Resin composition, cured product, prepreg, metal foil-clad laminate, resin composite sheet, printed wiring board, and semiconductor device

By blending a polyphenylene ether compound with a carbon-carbon unsaturated double bond and an aromatic vinyl polymer into a resin with an indane skeleton, the problems of difficulty in curing the resin and high dielectric loss tangent (Df) are solved. A resin composition with excellent formability and improved dielectric properties.

CN118871484APending Publication Date: 2024-10-29MITSUBISHI GAS CHEM CO INC

Patent Information

Application Number
CN202380027131.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-14
Filing Date
2023-03-13
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The resin with an indane skeleton used in the prior art is difficult to fully solidify and has a high dielectric loss tangent (Df), which cannot meet the requirements for formability and dielectric properties of semiconductor components and printed circuit boards.

Method used

By blending a polyphenylene ether compound having a carbon-carbon unsaturated double bond at the terminal and a specified aromatic vinyl polymer into a resin having an isopropenyl group at the terminal and an indane skeleton, a dielectric loss angle with excellent moldability can be obtained. A resin composition with low tangent (Df).

Benefits of technology

The resin composition is fully cured and the dielectric loss tangent (Df) is reduced, thereby improving the formability and dielectric properties of printed circuit boards and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118871484A_ABST
    Figure CN118871484A_ABST
Patent Text Reader

Abstract

Provided are a resin composition having excellent moldability and low dielectric loss tangent (Df), a cured product, a prepreg, a metal foil-clad laminate, a resin composite sheet, a printed wiring board, and a semiconductor device. A resin composition containing 10-300 parts by mass of a polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal and 10-300 parts by mass of a polymer having a structural unit represented by formula (V) per 100 parts by mass of a resin (A) having an indane skeleton and a terminal group represented by formula (T1). # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin composition, a cured product, a prepreg, a metal foil-clad laminate, a resin composite sheet, a printed wiring board, and a semiconductor device. Background Art

[0002] In recent years, semiconductor elements used in electronic devices such as portable terminals and communication devices have been increasingly integrated and miniaturized. In response, technologies that enable high-density mounting of semiconductor elements are required, and improvements are also required on printed circuit boards, which play an important role in this process.

[0003] On the other hand, the use of electronic devices and the like is diversified and continues to expand. Influenced by this, the various properties required of printed circuit boards, metal foil laminates, prepregs, etc. used therein are also diversified and stricter. In order to obtain a printed circuit board that takes into account such required properties and has been improved, various materials and processing methods have been proposed. As one of them, the improvement and development of resin materials constituting prepregs and resin composite sheets can be cited.

[0004] Patent Document 1 discloses a resin having an isopropenylphenyl group at the terminal and an indane skeleton as a material suitable for a semiconductor sealing material and a printed wiring board.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2021-143333 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] However, if the resin having an indane skeleton described in the above-mentioned patent document 1 is used directly, it will not be fully cured. Therefore, a novel resin composition obtained by blending with other compounds, especially other thermosetting compounds, is required. In particular, a resin composition having excellent formability and low dielectric loss tangent (Df) is required.

[0010] The present invention aims to solve the above problems and to provide a resin composition having excellent moldability and low dielectric loss tangent (Df), and a cured product, a prepreg, a metal foil-clad laminate, a resin composite sheet, a printed wiring board, and a semiconductor device.

[0011] Solutions for solving problems

[0012] The present inventors have studied to solve the above problems by blending a polyphenylene ether compound having a terminal carbon-carbon unsaturated double bond and a predetermined aromatic vinyl polymer into a resin having an isopropenyl group at the terminal and having an indane skeleton.

[0013] Specifically, the above-mentioned problems are solved by the following means.

[0014] <1> A resin composition comprising 10 to 300 parts by mass of a polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal and 10 to 300 parts by mass of a polymer having a structural unit represented by formula (V), relative to 100 parts by mass of a resin (A) having an indane skeleton and having a terminal group represented by formula (T1).

[0015]

[0016] (In formula (T1), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, and y represents an integer of 0 to 4. * represents a bonding position to another site.)

[0017]

[0018] (In formula (V), Ar represents an aromatic hydrocarbon linking group. * represents a bonding position.)

[0019] <2> according to <1> The resin composition, wherein the resin (A) comprises a resin represented by formula (T1-1).

[0020]

[0021] (In formula (T1-1), R is a group containing a structural unit represented by formula (Tx). Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom. y is an integer of 0 to 4.)

[0022]

[0023] (In formula (Tx), n, o and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, and 1.0≤n+o+p≤20.0. Ma each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom. x represents an integer from 0 to 4. Each of the structural units (a), (b), and (c) is bonded to the structural unit (a), (b), (c), or other groups at *, and each structural unit may be randomly bonded.)

[0024] <3> according to <1> or <2> In the resin composition, the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal includes a polyphenylene ether compound represented by formula (OP).

[0025]

[0026] (In formula (OP), X represents an aromatic group, -(YO) n1 - represents a polyphenylene ether structure, n1 represents an integer of 1 to 100, and n2 represents an integer of 1 to 4. Rx is a group represented by formula (Rx-1) or formula (Rx-2).

[0027]

[0028] (In formula (Rx-1) and formula (Rx-2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group. * represents a bonding site with an oxygen atom. Mc each independently represents a hydrocarbon group having 1 to 12 carbon atoms. z represents an integer of 0 to 4. r represents an integer of 1 to 6.

[0029] <4> according to <1> ~ <3> The resin composition described in any one of the preceding claims, wherein the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal includes a polyphenylene ether compound represented by formula (OP-1).

[0030]

[0031] (In formula (OP-1), X represents an aromatic group, -(YO)n2- represents a polyphenylene ether structure, and R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group, n1 represents an integer of 1 to 6, n2 represents an integer of 1 to 100, and n3 represents an integer of 1 to 4.)

[0032] <5> according to <1> ~ <4> The resin composition described above, wherein the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal has a number average molecular weight (Mn) of 500 to 3000 and a weight average molecular weight (Mw) of 800 to 6000.

[0033] <6> according to <1> ~ <5> The resin composition described above, wherein the number average molecular weight (Mn) of the resin (A) is 400 to 3,000.

[0034] <7> according to <1> ~ <6> The resin composition according to any one of the preceding claims, wherein the mass ratio of the resin (A) is 10 to 50 parts by mass relative to 100 parts by mass of the total of the resin (A) and the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond.

[0035] <8> according to <1> ~ <7> The resin composition described above does not substantially contain a polymerization inhibitor.

[0036] <9> according to <1> ~ <8> The resin composition described in any one of the above further comprises another compound (C) other than the resin (A), the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal, and the polymer having a structural unit represented by formula (V).

[0037] <10> according to <9> The resin composition, wherein the other compound (C) comprises one or more selected from the group consisting of a maleimide compound, a cyanate compound, an epoxy compound, a phenol compound, a compound containing a (meth)allyl group (e.g., an alkenyl nadic imide compound), an oxetane resin, a benzoxazine compound, an arylcyclobutene resin, a polyamide resin, a polyimide resin, a perfluorovinyl ether resin, a compound having a styrene group other than the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal, a compound having an isopropenyl group other than the resin (A) having an indane skeleton, a multifunctional (meth)acrylate compound other than the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal, an elastomer, and a petroleum resin.

[0038] <11> according to <1> ~ <10> The resin composition described in any one of the preceding claims, wherein the total content of the resin (A) and the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond is 40 parts by mass or more relative to 100 parts by mass of the resin solid content in the resin composition.

[0039] <12> according to <1> ~ <11> The resin composition described above further comprises a filler (D).

[0040] <13> according to <12> The resin composition described above, wherein the content of the filler (D) is 10 to 1000 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0041] <14> according to <1> ~ <13> The resin composition according to any one of the preceding claims, wherein the resin (A) comprises a resin represented by formula (T1-1),

[0042] The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal includes a polyphenylene ether compound represented by formula (OP-1),

[0043] The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal has a number average molecular weight (Mn) of 500 to 3000 and a weight average molecular weight (Mw) of 800 to 6000.

[0044] The number average molecular weight (Mn) of the resin (A) is 400 to 3000,

[0045] The mass ratio of the resin (A) is 10 to 50 parts by mass relative to 100 parts by mass of the total of the resin (A) and the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond,

[0046] The resin composition contains substantially no polymerization inhibitor.

[0047] The total content of the resin (A) and the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond is 40 parts by mass or more relative to 100 parts by mass of the resin solid content in the resin composition.

[0048]

[0049] (In formula (T1-1), R is a group containing a structural unit represented by formula (Tx). Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom. y is an integer of 0 to 4.)

[0050]

[0051] (In formula (Tx), n, o and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, and 1.0≤n+o+p≤20.0. Ma each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom. x represents an integer from 0 to 4. Each of the structural units (a), (b), and (c) is bonded to the structural unit (a), (b), (c), or other groups at *, and each structural unit may be randomly bonded.)

[0052]

[0053] (In formula (OP-1), X represents an aromatic group, -(YO)n2- represents a polyphenylene ether structure, and R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group, n1 represents an integer of 1 to 6, n2 represents an integer of 1 to 100, and n3 represents an integer of 1 to 4.)

[0054] <15> <1> ~ <14> A cured product of any one of the resin compositions.

[0055] <16> A prepreg comprising a base material and <1> ~ <14> The resin composition described in any one of the above is formed.

[0056] <17> A metal foil-clad laminate comprising: <16> At least one layer formed of the prepreg, and a metal foil disposed on one or both sides of the layer formed of the prepreg.

[0057] <18> A resin composite sheet comprising: a support body, and a <1> ~ <14> A layer formed from any one of the resin compositions.

[0058] <19> A printed circuit board comprises an insulating layer and a conductor layer arranged on the surface of the insulating layer, wherein the insulating layer comprises <1> ~ <14> A layer formed from any one of the resin compositions.

[0059] <20> A semiconductor device comprising <19> The printed circuit board.

[0060] Effects of the Invention

[0061] According to the present invention, a resin composition having excellent moldability and low dielectric loss tangent (Df), and a cured product, a prepreg, a metal foil-clad laminate, a resin composite sheet, a printed wiring board, and a semiconductor device can be provided. BRIEF DESCRIPTION OF THE DRAWINGS

[0062] Figure 1 The NMR spectrum of Synthesis Example 1 is shown. DETAILED DESCRIPTION

[0063] Hereinafter, a mode for implementing the present invention (hereinafter, simply referred to as "this embodiment") will be described in detail. It should be noted that the following this embodiment is an example for describing the present invention, and the present invention is not limited to only this embodiment.

[0064] In addition, in this specification, "to" is used to mean that the numerical values ​​described before and after it are included as a lower limit and an upper limit.

[0065] In this specification, various physical property values ​​and characteristic values ​​are values ​​at 23° C. unless otherwise specified.

[0066] In the description of the group (atomic radical) in this specification, the description of not indicating substitution and unsubstituted includes the group (atomic radical) without substitution, and also includes the group (atomic radical) with substitution. For example, "alkyl" includes not only the alkyl without substitution (unsubstituted alkyl), but also includes the alkyl with substitution (substituted alkyl). In this specification, the description of not indicating substitution and unsubstituted is preferably unsubstituted.

[0067] In the present specification, (meth)allyl means both or either of allyl and methallyl, “(meth)acrylate” means both or either of acrylate and methacrylate, “(meth)acrylic acid” means both or either of acrylic acid and methacrylic acid, and “(meth)acryloyl” means both or either of acryloyl and methacryloyl.

[0068] In the present specification, the term "process" includes not only an independent process but also a process that cannot be clearly distinguished from other processes as long as the intended effect of the process can be achieved.

[0069] When the measurement methods and the like described in the standards shown in this specification differ depending on the year, unless otherwise specified, the standards as of January 1, 2022 are applied.

[0070] In the present specification, the resin solid content refers to the components excluding fillers and solvents, and means including the resin (A), the polyphenylene ether compound (B) and the polymer having the structural unit represented by the formula (V), and other compounds (C) and other resin additive components (additives such as flame retardants, etc.) blended as needed.

[0071] In this specification, relative dielectric constant and dielectric constant are used with the same meaning.

