor", 500-530 is "medium", and >530 is "excellent") and first cycle coulomb efficiency (expressed in the first cycle efficiency). According to the test results of Comparative Example 1 (Li-Na), when the redox reaction potential of element B is higher than that of element A, the structure of the negative electrode substrate layer containing element A is unstable, and the formation of metal dendrites of element B cannot be effectively suppressed, and the cycle life and first cycle coulomb efficiency of the secondary battery are reduced. According to the test results of Comparative Example 2 (Cu-Li) and Comparative Example 3 (Mg-Zn), when element A is not one of sodium, potassium, rubidium, cesium, magnesium, and calcium, and / or element B is not one of lithium, sodium, potassium, magnesium, and calcium, the negative electrode substrate layer containing element A cannot suppress the generation of metal dendrites of element B, and the A-based protective film cannot suppress the formation of metal dendrites of element B and the occurrence of adverse side reactions, and the cycle life and first cycle coulomb efficiency of the secondary battery are reduced. According to the test results of Comparative Example 4 (Li-Li) and Comparative Example 5 (Na-Na), when element A and element B are the same element, the A-based protective film cannot effectively suppress the generation of dendrites, which will also cause the cycle life and first cycle coulomb efficiency of the secondary battery to decrease.
[0111]
[0112] Table 1
[0113] According to the test results of Examples 5 to 12 and Comparative Examples 6 to 7 in Table 2, when the electrolyte contains fluorine-containing anions, the main component of the A-based protective film includes metal fluorides, which have high ion conductivity and structural stability, can effectively inhibit the formation of metal dendrites of the B element, inhibit the occurrence of adverse side reactions in the battery, and improve the coulombic efficiency and cycle performance of the battery. According to the test results of Comparative Examples 6 to 7, when the electrolyte does not contain fluorine-containing anions, the ion conductivity of the negative electrode protective film is weak, it is difficult to inhibit the adverse side reactions between the negative electrode base layer and the electrolyte and the formation of metal dendrites of the B element, and the coulombic efficiency and cycle performance of the battery are poor.
[0114] Figure 2 This is a SEM image of the negative electrode substrate layer in Example 7 of the present application after the battery cycle is completed. Figure 2 As shown, when the electrolyte contains fluoride-containing anions, there are almost no dendrites in the negative electrode base layer.
[0115] Figure 3 This is a SEM image of the negative electrode substrate layer in Comparative Example 6 of the present application after the battery cycle is completed. Figure 3 As shown, when the electrolyte does not contain fluoride-containing anions, a large number of dendrites exist in the negative electrode base layer.
[0116]
[0117] Table 2
[0118] According to the test results of Examples 13 to 16 and Comparative Examples 8 to 9 in Table 3, when the film-forming reaction time of the A-based protective film is between 0.1 hours and 20 hours, the A-based protective film has a higher ion conductivity, can effectively block the adverse side reactions between the negative electrode substrate layer and the electrolyte, the battery has a higher coulombic efficiency and cycle stability, and the battery production efficiency is high. According to the test results of Comparative Example 8, when the film-forming time of the A-based protective film is too short, the film-forming effect of the A-based protective film is not ideal, it is difficult to effectively block the adverse side reactions between the negative electrode substrate layer and the electrolyte, the negative electrode is prone to form B element metal dendrites, and the coulombic efficiency and cycle stability of the battery are poor. According to the test results of Comparative Example 9, when the film-forming reaction time of the A-based protective film is too long, although the electrochemical performance of the battery is not significantly affected, the production efficiency of the battery is low, resulting in high production costs of the battery.