[0072] The resin composition of the present embodiment comprises: a resin (A) having an indane skeleton and a terminal group represented by formula (T1) (sometimes also simply referred to as "resin (A)"), a polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal (sometimes also simply referred to as "polyphenylene ether compound (B)"), and a polymer having a structural unit represented by formula (V). Specifically, the resin composition of the present embodiment is characterized in that, relative to 100 parts by mass of the resin (A) having an indane skeleton and a terminal group represented by formula (T1), it comprises 10 to 300 parts by mass of the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal and 10 to 300 parts by mass of the polymer having a structural unit represented by formula (V).

[0073]

[0074] (In formula (T1), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, and y represents an integer of 0 to 4. * represents a bonding position to another site.)

[0075]

[0076] (In formula (V), Ar represents an aromatic hydrocarbon linking group. * represents a bonding position.)

[0077]

[0078] (In formula (T1), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, and y represents an integer of 0 to 4. * represents a bonding position to another site.)

[0079] By setting it as such a structure, the resin composition which is excellent in moldability and has a low dielectric loss tangent (Df) when it is made into a cured product can be obtained.

[0080] The resin (A) with the terminal group shown in the formula (T1) and with the indane skeleton is difficult to polymerize alone. In addition, if the compound with compatibility with the resin (A) is not used in combination, phase separation is easily caused. In the present embodiment, it is inferred that by blending the polyphenylene ether compound (B) with a carbon-carbon unsaturated double bond at the end and the polymer with the structural unit shown in the formula (V) in the resin (A) at a specified ratio, the compatibility is improved, and a resin composition with excellent formability can be obtained. In addition, it is inferred that because the resin (A) has an indane skeleton, it is possible to obtain a resin composition that can reduce the dielectric loss tangent (Df) when making a cured product. In addition, it is inferred that by using a polymer with the structural unit shown in the formula (V), the dielectric loss tangent (Df) of the cured product obtained can be further reduced.

[0081] Furthermore, in the present embodiment, a resin composition with low melt viscosity can be obtained. When the melt viscosity is low, for example, when a resin with high melt viscosity and poor formability is mixed, the minimum melt viscosity can be reduced, and formability can be improved. In addition, in the present embodiment, a resin composition with high heat resistance can be obtained.

[0082] <Resin (A) Having a Terminal Group Represented by Formula (T1) and an Indane Skeleton>

[0083] The resin composition of the present embodiment includes a resin (A) having an indane skeleton and a terminal group represented by the formula (T1). By using the resin (A), a resin composition having excellent low dielectric properties (Dk and / or Df) can be obtained.

[0084]

[0085] (In formula (T1), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, and y represents an integer of 0 to 4. * represents a bonding position to another site.)

[0086] In formula (T1), Mb is preferably a hydrocarbon group having 1 to 10 carbon atoms which may be substituted by a halogen atom, more preferably a hydrocarbon group having 1 to 5 carbon atoms which may be substituted by a halogen atom, and further preferably a hydrocarbon group having 1 to 3 carbon atoms which may be substituted by a halogen atom. Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom, preferably a fluorine atom or a chlorine atom. Mb is preferably a hydrocarbon group having 1 to 12 carbon atoms which is not substituted by a halogen atom.

[0087] The hydrocarbon group is preferably an alkyl group, more preferably a linear alkyl group. Mb is preferably a methyl group or an ethyl group.

[0088] y is preferably an integer of 0 to 3, more preferably an integer of 0 to 2, further preferably 0 or 1, and even more preferably 0.

[0089] The resin (A) may have terminal groups represented by the formula (T1) at all or only some of the terminals of each resin molecule.

[0090] The number of terminal groups represented by the formula (T1) in the resin molecule of the resin (A) is preferably 2.

[0091] The resin (A) has an indane skeleton. The resin molecules contained in the resin (A) are not particularly limited as long as at least one molecule has at least one indane skeleton, but the number of indane skeletons in the resin molecules of the resin (A) is preferably one or more per molecule, and more preferably 1 to 20. By forming such a structure, there is a tendency to more effectively exert the effect of the present invention.

[0092] The resin (A) preferably includes a structural unit represented by the following formula (Txn).

[0093]

[0094] (In the formula (Txn), n is the average number of repeating units, which is a number greater than 0 and 20 or less. Ma each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, and x represents an integer of 0 to 4.)

[0095] In the formula (Txn), Ma is each independently preferably a hydrocarbon group having 1 to 10 carbon atoms which may be substituted by a halogen atom, more preferably a hydrocarbon group having 1 to 5 carbon atoms which may be substituted by a halogen atom, and further preferably a hydrocarbon group having 1 to 3 carbon atoms which may be substituted by a halogen atom. Examples of the halogen atom include a fluorine atom, a chlorine atom, and a bromine atom, preferably a fluorine atom or a chlorine atom. Ma is each independently preferably a hydrocarbon group having 1 to 12 carbon atoms which is not substituted by a halogen atom. The aforementioned hydrocarbon group is preferably an alkyl group, more preferably a straight-chain alkyl group.

[0096] As Ma, a methyl group or an ethyl group is particularly preferred.

[0097] x is preferably an integer of 0 to 3, more preferably an integer of 0 to 2, further preferably 0 or 1, and even more preferably 0.

[0098] The resin (A) more preferably includes a resin represented by the formula (T1-1), and more preferably includes a resin represented by the formula (T1-1-2).

[0099]

[0100] (In formula (T1-1), R is a group containing a structural unit represented by formula (Tx). Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom. y is an integer of 0 to 4.)

[0101] In formula (T1-1), Mb and y have the same meanings as Mb and y in formula (T1), and the preferred ranges are also the same.

[0102]

[0103] (In formula (T1-2), R is a group containing a structural unit represented by formula (Tx).)

[0104]

[0105] (In formula (Tx), n, o and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, and 1.0≤n+o+p≤20.0. Ma each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom. x represents an integer from 0 to 4. Each of the structural units (a), (b), and (c) is bonded to the structural unit (a), (b), (c), or other groups at *, and each structural unit may be randomly bonded.)

[0106] In formula (Tx), n, o and p each refer to the average number of repeating units in all molecules in the resin.

[0107] In the formula (Tx), the sum of n, o and p is preferably 1.1≤n+o+p, more preferably 1.2≤n+o+p, further preferably 1.5≤n+o+p, further preferably 2.0≤n+o+p, further preferably 2.5≤n+o+p, further preferably 3.0≤n+o+p, and particularly further preferably 3.3≤n+o+p. In addition, in the formula (Tx), the sum of n, o and p is preferably n+o+p≤20.0, more preferably n+o+p≤10.0, further preferably n+o+p≤8.0, further preferably n+o+p≤7.0, and further preferably n+o+p≤6.4. The sum of n, o and p can be calculated by the method described in the Examples described later.

[0108] In the formula (Tx), Ma and x have the same meanings as Ma and x in the formula (Txn), and the preferred ranges are also the same.

[0109] The resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)) is further preferably such that the parameter α calculated by formula (α) is greater than or equal to 0.55 and less than or equal to 1.00, and the parameter β calculated by formula (β) is greater than or equal to 0.20 and less than or equal to 3.00. By making the parameters α and β within the above ranges, there is a tendency that the obtained cured product has low dielectric properties (Dk and / or Df) and excellent heat resistance.

[0110]

[0111]

[0112] (The brackets in formula (α) and formula (β) represent 1 The integral value between corresponding chemical shift values ​​in H-NMR. )

[0113] Here, α represents the ratio of the structural unit having an indane skeleton (structural unit (a) in formula (Tx)) in the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)). More specifically, it is speculated that by adjusting the structural unit having an indane skeleton to a range that satisfies the above-mentioned parameter α, the obtained resin molecule has high rigidity and can increase the glass transition temperature. Furthermore, it is speculated that molecules with high rigidity have lower mobility than molecules with low rigidity, and have a long relaxation time during dielectric relaxation, which can reduce Df. α can be increased by diluting the concentration of the raw materials, using a high-polarity solvent, increasing the amount of catalyst, increasing the reaction temperature, and other conditions when synthesizing the resin represented by formula (T1-1).

[0114] On the other hand, β limits the double bond ratio at the end of the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)). More specifically, it is speculated that, for example, the number of crosslinking points with the functional groups possessed by other compounds (C) described later increases, and a network is easily formed during thermal curing, so that a cured product with a high glass transition temperature and low Df can be obtained. β can be increased by reducing the amount of catalyst, lowering the reaction temperature, using a low-polarity solvent, and other conditions when synthesizing the resin represented by formula (T1-1).

[0115] When synthesizing the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)), the parameters α and β of the resin represented by formula (T1-1) (preferably the resin represented by formula (T1-1-2)) can be adjusted by the method of increasing the parameters α and β described above. Of course, the parameters α and β can also be adjusted by methods other than the above.

[0116] Parameter α is preferably 0.57 or more, more preferably 0.59 or more, more preferably 0.60 or more, more preferably 0.62 or more, and may be 0.65 or more, 0.70 or more, 0.75 or more, or 0.80 or more. By setting it to above the aforementioned lower limit, there is a tendency that the heat resistance of the obtained cured product is further improved. For parameter α, the larger the parameter α, the better, from the perspective of having a substantially low dielectric property (Dk and / or Df) and excellent heat resistance, but it may also be 0.95 or less, 0.90 or less, 0.85 or less, 0.82 or less, 0.80 or less, 0.77 or less, 0.75 or less, or 0.74 or less.

[0117] The parameter β is preferably 0.25 or more, more preferably 0.30 or more, further preferably 0.35 or more, further preferably 0.40 or more, further preferably 0.43 or more, further preferably 0.50 or more, and may be 0.60 or more, 0.65 or more, 0.70 or more, 0.77 or more, 0.80 or more, 0.90 or more, and 0.95 or more. By setting it to the above lower limit value or more, there is a tendency that the heat resistance of the obtained cured product is improved and Df is reduced. The parameter β is preferably 2.50 or less, more preferably 2.00 or less, further preferably 1.50 or less, further preferably 1.30 or less, further preferably 1.20 or less, further preferably 1.10 or less, and further may be 1.00 or less, 0.95 or less, 0.90 or less, 0.85 or less, 0.83 or less, and 0.80 or less. By making the parameter β be below the above upper limit value, there is a tendency that the heat resistance of the obtained cured product is improved and Df is reduced.

[0118] The number average molecular weight (Mn) of the resin (A) based on polystyrene conversion by GPC (gel permeation chromatography) method (details are according to the method described in the embodiment described later) is preferably 400 or more, more preferably 500 or more, more preferably 550 or more, more preferably 600 or more, and more preferably 650 or more. By setting the number average molecular weight to above the aforementioned lower limit, the heat resistance of the obtained cured product is improved, and the Df tends to be reduced. In addition, the upper limit of the number average molecular weight (Mn) of the resin (A) based on polystyrene conversion by GPC (gel permeation chromatography) method is preferably 3000 or less, more preferably 2500 or less, more preferably 2000 or less, more preferably 1500 or less, and more preferably 1250 or less, and can also be 1000 or less, 800 or less, depending on the purpose, etc. By setting the number average molecular weight to below the aforementioned upper limit, the heat resistance of the cured product obtained is improved, and the relative dielectric constant (Dk) and the dielectric loss tangent (Df) tend to be reduced.

[0119] In addition, the weight average molecular weight (Mw) of the resin (A) based on polystyrene conversion by GPC (details are according to the method described in the embodiments described later) is preferably 500 or more, more preferably 800 or more, further preferably 900 or more, and further preferably 1000 or more. By setting the weight average molecular weight to above the aforementioned lower limit, the heat resistance of the obtained cured product is improved, and the Df tends to be reduced. The upper limit of the weight average molecular weight (Mw) of the resin (A) based on polystyrene conversion by GPC (details are according to the method described in the embodiments described later) is preferably 6000 or less, more preferably 5000 or less, further preferably 4000 or less, further preferably 3000 or less, and further preferably 2800 or less, and can also be 2500 or less, 2000 or less, or 1500 or less, depending on the purpose, etc. By setting the weight average molecular weight to below the aforementioned upper limit, the heat resistance of the cured product is improved, and the relative dielectric constant (Dk) and the dielectric loss tangent (Df) tend to be reduced.

[0120] The resin (A) preferably has a ratio of weight average molecular weight to number average molecular weight, i.e., Mw / Mn, of 1.1 to 3.0. The Mw / Mn of the resin (A) is more preferably 1.2 or more, further preferably 1.3 or more, further preferably 1.4 or more, further preferably 1.5 or more, further preferably 1.6 or more. In addition, the Mw / Mn of the resin (A) is more preferably 2.5 or less, further preferably 2.4 or less, may be 2.3 or less, may be 2.0 or less, and may be 1.8 or less.

[0121] The weight average molecular weight and the number average molecular weight are measured by the method described in Examples below.

[0122] The content of the resin (A) in the resin composition of the present embodiment is preferably more than 5 mass parts relative to 100 mass parts of the resin solids in the resin composition, more preferably more than 8 mass parts, or more than 10 mass parts, or more than 15 mass parts, more than 20 mass parts, or more than 25 mass parts according to the purpose, etc. By setting the content of the resin (A) to more than the aforementioned lower limit, there is a tendency to reduce the Df of the cured product obtained. In addition, relative to 100 mass parts of the resin solids in the resin composition, the upper limit of the content of the resin (A) is preferably less than 70 mass parts, more preferably less than 55 mass parts, more preferably less than 50 mass parts, more preferably less than 45 mass parts, more preferably less than 40 mass parts, and more preferably less than 35 mass parts. By setting the content of the resin (A) to less than the aforementioned upper limit, there is a tendency that the formability of the resin composition and the heat resistance of the cured product obtained are improved.

[0123] The resin composition of the present embodiment may contain only one type of resin (A) or two or more types thereof. When containing two or more types thereof, the total amount is preferably within the above range.

[0124] The manufacture method of the resin (A) in the present embodiment is not particularly limited, and the resin obtained by known manufacture method can be used. In addition, raw material, reaction temperature, catalyst type, catalyst amount, reaction solvent, raw material concentration etc. during synthetic resin (A) are not particularly limited, and can be appropriately selected or controlled according to the physical property of above-mentioned expectation.

[0125] In the present embodiment, as examples of raw materials for synthesizing the resin (A), m-bis(α-hydroxyisopropyl)benzene, p-bis(α-hydroxyisopropyl)benzene, 1,3-diisopropenylbenzene, 1,4-diisopropenylbenzene, and the like can be used.

[0126] The reaction temperature during the synthesis of the resin (A) in the present embodiment is preferably 40°C or more, more preferably 50°C or more, further preferably 60°C or more, and may be 70°C or more, 80°C or more, 90°C or more, 100°C or more, 110°C or more, or 120°C or more. By setting it to above the aforementioned lower limit, there is a tendency to increase the reaction rate and the ratio of the indane skeleton (structural unit (a) in formula (Tx)), which is preferred. In addition, the reaction temperature is preferably 180°C or less, more preferably 150°C or less, and further preferably 140°C or less. By setting it to below the aforementioned upper limit, there is a tendency to effectively suppress the generation of by-products.

[0127] In addition, the reaction temperature does not need to be the same from the start to the end of the reaction, and the temperature may be changed. In this case, it is preferred that the average temperature of the reaction temperature of the entire process is within the above range.

[0128] The catalyst used when synthesizing the resin (A) in the present embodiment is not particularly limited, and an acid catalyst can be exemplified. As the acid catalyst, inorganic acids such as hydrochloric acid, sulfuric acid, phosphoric acid, organic acids such as oxalic acid, benzenesulfonic acid, toluenesulfonic acid, methanesulfonic acid, fluoromethanesulfonic acid, BF3 ether complex, BF3 phenol complex, Lewis acids such as aluminum chloride, zinc chloride, indium chloride, activated clay, acid clay, silica alumina, zeolite, heteropoly hydrochloric acid, strongly acidic ion exchange resins, etc. can be used.

[0129] When a catalyst is used, the amount thereof may be 0.01 to 20.0 parts by mass based on 100 parts by mass of the above raw materials of the resin (A).

[0130] The catalyst is usually used alone, or two or more catalysts may be used in combination. When used in combination, the total amount is preferably within the above range.

[0131] In the present embodiment, the reaction solvent for synthesizing resin (A) is not particularly specified, and can be used in combination with aromatic hydrocarbon solvents such as toluene, benzene, chlorobenzene, xylene, halogenated hydrocarbon solvents such as methylene chloride, chloroform, aliphatic hydrocarbon solvents such as hexane, heptane, ester solvents such as ethyl acetate, propyl acetate, amide solvents such as dimethylformamide, dimethylacetamide, alcohol solvents or ketone solvents, and water can also be added. As alcohol solvents, methanol, ethanol, butanol, propanol, methyl propylene glycol, diethylene glycol ethyl ether, butyl propylene glycol, propyl propylene glycol, etc. can be listed, as ketone solvents, acetone, methyl ethyl ketone, diethyl ketone, methyl butyl ketone, methyl isobutyl ketone, etc. can be listed, and tetrahydrofuran, dioxane, etc. can be listed, but are not limited to these.

[0132] An example of the reaction solvent in the present embodiment includes an aromatic hydrocarbon solvent.

[0133] The concentration of the above-mentioned raw material during the synthetic resin (A) in the present embodiment is preferably 5% or more, more preferably 8% or more, preferably 10% or more, and may also be 12% or more, 15% or more, 17% or more, 20% or more, 22% or more, or 25% or more. By setting it to above the aforementioned lower limit, there is a tendency that the reaction rate is increased and the ratio of the indane skeleton (structural unit (a) in formula (Tx)) is increased, which is preferred. In addition, the concentration of the above-mentioned raw material is preferably 49% or less, more preferably 40% or less. By setting it to below the aforementioned upper limit, there is a tendency that the generation of by-products can be effectively suppressed.

[0134] Furthermore, the concentration does not need to be the same from the start to the end of the reaction, and the concentration may be changed.

[0135] <<Polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal>>

[0136] The resin composition of the present embodiment contains a polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal. In the present embodiment, the polyphenylene ether compound (B) preferably contains a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds.

[0137] The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal is preferably a polyphenylene ether compound having a group selected from the group consisting of a vinyl benzyl group represented by the formula (Rx-1), a (meth) acrylic group represented by the formula (Rx-2), and a maleimide group at a terminal, more preferably a polyphenylene ether compound having a group represented by the vinyl benzyl group formula (Rx-1) and / or a group represented by the (meth) acrylic group formula (Rx-2) at a terminal, and further preferably a polyphenylene ether compound having two or more vinyl benzyl groups represented by the formula (Rx-1) and / or groups represented by the (meth) acrylic group formula (Rx-2) at a terminal.

[0138]

[0139] (In formula (Rx-1) and formula (Rx-2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group. * represents a bonding site with an oxygen atom. Mc each independently represents a hydrocarbon group having 1 to 12 carbon atoms. z represents an integer of 0 to 4. r represents an integer of 1 to 6.

[0140] By using these polyphenylene ether compounds, there is a tendency to more effectively improve the low dielectric properties (Dk and / or Df) and low water absorption of printed circuit boards, etc. In the present embodiment, polyphenylene ether compounds having a vinyl benzyl group at the end are particularly preferred. By having a vinyl benzyl group, there is a tendency to significantly improve the compatibility with resin (A).

[0141] The following describes these details.

[0142] Examples of the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond (preferably a polyphenylene ether compound (B2) having two or more carbon-carbon unsaturated double bonds) include compounds having a phenylene ether skeleton represented by the following formula (X1).

[0143]

[0144] (In formula (X1), R 24 , R 25 , R 26 and R 27 may be the same or different and represent an alkyl group, an aryl group, a halogen atom or a hydrogen atom having 6 or less carbon atoms.

[0145] The polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond (preferably a polyphenylene ether compound (B2) having two or more carbon-carbon unsaturated double bonds) may further contain a repeating unit represented by formula (X2) and / or a repeating unit represented by formula (X3).

[0146]

[0147] (In formula (X2), R 28 , R 29 , R 30 , R 34 and R 35 R may be the same or different and represent an alkyl group having 6 or less carbon atoms or a phenyl group. 31 , R 32 and R 33 They may be the same or different and are a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group.)

[0148]

[0149] (In formula (X3), R 36 , R 37 , R 38 , R 39 , R 40 , R 41 , R 42 and R 43 They may be the same or different and are a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group. -A- is a linear, branched, or cyclic divalent hydrocarbon group having 20 or less carbon atoms).

[0150] The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end (preferably a polyphenylene ether compound (B2) containing more than two carbon-carbon unsaturated double bonds) is preferably a modified polyphenylene ether compound (hereinafter sometimes referred to as "modified polyphenylene ether compound (g)") in which a part or all of the end is functionalized with an ethylenically unsaturated group, and more preferably a modified polyphenylene ether compound having two or more groups selected from the group consisting of a vinyl benzyl group formula (Rx-1), a (meth) acrylic group formula (Rx-2), and a maleimide group, and more preferably a vinyl benzyl group formula (Rx-1) and / or a (meth) acrylic group formula (Rx-2). By adopting such a modified polyphenylene ether compound (g), the low dielectric properties (Dk and / or Df) of the cured product of the resin composition can be made smaller, and low water absorption and metal foil peeling strength can be improved. These can be used in one or in combination of two or more.

[0151] Examples of the modified polyphenylene ether compound (g) include polyphenylene ether compounds represented by formula (OP).

[0152]

[0153] (In formula (OP), X represents an aromatic group, -(YO) n1 - represents a polyphenylene ether structure, n1 represents an integer of 1 to 100, and n2 represents an integer of 1 to 4. Rx is a group represented by formula (Rx-1) or formula (Rx-2).

[0154]

[0155] (In formula (Rx-1) and formula (Rx-2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group. * represents a bonding site with an oxygen atom. Mc each independently represents a hydrocarbon group having 1 to 12 carbon atoms. z represents an integer of 0 to 4. r represents an integer of 1 to 6.

[0156] When n1 and / or n2 are integers greater than 2, n1 structural units (YO) and / or n2 structural units may be the same or different. n2 is preferably 2 or greater, more preferably 2.

[0157] In formula (Rx-1) and formula (Rx-2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group.

[0158] R 1 It is preferably a hydrogen atom or an alkyl group, more preferably a hydrogen atom or a methyl group, and still more preferably a hydrogen atom.

[0159] R 2 and R 3 Each independently is preferably a hydrogen atom or an alkyl group, more preferably a hydrogen atom or a methyl group, and further preferably a hydrogen atom.

[0160] As R 1 , R 2 and R 3 The carbon number of the alkyl group, alkenyl group or alkynyl group is preferably 5 or less, more preferably 3 or less.

[0161] r in the formula (Rx-1) represents an integer of 1 to 6, preferably an integer of 1 to 5, more preferably an integer of 1 to 4, further preferably an integer of 1 to 3, further preferably 1 or 2, further preferably 1.

[0162] Mc in formula (Rx-1) each independently represents a hydrocarbon group having 1 to 12 carbon atoms, preferably a hydrocarbon group having 1 to 10 carbon atoms, more preferably a straight-chain or branched alkyl group having 1 to 10 carbon atoms, further preferably a methyl group, ethyl group, isopropyl group, isobutyl group, tert-butyl group, pentyl group, octyl group or nonyl group, and further preferably a methyl group, ethyl group, isopropyl group, isobutyl group or tert-butyl group.

[0163] In the formula (Rx-1), z represents an integer of 0 to 4, preferably an integer of 0 to 3, more preferably an integer of 0 to 2, further preferably 0 or 1, and further preferably 0.

[0164] A specific example of the group represented by the formula (Rx-1) is a vinylbenzyl group, and a specific example of the group represented by the formula (Rx-2) is a (meth)acryloyl group.

[0165] Rx is preferably a group represented by formula (Rx-1).

[0166] Examples of the modified polyphenylene ether compound (g) include a polyphenylene ether compound represented by the formula (OP-1).