[0119]
[0120] Table 3
[0121] According to the test results of Examples 17 to 20 and Comparative Examples 10 to 11 in Table 4, when the concentration of the electrolyte is in the range of 0.5 mol / L to 7 mol / L, the electrolyte has good film-forming performance of the A-based protective film, the electrolyte has high ionic conductivity and wettability, the polarization is small during the battery cycle, and the formation of metal dendrites of the B element can be effectively suppressed, and the adverse side reactions are suppressed, and the battery has high coulombic efficiency and cycle performance. According to the test results of Comparative Example 10, when the electrolyte concentration is too small, the film-forming performance of the electrolyte is weak, the A-based protective film is difficult to effectively suppress the adverse side reactions between the negative electrode base layer and the electrolyte, the negative electrode forms B element metal dendrites, the active material and the electrolyte are consumed quickly, and the coulombic efficiency and cycle performance of the battery are poor. According to the test results of Comparative Example 11, when the concentration of the electrolyte is too large, the viscosity of the electrolyte is high, the ionic conductivity is low, the polarization is large during the battery cycle, the negative electrode is prone to dendrite formation, and the coulombic efficiency and cycle performance of the battery are poor.
[0122]
[0123] Table 4
[0124] Test Method
[0125] 1. Cycle performance test
[0126] At 25°C, the secondary batteries prepared in the examples and comparative examples were subjected to full charge and discharge cycle tests at a rate of 0.5C. The cycles were operated in this way, and the number of cycles when the capacity of the battery was less than or equal to 80% of the initial capacity was recorded as the nth cycle. The larger n is, the better the cycle performance of the battery. n greater than 530 cycles indicates excellent cycle performance, n in the range of 500-530 cycles indicates average cycle performance, and n less than 500 cycles indicates poor cycle performance.
Claims
1. An A-based protective film for a metal negative electrode of a secondary battery, wherein the A-based protective film conducts the B element as an active material in the electrolyte of the secondary battery; in, The metal negative electrode includes a negative electrode base layer, the negative electrode base layer includes at least one inactive layer containing an element A, and the element A is at least one of sodium, potassium, rubidium, cesium, magnesium and calcium, The B element is different from the A element and is at least one of lithium, sodium, potassium, magnesium and calcium, and the redox reaction potential of the B element is lower than that of the A element. Wherein, the A-based protective film contains fluoride of element A and is located on at least a portion of the surface of the negative electrode base layer of the metal negative electrode.
2. The A-based protective film according to claim 1, characterized in that: The A-based protective film includes a solid electrolyte interface (SEI) film artificially constructed on the surface of the negative electrode substrate layer, or an SEI film formed in situ by the electrolyte and the negative electrode substrate layer, or a combination thereof; preferably, the in situ formed SEI film is formed by a self-limiting reaction occurring between the negative electrode substrate layer and the electrolyte.
3. The A-based protective film according to claim 1, characterized in that: The A-based protective film further contains a fluoride of the B element.
4. The A-based protective film according to claim 2, characterized in that: The electrolyte contains fluorine-containing anions. Preferably, the fluorine-containing anions contained in the electrolyte are at least one selected from bis(fluorosulfonyl)imide, hexafluorophosphate, bis(trifluoromethanesulfonyl)imide, difluorooxalatoborate, tetrafluoroborate, hexafluoroarsenate and difluorophosphate.
5. The A-based protective film according to claim 2, characterized in that: The solvent of the electrolyte is selected from at least one of an ether compound, an acetal compound and a ketal compound.
6. The A-based protective film according to claim 2, characterized in that: The concentration of the electrolyte is between 0.5 mol / L and 7 mol / L.
7. A secondary battery comprising a positive electrode plate, an electrolyte, a metal negative electrode plate and the A-based protective film according to any one of claims 1 to 6.
8. The secondary battery according to claim 7, characterized in that: Also included is a negative electrode enhancement film located on at least a portion of the surface of the A-based protective film.
9. The secondary battery according to claim 7, characterized in that: The element A and the element B are combined in any of the following ways: a combination of magnesium and sodium, a combination of magnesium and lithium, a combination of magnesium and potassium, a combination of magnesium and calcium, a combination of sodium and potassium, a combination of sodium and lithium, a combination of sodium and calcium, a combination of calcium and potassium, a combination of calcium and lithium, or a combination of potassium and lithium.
10. An electrical device comprising the secondary battery according to any one of claims 7 to 9.