[0167]

[0168] (In formula (OP-1), X represents an aromatic group, -(YO)n2- represents a polyphenylene ether structure, and R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group, n1 represents an integer of 1 to 6, n2 represents an integer of 1 to 100, and n3 represents an integer of 1 to 4.)

[0169] When n2 and / or n3 are integers greater than 2, n2 structural units (YO) and / or n3 structural units may be the same or different. n3 is preferably 2 or greater, more preferably 2.

[0170] The modified polyphenylene ether compound (g) in the present embodiment is preferably a compound represented by the formula (OP-2), and more preferably a compound represented by the formula (OP-2-2).

[0171]

[0172] Here, -(OXO)- is preferably represented by Formula (OP-3) and / or Formula (OP-4).

[0173]

[0174] (In formula (OP-3), R 4 , R 5 , R 6 , R 10 and R11 R may be the same or different and is an alkyl group having 6 or less carbon atoms or a phenyl group. 7 , R 8 and R 9 They may be the same or different and are a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group.)

[0175]

[0176] (In formula (OP-4), R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , R 18 and R 19 They may be the same or different and are a hydrogen atom, an alkyl group having 6 or less carbon atoms, or a phenyl group. -A- is a linear, branched, or cyclic divalent hydrocarbon group having 20 or less carbon atoms).

[0177] In addition, -(YO)- is preferably represented by formula (OP-5).

[0178]

[0179] (In formula (OP-5), R 20 , R 21 R may be the same or different and is an alkyl group having 6 or less carbon atoms or a phenyl group. 22 , R 23 may be the same or different and are a hydrogen atom, an alkyl group with a carbon number of 6 or less, or a phenyl group). In particular, by making R 20 and R 21 Each independently being a group having one or more methyl and / or cyclohexyl groups, the rigidity of the obtained resin molecule becomes higher. Molecules with high rigidity have lower mobility than molecules with low rigidity, so the relaxation time during dielectric relaxation becomes longer, and the low dielectric properties (Dk and / or Df) are improved, which is preferred.

[0180] An example of the formula (OP-5) is the following structure.

[0181]

[0182] Regarding the polyphenylene compound having the above structure, reference can be made to the description of Japanese Patent Application Laid-Open No. 2019-194312, the contents of which are incorporated into this specification.

[0183] In formula (OP-2), a and b each independently represent an integer from 0 to 100, and at least one of a and b is an integer from 1 to 100. a and b are each independently preferably an integer from 0 to 50, more preferably an integer from 1 to 30, and preferably an integer from 1 to 10. When a and / or b is an integer of 2 or more, two or more -(Y-O)-s can be arranged independently in one structure, or can be arranged in a block or random manner of two or more structures.

[0184] In addition, when a plurality of compounds represented by formula (OP-2) are included, the average value of a is preferably 1 < a < 10, and the average value of b is preferably 1 < b < 10.

[0185] Examples of -A- in formula (OP-4) include divalent organic groups such as methylene, ethylidene, 1-methylethylidene, 1,1-propylidene, 1,4-phenylene bis(1-methylethylidene), 1,3-phenylene bis(1-methylethylidene), cyclohexylidene, phenylmethylene, naphthylmethylene, 1-phenylethylidene, etc., but are not limited to these.

[0186] Rx has the same meaning as Rx in formula (OP), and the preferred range is also the same.

[0187] Among the compounds represented by the above formula (OP-2), preferably R 4 , R 5 , R 6 , R 10 , R 11 , R 20 and R 21 are alkyl groups having 3 or fewer carbon atoms and R 7 , R 8 , R 9 , R 12 , R 13 , R 14 , R 15 , R 16 , R 17 , R 18 , R 19 , R 22 and R 23 are a polyphenylene ether compound of a hydrogen atom or an alkyl group having 3 or fewer carbon atoms. Particularly preferably, -(O-X-O)- represented by formula (OP-3) or formula (OP-4) is formula (OP-9), formula (OP-10) and / or formula (OP-11), and -(Y-O)- represented by formula (OP-5) is formula (OP-12) or formula (OP-13). When a and / or b is an integer of 2 or more, two or more -(Y-O)-s can be a structure formed by arranging two or more of formula (OP-12) and / or formula (OP-13), or a structure formed by arranging formula (OP-12) and formula (OP-13) in a block or random manner.

[0188]

[0189] (In formula (OP-10), R 44 , R 45 , R 46 and R 47 They may be the same or different and are hydrogen atoms or methyl groups. -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.

[0190] As specific examples of -B-, the same ones as the specific examples of -A- in formula (OP-4) can be given.

[0191]

[0192] (In formula (OP-11), -B- is a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms.)

[0193] As specific examples of -B-, the same ones as the specific examples of -A- in formula (OP-4) can be given.

[0194]

[0195] The modified polyphenylene ether compound (g) used in the present embodiment is more preferably a compound represented by formula (OP-14) and / or a compound represented by formula (OP-15).

[0196]

[0197] (In formula (OP-14), a and b each independently represent an integer of 0 to 100, and at least one of a and b is an integer of 1 to 100.)

[0198] a and b in formula (OP-14) have the same meanings as a and b in formula (OP-2) independently, and the preferred ranges are also the same.

[0199]

[0200] (In formula (OP-15), a and b each independently represent an integer of 0 to 100, and at least one of a and b is an integer of 1 to 100.)

[0201] a and b in formula (OP-15) have the same meanings as a and b in formula (OP-2) independently, and the preferred ranges are also the same.

[0202] The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds, more preferably a modified polyphenylene ether compound (g)) has a polystyrene-converted number average molecular weight (Mn) based on the GPC (gel permeation chromatography) method (details are in accordance with the method described in the embodiments described later) of, for example, 500 or more, more preferably 800 or more, and preferably 3000 or less. By making the number average molecular weight 500 or more, there is a tendency to further suppress stickiness when the resin composition of the present embodiment is made into a coating film. By making the number average molecular weight 3000 or less, there is a tendency to further improve the solubility in a solvent.

[0203] In addition, the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the end (preferably a polyphenylene ether compound (B2) containing two or more carbon-carbon unsaturated double bonds, more preferably a modified polyphenylene ether compound (g)) has a polystyrene-converted weight average molecular weight (Mw) based on GPC (details are according to the method described in the embodiments described later) of preferably 800 or more and 6000 or less, more preferably 800 or more and 5000 or less. By setting it to above the lower limit, there is a tendency that the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the cured product of the resin composition become lower, and by setting it to below the upper limit, there is a tendency that the solubility, low viscosity and formability of the resin composition in the solvent when making the varnish described later, etc., are further improved.

[0204] Furthermore, the carbon-carbon unsaturated double bond equivalent of the terminal when being a modified polyphenylene ether compound (g) is preferably 400 to 5000 g per 1 carbon-carbon unsaturated double bond, more preferably 400 to 2500 g. By being set to above the aforementioned lower limit, the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the cured product of the resin composition tend to become lower. By being set to below the aforementioned upper limit, the solubility, low viscosity and formability of the resin composition in a solvent tend to be further improved.

[0205] The lower limit of the content of the polyphenylene ether compound (B) (preferably a polyphenylene ether compound (B2) comprising more than 2 carbon-carbon unsaturated double bonds) having a carbon-carbon unsaturated double bond at the end of the resin composition of the present embodiment is 10 mass parts or more, preferably 50 mass parts or more, more preferably 100 mass parts or more, more preferably 150 mass parts or more, and more preferably 180 mass parts or more relative to 100 mass parts of resin (A). By being set to more than the aforementioned lower limit, there is a tendency that the moldability of the resin composition, the low water absorption of the obtained cured product, and the low dielectric properties (Dk and / or Df) are further improved. In addition, the upper limit of the content of the polyphenylene ether compound (B) (preferably a polyphenylene ether compound (B2) comprising more than 2 carbon-carbon unsaturated double bonds) having a carbon-carbon unsaturated double bond at the end is 300 mass parts or less, preferably 280 mass parts or less, more preferably less than mass parts, and can also be less than 250 mass parts, and further can also be less than 220 mass parts. By setting the content to be equal to or greater than the above lower limit, the low dielectric properties (Dk and / or Df), heat resistance, and chemical resistance of the obtained cured product tend to be further improved.

[0206] Relative to 100 parts by mass of the resin solids in the resin composition of the present embodiment, the total content of resin (A) and polyphenylene ether compound (B) is preferably more than 40 parts by mass, more preferably more than 45 parts by mass, more preferably more than 50 parts by mass, or more than 55 parts by mass. By setting the total content of resin (A) and polyphenylene ether compound (B) to more than the aforementioned lower limit, there is a tendency that the low water absorption and low dielectric properties (Dk and / or Df) of the obtained solidified material are further improved. In addition, relative to 100 parts by mass of the resin solids in the resin composition, the total content of resin (A) and polyphenylene ether compound (B) is preferably less than 80 parts by mass. By setting the total content of resin (A) and polyphenylene ether compound (B) to less than the aforementioned upper limit, there is a tendency that the balance of the moldability of the resin composition, the low dielectric properties (Dk and / or Df) of the obtained solidified material, heat resistance, chemical resistance, etc. is excellent.

[0207] In the present embodiment, relative to a total of 100 parts by mass of resin (A) and polyphenylene ether compound (B), the mass ratio of resin (A) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, more preferably 20 parts by mass or more, more preferably 25 parts by mass or more, and more preferably 30 parts by mass or more. By setting the aforementioned mass ratio to above the above lower limit, there is a tendency that the low dielectric properties (Dk and / or Df) of the obtained solidified material are further improved. In addition, relative to a total of 100 parts by mass of resin (A) and polyphenylene ether compound (B), the mass ratio of resin (A) is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, more preferably 40 parts by mass or less, and more preferably 38 parts by mass or less. By setting the aforementioned mass ratio to below the above upper limit, there is a tendency that the moldability of the resin composition and the low dielectric properties (Dk and / or Df) of the obtained solidified material are further improved.

[0208] The lower limit of the content of the polyphenylene ether compound (B) (preferably a polyphenylene ether compound (B2) comprising more than 2 carbon-carbon unsaturated double bonds) having a carbon-carbon unsaturated double bond at the end of the resin composition of the present embodiment is preferably 30 mass parts or more, more preferably 35 mass parts or more relative to 100 mass parts of the resin solids in the resin composition. By being set to more than the aforementioned lower limit, there is a tendency that the low water absorption and low dielectric properties (Dk and / or Df) of the obtained cured product are further improved. In addition, the upper limit of the content of the polyphenylene ether compound (B) (preferably a polyphenylene ether compound (B2) comprising more than 2 carbon-carbon unsaturated double bonds) having a carbon-carbon unsaturated double bond at the end is preferably less than 75 mass parts relative to 100 mass parts of the resin solids in the resin composition, more preferably less than 70 mass parts, can be less than 65 mass parts, and then can also be less than 60 mass parts. By being set to less than the aforementioned upper limit, there is a tendency that the heat resistance and chemical resistance of the cured product obtained are further improved.

[0209] The resin composition in the present embodiment may contain only one polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal, or may contain two or more. When containing two or more, the total amount is preferably within the above range.

[0210] <Polymer having a structural unit represented by formula (V)>

[0211] The resin composition of this embodiment includes a polymer having a structural unit represented by formula (V). By including a polymer having a structural unit represented by formula (V), a resin composition capable of providing a cured product having excellent low dielectric properties (Dk and / or Df) can be obtained.

[0212]

[0213] (In formula (V), Ar represents an aromatic hydrocarbon linking group. * represents a bonding position.)

[0214] The aromatic hydrocarbon linking group may be a group formed only by an aromatic hydrocarbon optionally having a substituent, or may be a group formed by a combination of an aromatic hydrocarbon optionally having a substituent and other linking groups, preferably a group formed only by an aromatic hydrocarbon optionally having a substituent. It should be noted that the substituent optionally possessed by the aromatic hydrocarbon may include a substituent Z (e.g., an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 2 to 6 carbon atoms, an alkynyl group having 2 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a hydroxyl group, an amino group, a carboxyl group, a halogen atom, etc.). In addition, the above aromatic hydrocarbon preferably has no substituent.

[0215] The aromatic hydrocarbon linking group is usually a divalent linking group.

[0216] Specifically, the aromatic hydrocarbon linking group includes phenylene, naphthalene diyl, anthracene diyl, phenanthrene diyl, biphenyl diyl, and fluorene diyl, which may have a substituent, and preferably phenylene which may have a substituent. The substituent may be exemplified by the substituent Z mentioned above, but the phenylene group preferably has no substituent.

[0217] The structural unit represented by formula (V) more preferably includes at least one of the structural unit represented by the following formula (V1), the structural unit represented by the following formula (V2), and the structural unit represented by the following formula (V3). It should be noted that the * in the following formula represents a bonding position. In addition, the structural units represented by formulas (V1) to (V3) are sometimes collectively referred to as "structural units (a)".

[0218]

[0219] In formulas (V1) to (V3), L 1 It is an aromatic hydrocarbon linking group (the carbon number is preferably 6 to 22, more preferably 6 to 18, and further preferably 6 to 10). Specifically, it includes phenylene, naphthalene diyl, anthracene diyl, phenanthrene diyl, biphenyl diyl, and fluorene diyl, which may have a substituent, and among them, phenylene which may have a substituent is preferred. The substituent may be exemplified by the substituent Z mentioned above, but the above-mentioned phenylene group and the like preferably have no substituent.

[0220] As the compound forming the structural unit (a), preferably a divinyl aromatic compound, for example, divinylbenzene, bis(1-methylvinyl)benzene, divinylnaphthalene, divinylanthracene, divinylbiphenyl, divinylphenanthrene etc. can be listed. Among them, divinylbenzene is particularly preferred. These divinyl aromatic compounds can be used in one kind, or in two or more kinds as required.

[0221] As described above, the polymer having the structural unit represented by formula (V) may be a homopolymer of the structural unit (a) or a copolymer with a structural unit derived from another monomer.

[0222] When the polymer having the structural unit shown in formula (V) is a copolymer, the copolymerization ratio of the structural unit (a) is preferably 3 mol% or more, more preferably 5 mol% or more, further preferably 10 mol% or more, and may be 15 mol% or more. As the upper limit, it is preferably 90 mol% or less, more preferably 85 mol% or less, further preferably 80 mol% or less, further preferably 70 mol% or less, further preferably 60 mol% or less, further preferably 50 mol% or less, further preferably 40 mol% or less, particularly preferably 30 mol% or less, and further may be 25 mol% or less, 20 mol% or less.

[0223] As the structural unit derived from other monomers, there can be exemplified a structural unit (b) derived from an aromatic compound having one vinyl group (monovinyl aromatic compound).

[0224] The structural unit (b) derived from a monovinyl aromatic compound is preferably a structural unit represented by the following formula (V4).

[0225]

[0226] In formula (V4), L 2 is an aromatic hydrocarbon linking group, and specific examples of preferred groups include the above-mentioned L 1 Example.

[0227] R V1 R is a hydrogen atom or a hydrocarbon group having 1 to 12 carbon atoms (preferably an alkyl group). V1 When it is a hydrocarbon group, the carbon number is preferably 1 to 6, more preferably 1 to 3. V1 and L 2 The above-mentioned substituent Z may be present.

[0228] When the polymer having the structural unit shown in formula (V) is a copolymer containing the structural unit (b) derived from a monovinyl aromatic compound, examples of monovinyl aromatic compounds include vinyl aromatic compounds such as styrene, vinyl naphthalene, and vinyl biphenyl; vinyl aromatic compounds substituted with nucleus alkyl groups such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o-dimethylstyrene, p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, p-ethylvinylbenzene, methylvinylbiphenyl, and ethylvinylbiphenyl, etc. The monovinyl aromatic compounds exemplified herein may appropriately have the substituent Z described above. In addition, these monovinyl aromatic compounds may be used alone or in combination of two or more.

[0229] When the polymer having the structural unit shown in formula (V) is a copolymer comprising structural unit (b), the copolymerization ratio of structural unit (b) is preferably 10 mol% or more, more preferably 15 mol% or more, and furthermore, 20 mol% or more, 30 mol% or more, 40 mol% or more, 50 mol% or more, 60 mol% or more, 70 mol% or more, 75 mol% or more. As the upper limit, it is preferably 98 mol% or less, more preferably 90 mol% or less, and more preferably 85 mol% or less.

[0230] The polymer having the structural unit shown in formula (V) may also have other structural units other than structural unit (a) and structural unit (b). As other structural units, for example, structural unit (c) derived from cycloolefin compounds can be listed. As cycloolefin compounds, hydrocarbons having double bonds in the ring structure can be listed. Specifically, monocyclic cyclic olefins such as cyclobutene, cyclopentene, cyclohexene, and cyclooctene, and compounds having norbornene ring structures such as norbornene, dicyclopentadiene, and cycloolefin compounds formed by aromatic ring condensation such as indene and acenaphthylene can be listed. As examples of norbornene compounds, compounds described in paragraphs 0037 to 0043 of Japanese Patent Publication No. 2018-39995 can be listed, and the contents are incorporated into this specification. It should be noted that the cycloolefin compounds exemplified here may further have the above-mentioned substituent Z.

[0231] When the polymer having the structural unit shown in formula (V) is a copolymer comprising structural unit (c), the copolymerization ratio of structural unit (c) is preferably 10 mol% or more, more preferably 20 mol% or more, and further preferably 30 mol% or more. As the upper limit, it is preferably 90 mol% or less, more preferably 80 mol% or less, further preferably 70 mol% or less, and can be 50 mol% or less, or 30 mol% or less.

[0232] In the polymer having the structural unit shown in formula (V), a structural unit (d) derived from a different polymerizable compound (hereinafter, also referred to as other polymerizable compounds) may also be further incorporated. As other polymerizable compounds (monomers), for example, compounds containing three vinyl groups can be listed. Specifically, 1,3,5-trivinylbenzene, 1,3,5-trivinylnaphthalene, 1,2,4-trivinylcyclohexane can be listed. Alternatively, ethylene glycol diacrylate, butadiene, etc. can be listed. The copolymerization ratio of the structural unit (d) derived from other polymerizable compounds is preferably 30 mol% or less, more preferably 20 mol% or less, and further preferably 10 mol% or less.

[0233] As an embodiment of the polymer having the structural unit represented by formula (V), there can be exemplified a polymer having structural unit (a) as an essential structural unit and containing at least one of structural units (b) to (d). Further, there can be exemplified an embodiment in which the total of structural units (a) to (d) accounts for 95 mol% or more of all structural units, and further 98 mol% or more.

[0234] As another embodiment of the polymer having the structural unit represented by formula (V), it is preferably a polymer having the structural unit (a) as an essential structural unit and wherein the structural units containing aromatic rings account for 90 mol % or more of all the structural units except the terminal, more preferably the structural units containing aromatic rings account for 95 mol % or more, and the structural units containing aromatic rings may also account for 100 mol %.

[0235] When calculating the mol % relative to all structural units, one structural unit refers to a structural unit derived from one molecule of a monomer (e.g., a divinyl aromatic compound, a monovinyl aromatic compound, etc.) used in the production of a polymer having a structural unit represented by formula (V).

[0236] The method for producing the polymer having the structural unit shown in formula (V) is not particularly limited, and conventional methods may be used, for example, by polymerizing a raw material comprising a divinyl aromatic compound (coexisting with a monovinyl aromatic compound, a cycloolefin compound, etc. as required) in the presence of a Lewis acid catalyst. As the Lewis acid catalyst, a metal fluoride such as boron trifluoride or a complex thereof may be used.

[0237] The structure of the chain end of the polymer having the structural unit represented by formula (V) is not particularly limited, and the group derived from the divinyl aromatic compound may be a structure of the following formula (E1). 1 The same as defined in the above formula (V1). * indicates a bonding position.

[0238] *-CH=CH-L 1 -CH=CH2(E1)

[0239] When the group derived from a monovinyl aromatic compound is a chain terminal, a structure of the following formula (E2) can be used. 2 and R V1 They have the same meanings as defined in the above formula (V4). * represents a bonding position.

[0240] *-CH=CH-L 2 -R V1 (E2)

[0241] The molecular weight of the polymer having the structural unit represented by formula (V) is preferably 300 or more, more preferably 500 or more, further preferably 1000 or more, and further preferably 1500 or more in terms of number average molecular weight Mn. The upper limit is preferably 130,000 or less, more preferably 120,000 or less, further preferably 110,000 or less, and further preferably 100,000 or less.

[0242] The molecular weight of the polymer with the structural unit shown in formula (V) is in terms of weight-average molecular weight Mw, preferably more than 3000, more preferably more than 5000, more preferably more than 10000.By being set to more than the aforementioned lower limit, thus the cured product of resin combination can be effectively brought into play the excellent low dielectric properties possessed by the polymer with the structural unit shown in formula (V), particularly the dielectric properties after Df, moisture absorption.As the upper limit, preferably less than 130000, more preferably less than 100000, more preferably less than 80000, more preferably less than 50000.By being set to less than the aforementioned upper limit, thus having prepreg or resin sheet laminated on circuit forming substrate when being difficult for poor embedding tendency.

[0243] The monodispersity (Mw / Mn) represented by the ratio of the weight average molecular weight Mw to the number average molecular weight Mn is preferably 100 or less, more preferably 50 or less, and even more preferably 20 or less. The lower limit is practically 1.1 or more, preferably 5 or more, more preferably 7 or more, and even more preferably 10 or more.

[0244] The above-mentioned Mw and Mn are measured according to the description in the Examples described later.

[0245] When the resin composition of the present embodiment contains two or more polymers having a structural unit represented by formula (V), it is preferred that Mw, Mn, and Mw / Mn of the mixture satisfy the above ranges.

[0246] The equivalent of the vinyl group of the polymer having the structural unit shown in formula (V) is preferably 200 g / eq. or more, more preferably 230 g / eq. or more, and further preferably 250 g / eq. or more. In addition, the equivalent of the vinyl group is preferably 1200 g / eq. or less, more preferably 1000 g / eq. or less, and furthermore may be 800 g / eq. or less, 600 g / eq. or less, 400 g / eq. or less, or 300 g / eq. or less. By setting it to above the above lower limit, there is a tendency that the storage stability of the resin composition is improved and the fluidity of the resin composition is improved. Therefore, there is a tendency that the formability is improved, it is not easy to produce pores when forming a prepreg, and a printed circuit board with higher reliability can be obtained. On the other hand, by setting it to below the above upper limit, there is a tendency that the heat resistance of the obtained cured product is improved.

[0247] In this specification, for the polymer having a structural unit represented by formula (V), reference can be made to the compounds and their synthesis reaction conditions described in paragraphs 0029 to 0058 of International Publication No. 2017 / 115813, the compounds and their synthesis reaction conditions described in paragraphs 0013 to 0058 of Japanese Patent Application Publication No. 2018-039995, and the compounds and their synthesis reaction conditions described in paragraphs 0008 to 0043 of Japanese Patent Application Publication No. 2018-168347. The compounds and their synthesis reaction conditions, etc. described in paragraphs 0014 to 0042 of Japanese Patent Application Laid-Open No. 2006-070136, the compounds and their synthesis reaction conditions, etc. described in paragraphs 0014 to 0061 of Japanese Patent Application Laid-Open No. 2006-089683, and the compounds and their synthesis reaction conditions, etc. described in paragraphs 0008 to 0036 of Japanese Patent Application Laid-Open No. 2008-248001, and their contents are incorporated into this specification.

[0248] The lower limit of the content of the polymer with the structural unit shown in formula (V) is more than 10 mass parts, more preferably more than 20 mass parts, more preferably more than 40 mass parts, more preferably more than 60 mass parts, more preferably more than 80 mass parts relative to resin (A) 100 mass parts. On the other hand, the upper limit of the content of the polymer with the structural unit shown in formula (V) is less than 300 mass parts, preferably less than 280 mass parts, more preferably less than 260 mass parts, more preferably less than 240 mass parts, more preferably less than 220 mass parts relative to resin (A) 100 mass parts. By setting content to above-mentioned scope, there is a tendency of excellent balance of the formability of resin combination, the low dielectric properties (Dk and / or Df) of the cured product obtained, heat resistance, chemical resistance, etc.

[0249] When the resin solid content in the resin composition is set to 100 parts by mass, the lower limit of the content of the polymer having the structural unit shown in formula (V) is more preferably 5 parts by mass or more, further preferably 10 parts by mass or more, further preferably 15 parts by mass or more, and further preferably 20 parts by mass or more. On the other hand, when the resin solid content in the resin composition is set to 100 parts by mass, the upper limit of the content of the polymer having the structural unit shown in formula (V) is preferably 60 parts by mass or less, more preferably 55 parts by mass or less, further preferably 50 parts by mass or less, and further preferably 45 parts by mass or less.

[0250] In the present embodiment, the mass ratio of resin (A) is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, further preferably 20 parts by mass or more, and further preferably 25 parts by mass or more, relative to a total of 100 parts by mass of the polymer having the structural unit represented by formula (V). By setting it to above the aforementioned lower limit, there is a tendency for the low dielectric properties (Dk and / or Df) to be further improved.

[0251] In addition, the mass ratio of resin (A) is preferably 70 parts by mass or less, and may be 65 parts by mass or less, relative to 100 parts by mass of the total of resin (A) and the polymer having the structural unit represented by formula (V). By setting it below the above upper limit, there is a tendency for heat resistance to be further improved.

[0252] The resin composition may contain only one polymer having a structural unit represented by formula (V), or two or more polymers thereof. When the resin composition contains two or more polymers, the total amount thereof is preferably within the above range.

[0253] In the present embodiment, the total amount of the resin (A), the polyphenylene ether compound (B), and the polymer having the structural unit represented by the formula (V) accounts for 90 parts by mass or more of the resin composition in 100 parts by mass of the resin solid content.

[0254] <Other compounds (C)>

[0255] The resin composition of the present embodiment preferably further comprises other compounds (C) (preferably other curable compounds and / or plasticizing compounds, more preferably other thermosetting compounds and / or thermoplastic compounds, and further preferably other thermosetting compounds) other than the resin (A), the polyphenylene ether compound (B) and the polymer having the structural unit represented by the formula (V). The other compound (C) preferably contains one or more selected from the group consisting of maleimide compounds, cyanate compounds, epoxy compounds, phenol compounds, compounds containing a (meth)allyl group (e.g., alkenyl nadic imide compounds), oxetane resins, benzoxazine compounds, arylcyclobutene resins, polyamide resins, polyimide resins, perfluorovinyl ether resins, compounds having a styrene group other than the aforementioned polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal, compounds having an isopropenyl group other than the aforementioned resin (A) having an indane skeleton, polyfunctional (meth)acrylate compounds other than the aforementioned polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal, elastomers, and petroleum resins, and more preferably contains at least one or more selected from the group consisting of maleimide compounds, cyanate compounds, epoxy compounds, phenol compounds, compounds containing a (meth)allyl group (e.g., alkenyl nadic imide compounds), oxetane resins, and benzoxazine compounds. By including such a component, desired performance required for a printed wiring board can be more effectively exhibited.

[0256] When the resin combination of the present embodiment includes other compounds (C), its content (total amount) is preferably more than 1 mass part relative to 100 mass parts of resin solids, more preferably more than 10 mass parts, more preferably more than 15 mass parts, more preferably more than 20 mass parts, more preferably more than 30 mass parts.By being set to more than the aforementioned lower limit, so as to have the tendency of further improving heat resistance, coating adhesion, low thermal expansion etc.In addition, the upper limit of the content of other compounds (C) (preferably other curable compounds and / or plasticizing compounds, more preferably other thermosetting compounds and / or thermoplastic compounds, more preferably other thermosetting compounds) is preferably less than 50 mass parts, more preferably less than 45 mass parts, more preferably less than 40 mass parts relative to 100 mass parts of resin solids.By being set to less than the aforementioned upper limit, so as to have the tendency of further improving low dielectric properties (Dk and / or Df), low water absorption.

[0257] The resin composition of the present embodiment may contain only one other compound (C) or two or more other compounds (C). When containing two or more other compounds (C), the total amount is preferably within the above range.

[0258] <<Maleimide Compounds>>

[0259] The resin composition of the present embodiment may contain a maleimide compound.

[0260] The maleimide compound is not particularly limited as long as it is a compound containing one or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, further preferably 2 or 3, further preferably) maleimide groups in the molecule, and compounds commonly used in the field of printed wiring boards can be widely used.

[0261] In the present embodiment, the maleimide compound preferably includes one or more selected from the group consisting of a compound represented by formula (M0), a compound represented by formula (M1), a compound represented by formula (M2), a compound represented by formula (M3), a compound represented by formula (M4), a compound represented by formula (M5), a maleimide compound (M6) and a maleimide compound (M7), and more preferably includes a compound represented by formula (M0), a compound represented by formula (M1), a compound represented by formula (M3), a compound represented by formula (M4), a compound represented by formula (M5) and a maleimide compound (M6). The present invention is preferably a maleimide compound (M6) of the group consisting of one or more, preferably including a compound selected from the group consisting of a compound represented by formula (M1), a compound represented by formula (M3), a compound represented by formula (M4) and a compound represented by formula (M5), and more preferably including a compound selected from the group consisting of a compound represented by formula (M1), a compound represented by formula (M3) and a compound represented by formula (M5), and more preferably including a compound represented by formula (M1) and / or a compound represented by formula (M3), and more preferably a compound represented by formula (M1). If these maleimide compounds are used for printed circuit board materials (such as metal foil laminates), etc., excellent heat resistance can be imparted.

[0262]

[0263] (In formula (M0), R 51 Each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms or a phenyl group, and R 52 Each independently represents a hydrogen atom or a methyl group, and n1 represents an integer greater than 1.)

[0264] R 51 Each independently is preferably one selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group and a phenyl group, more preferably a hydrogen atom and / or a methyl group, and further preferably a hydrogen atom.

[0265] R 52 Preferred is methyl.

[0266] n1 is preferably an integer of 1 to 10, more preferably an integer of 1 to 5, further preferably an integer of 1 to 3, further preferably 1 or 2, further preferably 1.

[0267] Specifically, the following compounds can be mentioned as preferred examples of formula (M0).

[0268]

[0269] In the above formula, R 8 Each independently represents a hydrogen atom, a methyl group or an ethyl group, and is preferably a methyl group.

[0270] The compound represented by formula (M0) may be a mixture of two or more compounds in addition to being a single compound. Examples of the mixture include a mixture of compounds having different n1, a mixture of compounds having different n1, and a mixture of compounds having different n1. 51 and / or R 52 A mixture of compounds having different types of substituents, a mixture of compounds having different bonding positions (meta, para, or ortho) of the maleimide group and the oxygen atom relative to the benzene ring, and a mixture of compounds combining two or more of the aforementioned different points. The same applies to the compounds represented by formulas (M1) to (M6).

[0271]

[0272] (In formula (M1), R M1 , R M2 , R M3 and R M4 Each independently represents a hydrogen atom or an organic group. M5 and R M6 Each independently represents a hydrogen atom or an alkyl group. M is a divalent aromatic group. A is a 4- to 6-membered alicyclic group. M7 and R M8 Each is independently an alkyl group. mx is 1 or 2, and lx is 0 or 1. M9 and R M10 Each independently represents a hydrogen atom or an alkyl group. M11 , R M12 , R M13 and R M14 Each independently represents a hydrogen atom or an organic group. M15 Each independently represents an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group. px represents an integer of 0 to 3. nx represents an integer of 1 to 20.)

[0273] R in the formulaM1 , R M2 , R M3 and R M4 Each independently represents a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and particularly preferably a methyl group. M1 and R M3 Each is independently preferably an alkyl group, R M2 and R M4 Preferred is a hydrogen atom.

[0274] R M5 and R M6 Each independently represents a hydrogen atom or an alkyl group, and is preferably an alkyl group. The alkyl group herein is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and among these, a methyl group is particularly preferred.

[0275] Ar M Ar represents a divalent aromatic group, preferably phenylene, naphthalene diyl, phenanthrene diyl, anthracene diyl, more preferably phenylene, and still more preferably m-phenylene. M The substituent is preferably an alkyl group, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and particularly preferably a methyl group. M Preferably, there is no substitution.

[0276] A is a 4- to 6-membered alicyclic group, more preferably a 5-membered alicyclic group (preferably a group forming an indane ring together with a benzene ring). M7 and R M8 Each independently represents an alkyl group, preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and particularly preferably a methyl group.

[0277] mx is 1 or 2, preferably 2.

[0278] lx is 0 or 1, preferably 1.

[0279] R M9 and R M10 Each independently represents a hydrogen atom or an alkyl group, and is preferably an alkyl group. The alkyl group herein is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and among these, a methyl group is particularly preferred.

[0280] R M11 , R M12 , R M13 and R M14Each independently represents a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and particularly preferably a methyl group. M12 and R M13 Each is independently preferably an alkyl group, R M11 and R M14 Preferred is a hydrogen atom.

[0281] R M15 Each independently represents an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group, and is preferably an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms.

[0282] px represents an integer of 0 to 3, preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0.

[0283] nx represents an integer of 1 to 20. nx may be an integer of 10 or less.

[0284] It should be noted that the resin composition of the present embodiment may include only one compound represented by the formula (M1) and at least a compound having different values ​​of nx, or may include more than two kinds. When including more than two kinds, in order to achieve a low melting point (low softening point), and low melt viscosity, excellent operability, the average value (average number of repeating units) n of nx in the compound represented by the formula (M1) in the resin composition is preferably more than 0.92, more preferably more than 0.95, further preferably more than 1.0, and further preferably more than 1.1. In addition, n is preferably less than 10.0, more preferably less than 8.0, further preferably less than 7.0, further preferably less than 6.0, and may also be less than 5.0. The same is true for the compounds represented by the formula (M1-2) and formula (M1-3) described later.

[0285] The compound represented by the formula (M1) is preferably a compound represented by the following formula (M1-1).

[0286]

[0287] (In formula (M1-1), R M21 , R M22 , R M23 and R M24 Each independently represents a hydrogen atom or an organic group. M25 and R M26 Each independently represents a hydrogen atom or an alkyl group. M27 , RM28 , R M29 and R M30 Each independently represents a hydrogen atom or an organic group. M31 and R M32 Each independently represents a hydrogen atom or an alkyl group. M33 , R M34 , R M35 and R M36 Each independently represents a hydrogen atom or an organic group. M37 , R M38 and R M39 Each independently represents a hydrogen atom or an alkyl group. nx represents an integer of 1 to 20.

[0288] R in the formula M21 , R M22 , R M23 and R M24 Each independently represents a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and particularly preferably a methyl group. M21 and R M23 Preferably, R M22 and R M24 Preferred is a hydrogen atom.

[0289] R M25 and R M26 Each independently represents a hydrogen atom or an alkyl group, and is preferably an alkyl group. The alkyl group herein is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and among these, a methyl group is particularly preferred.

[0290] R M27 , R M28 , R M29 and R M30 Each independently represents a hydrogen atom or an organic group, preferably a hydrogen atom. The organic group here is preferably an alkyl group, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and particularly preferably a methyl group.

[0291] R M31 and R M32 Each independently represents a hydrogen atom or an alkyl group, and is preferably an alkyl group. The alkyl group herein is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and among these, a methyl group is particularly preferred.

[0292] R M33 , R M34 , R M35 and RM36 Each independently represents a hydrogen atom or an organic group. The organic group here is preferably an alkyl group, more preferably an alkyl group having 1 to 12 carbon atoms, further preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and particularly preferably a methyl group.

[0293] R M33 and R M36 Preferably, a hydrogen atom, R M34 and R M35 An alkyl group is preferred.

[0294] R M37 , R M38 and R M39 Each independently represents a hydrogen atom or an alkyl group, and is preferably an alkyl group. The alkyl group herein is preferably an alkyl group having 1 to 12 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, further preferably a methyl group, an ethyl group, a propyl group, or a butyl group, and among these, a methyl group is particularly preferred.

[0295] nx represents an integer of 1 to 20. nx may be an integer of 10 or less.

[0296] The compound represented by formula (M1-1) is preferably a compound represented by the following formula (M1-2).

[0297]

[0298] (In formula (M1-2), R M21 , R M22 , R M23 and R M24 Each independently represents a hydrogen atom or an organic group. M25 and R M26 Each independently represents a hydrogen atom or an alkyl group. M27 , R M28 , R M29 and R M30 Each independently represents a hydrogen atom or an organic group. M31 and R M32 Each independently represents a hydrogen atom or an alkyl group. M33 , R M34 , R M35 and R M36 Each independently represents a hydrogen atom or an organic group. M37 , R M38 and R M39 Each independently represents a hydrogen atom or an alkyl group. nx represents an integer of 1 to 20.

[0299] In formula (M1-2), R M21 , R M22 , R M23 , R M24, R M25 , R M26 , R M27 , R M28 , R M29 , R M30 , R M31 , R M32 , R M33 , R M34 , R M35 , R M36 , R M37 , R M38 , R M39 and nx are respectively the same as R in formula (M1-1) M21 , R M22 , R M23 , R M24 , R M25 , R M26 , R M27 , R M28 , R M29 , R M30 , R M31 , R M32 , R M33 , R M34 , R M35 , R M36 , R M37 , R M38 , R M39 It has the same meaning as nx and the preferred range is also the same.

[0300] The compound represented by the formula (M1-1) is preferably a compound represented by the following formula (M1-3), and more preferably a compound represented by the following formula (M1-4).

[0301]

[0302] (In formula (M1-3), nx represents an integer of 1 to 20.)

[0303] nx may be an integer less than 10.

[0304]

[0305] (In formula (M1-4), nx represents an integer of 1 to 20.)

[0306] nx may be an integer less than 10.

[0307] The molecular weight of the compound represented by formula (M1) is preferably 500 or more, more preferably 600 or more, and further preferably 700 or more. By setting it to above the aforementioned lower limit, there is a tendency that the low dielectric properties (Dk and / or Df) and low water absorption of the obtained cured product are further improved. In addition, the molecular weight of the compound represented by formula (M1) is preferably 10000 or less, more preferably 9000 or less, further preferably 7000 or less, further preferably 5000 or less, and further preferably 4000 or less. By setting it to below the aforementioned upper limit, there is a tendency that the heat resistance and handleability of the obtained cured product are further improved.

[0308] The maleimide equivalent of the compound represented by formula (M1) is preferably 50 g / eq. or more, more preferably 100 g / eq. or more, and further preferably 200 g / eq. or more. The upper limit of the maleimide equivalent is preferably 2000 g / eq. or less, more preferably 1000 g / eq. or less, and further preferably 800 g / eq. or less. Here, the maleimide equivalent represents the mass of the maleimide compound per 1 equivalent of maleimide group. When the maleimide equivalent of the compound represented by formula (M1) is within the above range, there is a tendency that the low dielectric properties (Dk and / or Df), low water absorption, heat resistance and handling properties of the obtained cured product are further improved.

[0309] The molecular weight distribution Mw / Mn of the compound represented by formula (M1) calculated by gel permeation chromatography (GPC) is preferably 1.0 to 4.0, more preferably 1.1 to 3.8, further preferably 1.2 to 3.6, and further preferably 1.3 to 3.4. When the Mw / Mn of the compound represented by formula (M1) is within the above range, the low dielectric properties (Dk and / or Df), low water absorption, heat resistance and handling properties of the obtained cured product tend to be further improved.

[0310] In addition, for details of the compound represented by formula (M1), reference can be made to the description of International Publication No. 2020-217679, the contents of which are incorporated into the present specification.

[0311]

[0312] (In formula (M2), R 54 Each independently represents a hydrogen atom or a methyl group, and n4 represents an integer greater than 1.)

[0313] n4 is preferably an integer of 1 to 10, more preferably an integer of 1 to 5, further preferably an integer of 1 to 3, further preferably 1 or 2, and may be 1.

[0314] The compound represented by formula (M2) may be a mixture of compounds having different n4, preferably a mixture. In addition, as described in the part of the compound represented by formula (M0), it may be a mixture of compounds having different other parts.

[0315]

[0316] (In formula (M3), R 55 Each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms, or a phenyl group, and n5 represents an integer of 1 to 10.

[0317] R 55 Each independently is preferably one selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group and a phenyl group, more preferably a hydrogen atom and / or a methyl group, and further preferably a hydrogen atom.

[0318] n5 is preferably an integer of 1 to 5, more preferably an integer of 1 to 3, and even more preferably 1 or 2.

[0319] The compound represented by formula (M3) may be a mixture of compounds having different n5, preferably a mixture. In addition, as described in the part of the compound represented by formula (M0), it may be a mixture of compounds having different other parts.

[0320]

[0321] (In formula (M4), R 56 Each independently represents a hydrogen atom, a methyl group or an ethyl group, and R 57 Each independently represents a hydrogen atom or a methyl group. )

[0322] R 56 Each of the two benzene rings is preferably a methyl group or an ethyl group, and more preferably a methyl group and an ethyl group in each of the two benzene rings. 57 Preferred is methyl.

[0323]

[0324] (In formula (M5), R 58 Each independently represents a hydrogen atom, an alkyl group having 1 to 8 carbon atoms or a phenyl group, and R 59 Each independently represents a hydrogen atom or a methyl group, and n6 represents an integer greater than 1.)

[0325] R 58 Each independently is preferably one selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, an n-pentyl group and a phenyl group, more preferably a hydrogen atom and / or a methyl group, and further preferably a hydrogen atom.

[0326] R 59 Preferred is methyl.

[0327] n6 is preferably an integer of 1 to 10, more preferably an integer of 1 to 5, further preferably an integer of 1 to 3, further preferably 1 or 2, and may be 1.

[0328] The compound represented by formula (M5) may be a mixture of compounds having different n6, preferably a mixture. In addition, as described in the part of the compound represented by formula (M0), it may be a mixture of compounds having different other parts.

[0329] The maleimide compound (M6) is a compound having a structural unit represented by the formula (M6) and having maleimide groups at both ends of the molecular chain.

[0330]

[0331] (In formula (M6), R 61 R represents a linear or branched alkylene group having 1 to 16 carbon atoms, or a linear or branched alkenylene group having 2 to 16 carbon atoms. 62 R represents a linear or branched alkylene group having 1 to 16 carbon atoms, or a linear or branched alkenylene group having 2 to 16 carbon atoms. 63 Each independently represents a linear or branched alkyl group having 1 to 16 carbon atoms, or a linear or branched alkenyl group having 2 to 16 carbon atoms. Each independently represents an integer of 0 to 10.

[0332] For details of the maleimide compound (M6) and its production method, reference can be made to the description in paragraphs 0061 to 0066 of International Publication No. 2020 / 262577, the contents of which are incorporated into this specification.

[0333] The maleimide compound (M7) is a maleimide compound comprising an aromatic amine compound (a1) having one or more and three or less alkyl groups on the aromatic ring, an aromatic divinyl compound (a2) having two vinyl groups, and maleic anhydride as reaction materials (1).

[0334] The maleimide compound (M7) is preferably a compound represented by formula (M7).

[0335]

[0336] (In the above formula (M7), R 1 Each independently represents the aforementioned alkyl group, R 2 each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms; an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms; a cycloalkyl group having 3 to 10 carbon atoms; a halogen atom; a hydroxyl group; or a mercapto group,

[0337] R 3 , R 4 , R 5 and R 6 Each independently represents a hydrogen atom or a methyl group, and R 3 and R 4 One of them is a hydrogen atom and the other is a methyl group. 5 and R 6 One of them is a hydrogen atom and the other is a methyl group.

[0338] X 1 represents a substituent represented by the following formula (x),

[0339]

[0340] (In formula (x), R 7 and R 8 Each independently represents a hydrogen atom or a methyl group, and R 7 and R 8 One of them is a hydrogen atom and the other is a methyl group, R 9 Each independently represents an alkyl group, alkoxy group or alkylthio group having 1 to 10 carbon atoms; an aryl group, aryloxy group or arylthio group having 6 to 10 carbon atoms; a cycloalkyl group having 3 to 10 carbon atoms; a halogen atom; a hydroxyl group; or a mercapto group, and t represents an integer of 0 to 4.

[0341] r is the number of X per bond 1 The X of the benzene ring 1 The average value of the number of substitutions is represented by , p represents an integer from 1 to 3, q ​​represents an integer from 0 to 4, and k represents an integer from 1 to 100. )

[0342] The details of the polymaleimide compound (M7) used in the present embodiment can be found in Japanese Patent No. 7160151, the contents of which are incorporated herein.

[0343] The maleimide compound can be produced by a known method, or a commercially available product can be used. As commercially available products, for example, as a compound represented by formula (M0), "BMI-80" manufactured by KI Chemicals Co., Ltd. can be listed; as a compound represented by formula (M1), "NE-X-9470S" manufactured by DIC Corporation can be listed; as a compound represented by formula (M2), "BMI-2300" manufactured by Yamato Chemical Industries, Ltd. can be listed; as a compound represented by formula (M3), "MIR-3000-70MT" manufactured by Nippon Kayaku Co., Ltd. can be listed; as a compound represented by formula (M4), "BMI-70" manufactured by KI Chemicals Co., Ltd. can be listed; as a compound represented by formula (M5), "MIR-5000" manufactured by Nippon Kayaku Co., Ltd. can be listed; as a maleimide compound (M6), "MIZ-001" manufactured by Nippon Kayaku Co., Ltd. can be listed; as a maleimide compound (M7), "NE-X-9500" manufactured by DIC Corporation can be listed.

[0344] In addition, examples of maleimide compounds other than the above include N-phenylmaleimide, N-cyclohexylmaleimide, oligomers of phenylmethanemaleimide, m-phenylene bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, 4,4'-diphenyl ether bismaleimide, 4,4'-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimidephenoxy)benzene, 1,3-bis(4-maleimidephenoxy)benzene, prepolymers thereof, and prepolymers of these maleimides and amines.

[0345] Among them, monofunctional maleimide compounds such as N-phenylmaleimide and N-cyclohexylmaleimide tend to provide a resin composition capable of providing a cured product having better low dielectric properties by using them in combination with a polymer having a structural unit represented by the following formula (V).

[0346] When the resin combination of the present embodiment includes maleimide compounds, the lower limit of its content is preferably more than 1 mass part relative to 100 mass parts of resin solids in the resin combination, more preferably more than 5 mass parts, more preferably more than 10 mass parts, more preferably more than 20 mass parts, more preferably more than 25 mass parts. By making the content of maleimide compounds more than 1 mass part, so that there is a tendency for the low dielectric properties and flame retardancy of the cured product obtained to improve. In addition, the upper limit of the content of maleimide compounds is preferably less than 70 mass parts relative to 100 mass parts of resin solids in the resin combination, more preferably less than 50 mass parts, or less than 40 mass parts. By making the content of maleimide compounds less than 70 mass parts, so that there is a tendency for metal foil peeling strength and low water absorption to improve.

[0347] The resin composition of the present embodiment may contain only one maleimide compound or two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0348] In addition, the resin composition in the present embodiment may also be a composition that does not substantially contain a maleimide compound. Substantially containing means that the content of the maleimide compound is less than 1 mass part, preferably less than 0.1 mass part, and more preferably less than 0.01 mass part, relative to 100 mass parts of resin solid components in the resin composition.

[0349] <<Cyanate Ester Compounds>>

[0350] The resin composition of the present embodiment may contain a cyanate compound.

[0351] The cyanate compound is not particularly limited as long as it is a compound containing one or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, further preferably 2 or 3, further preferably 2) cyanate groups (cyanato groups) in the molecule, and a wide range of compounds commonly used in the field of printed wiring boards can be used.

[0352] The cyanate ester compound is preferably a cyanate ester compound which is generally used for printed wiring boards and has two or more aromatic moieties substituted with at least one cyanato group in the molecule.

[0353] Specifically, the lower limit of the number of cyanato groups possessed by the cyanate ester compound is preferably more than 2, more preferably more than 3. By being set to below the above-mentioned upper limit, there is a tendency for heat resistance to further improve. In addition, the upper limit of the number of cyanato groups is preferably less than 100, more preferably less than 50.

[0354] In addition, the cyanate compound preferably has excellent low dielectric properties (Dk and / or Df) of its cured product. For example, the cured product of the cyanate compound preferably has a dielectric constant (Dk) of 4.0 or less at a frequency of 10 GHz measured by a cavity resonator perturbation method, more preferably less than 3.5. In addition, the lower limit of the aforementioned dielectric constant is, for example, 2.0 or more, which is practical. In addition, the cured product of the cyanate compound (B) preferably has a dielectric loss tangent (Df) of 0.02 or less at a frequency of 10 GHz measured by a cavity resonator perturbation method, more preferably less than 0.015. In addition, the lower limit of the aforementioned dielectric loss tangent is, for example, 0.0001 or more, which is practical. Dielectric constant, dielectric loss tangent, for example, can be measured according to the method (curing conditions, measurement conditions) described in the embodiment.

[0355] In addition, the cyanate compound preferably has a high heat resistance in its cured product. The cured product of the cyanate compound preferably has a glass transition temperature of 150° C. or higher, more preferably 180° C. or higher, and further preferably 200° C. or higher, as measured by dynamic viscoelasticity measurement according to JIS C6481. By setting the glass transition temperature to be above the above lower limit, a cured product having excellent heat resistance can be obtained.

[0356] The weight average molecular weight of the cyanate ester compound based on polystyrene conversion by GPC method is preferably 200 or more, more preferably 300 or more, and further preferably 400 or more. By setting the weight average molecular weight to above the aforementioned lower limit, there is a tendency for heat resistance to be further improved. In addition, the weight average molecular weight of the cyanate ester compound is preferably 1000 or less, more preferably 900 or less, and further preferably 800 or less. By setting the weight average molecular weight to below the aforementioned upper limit, there is a tendency for formability and handleability to be further improved.

[0357] For the preferred range of the cyanate ester compound, reference may be made to the description in paragraphs 0028 to 0033 of International Publication No. 2021 / 172317, the contents of which are incorporated herein.

[0358] Preferred cyanate compounds include at least one selected from the group consisting of phenol novolac type cyanate compounds, naphthol aralkyl type cyanate compounds (naphthol aralkyl type cyanate), naphthylene ether type cyanate compounds, biphenyl aralkyl type cyanate compounds, xylene resin type cyanate compounds, triphenol methane type cyanate compounds, adamantane skeleton type cyanate compounds, bisphenol M type cyanate compounds and bisphenol A type cyanate compounds. Among these, from the viewpoint of further improving low water absorption, at least one selected from the group consisting of phenol novolac type cyanate ester compounds, naphthol aralkyl type cyanate ester compounds, naphthylene ether type cyanate ester compounds, xylene resin type cyanate ester compounds, bisphenol M type cyanate ester compounds, and bisphenol A type cyanate ester compounds is preferred; at least one selected from the group consisting of phenol novolac type cyanate ester compounds, naphthol aralkyl type cyanate ester compounds, naphthylene ether type cyanate ester compounds, bisphenol A type cyanate ester compounds, and bisphenol M type cyanate ester compounds is more preferred; at least one selected from the group consisting of phenol novolac type cyanate ester compounds, naphthol aralkyl type cyanate ester compounds, and bisphenol A type cyanate ester compounds is further preferred; naphthol aralkyl type cyanate ester compounds and / or bisphenol A type cyanate ester compounds are further preferred; and naphthol aralkyl type cyanate ester compounds are further preferred.

[0359] As the naphthol aralkyl type cyanate ester compound, a compound represented by formula (N1) is more preferable.

[0360] Formula (N1)

[0361]

[0362] (In formula (N1), R 3 Each independently represents a hydrogen atom or a methyl group, and n3 represents an integer greater than 1.)

[0363] In formula (N1), R 3 Each independently represents a hydrogen atom or a methyl group, among which a hydrogen atom is preferred.

[0364] In formula (N1), n3 is an integer of 1 or more, preferably an integer of 1-50, more preferably an integer of 1-20, further preferably an integer of 1-10, and further preferably an integer of 1-6.

[0365] The phenol novolac-type cyanate compound is not particularly limited, but is preferably a compound represented by the following formula (VII), for example.

[0366]

[0367] (In formula (VII), R 6 Each independently represents a hydrogen atom or a methyl group, and n7 represents an integer greater than 1.)

[0368] In formula (VII), R 6 Each independently represents a hydrogen atom or a methyl group, among which a hydrogen atom is preferred.

[0369] In formula (VII), n7 is an integer of 1 or more, preferably an integer of 1-20, more preferably an integer of 1-10, and further preferably an integer of 1-6.

[0370] As the bisphenol A type cyanate ester compound, one or more selected from the group consisting of 2,2-bis(4-cyanatophenyl)propane and a prepolymer of 2,2-bis(4-cyanatophenyl)propane can be used.

[0371] These cyanate compounds can be prepared by known methods, and commercially available products can also be used. It should be noted that the functional group equivalent number of the cyanate compounds with naphthol aralkyl skeleton, naphthylene ether skeleton, xylene skeleton, triphenol methane skeleton or adamantane skeleton is relatively large, and unreacted cyanate groups can decrease. Therefore, the resin composition using them has a tendency that low water absorption is more excellent. In addition, mainly due to having an aromatic skeleton or adamantane skeleton, there is a tendency that the coating adhesion further improves.

[0372] When the resin combination of the present embodiment includes cyanate compounds, the lower limit of its content is preferably more than 1 mass part relative to the resin solids 100 mass parts in the resin combination, more preferably more than 5 mass parts, further preferably more than 10 mass parts, and can also be more than 20 mass parts.By making the content of cyanate compounds be more than the above-mentioned lower limit, so as to have the tendency that heat resistance, combustion resistance, chemical resistance, low dielectric constant, low dielectric loss tangent, insulation improve.When the resin combination of the present embodiment includes cyanate compounds, the upper limit of the content of cyanate compounds is preferably less than 70 mass parts relative to the resin solids 100 mass parts in the resin combination, more preferably less than 60 mass parts, further preferably less than 50 mass parts, and can also be less than 40 mass parts, less than 30 mass parts.

[0373] The resin composition in the present embodiment may contain only one cyanate compound or two or more cyanate compounds. When containing two or more cyanate compounds, the total amount is preferably within the above range.

[0374] In addition, the resin composition in the present embodiment may also be configured to be substantially free of cyanate compounds. Substantially free means that the content of cyanate compounds is less than 1 mass part, preferably less than 0.1 mass part, and more preferably less than 0.01 mass part, relative to 100 mass parts of resin solids in the resin composition.

[0375] <<Epoxides>>

[0376] The resin composition of the present embodiment may contain an epoxy compound.

[0377] The epoxy compound is not particularly limited as long as it is a compound or resin having one or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, further preferably 2 or 3, further preferably 2) epoxy groups in one molecule, and a wide range of compounds commonly used in the field of printed wiring boards can be used.

[0378] Examples of the epoxy compound include bisphenol A epoxy resin, bisphenol E epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, phenol novolac epoxy resin, bisphenol A novolac epoxy resin, glycidyl ester epoxy resin, aralkyl novolac epoxy resin, biphenyl aralkyl epoxy resin, naphthylene ether epoxy resin, cresol novolac epoxy resin, polyfunctional phenol epoxy resin, naphthalene epoxy resin, anthracene epoxy resin, naphthalene skeleton-modified novolac epoxy resin, phenol aralkyl epoxy resin, naphthol aralkyl epoxy resin, dicyclopentadiene epoxy resin, biphenyl epoxy resin, alicyclic epoxy resin, polyol epoxy resin, phosphorus-containing epoxy resin, glycidylamine, glycidyl ester, compounds obtained by epoxidizing double bonds of butadiene or the like, compounds obtained by reacting hydroxyl-containing silicone resins with epichlorohydrin, and the like. By using these, the moldability and adhesion of the resin composition are improved. Among these, from the viewpoint of further improving flame retardancy and heat resistance, biphenyl aralkyl type epoxy resins, naphthylene ether type epoxy resins, multifunctional phenol type epoxy resins, and naphthalene type epoxy resins are preferred, and biphenyl aralkyl type epoxy resins are more preferred.

[0379] The resin composition of the present embodiment preferably includes epoxy compounds within the scope of not damaging the effect of the present invention. From the viewpoint of formability and adhesion, when the resin composition of the present embodiment includes epoxy compounds, its content is preferably 0.1 mass parts or more relative to 100 mass parts of resin solid components in the resin composition, more preferably 1 mass parts or more, and further preferably 2 mass parts or more. By making the content of epoxy compounds more than 0.1 mass parts, there is a tendency for metal foil peeling strength and toughness to improve. In the case where the resin composition of the present embodiment includes epoxy compounds, the upper limit of the content of epoxy compounds is preferably less than 50 mass parts relative to 100 mass parts of resin solid components in the resin composition, more preferably less than 30 mass parts, more preferably less than 20 mass parts, further preferably less than 10 mass parts, and can also be less than 8 mass parts, less than 5 mass parts. By making the content of epoxy compounds less than 50 mass parts, there is a tendency for the electrical properties of the cured product obtained to improve.

[0380] The resin composition in the present embodiment may contain only one epoxy compound or two or more epoxy compounds. When containing two or more epoxy compounds, the total amount is preferably within the above range.

[0381] In addition, the resin composition in the present embodiment may also be configured to be substantially free of epoxy compounds. Substantially free means that the content of epoxy compounds is less than 0.1 parts by mass, preferably less than 0.01 parts by mass, and further less than 0.001 parts by mass, relative to 100 parts by mass of the resin solid content in the resin composition.

[0382] <<Phenol compounds>>

[0383] The resin composition of the present embodiment may contain a phenol compound.

[0384] For details of the phenolic resin, reference may be made to paragraph 0049 of International Publication No. 2021 / 172317, the contents of which are incorporated into this specification.

[0385] The resin composition of the present embodiment preferably contains a phenol compound within a range that does not impair the effects of the present invention. When the resin composition of the present embodiment contains a phenol compound, its content is preferably 0.1 parts by mass or more relative to 100 parts by mass of the resin solid content in the resin composition, and preferably 50 parts by mass or less.

[0386] The resin composition in the present embodiment may contain only one phenol compound or two or more phenol compounds. When containing two or more phenol compounds, the total amount is preferably within the above range.

[0387] The resin composition in the present embodiment may be configured to contain substantially no phenol compound. Substantially containing no phenol compound means that the content of the phenol compound is less than 0.1 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0388] <<Compounds containing a (meth)allyl group>>

[0389] The resin composition of the present embodiment preferably contains a compound containing a (meth)allyl group, and more preferably contains a compound containing an allyl group.

[0390] The compound containing a (meth)allyl group is preferably a compound containing two or more (meth)allyl groups, and more preferably a compound containing two or more allyl groups.

[0391] The compound containing a (meth)allyl group is preferably a compound containing at least one selected from the group consisting of a (meth)allyl isocyanurate compound, a tri(meth)allyl cyanurate compound, a (meth)allyl-substituted nadic imide compound, a (meth)allyl compound having a glycoluril structure, and diallyl phthalate. It is more preferred that the compound contains at least one selected from the group consisting of a (meth)allyl isocyanurate compound, a (meth)allyl-substituted nadic imide compound, and a (meth)allyl compound having a glycoluril structure. It is further preferred that the compound contains a (meth)allyl isocyanurate compound and / or a (meth)allyl-substituted nadic imide compound. It is further preferred that the compound contains a (meth)allyl-substituted nadic imide compound.

[0392] Examples of the tri(meth)allyl cyanurate compound include tri(meth)allyl cyanurate compounds (for example, triallyl cyanurate having the structure shown below).

[0393]

[0394] In addition, examples of the compound containing a (meth)allyl group include resins having an allyl group described in International Publication No. 2022 / 210095 (for example, compounds described in Synthesis Examples 3, 4, 6, 20, and 22 of the publication), the contents of which are incorporated into the present specification.

[0395] When the resin combination of present embodiment contains the compound comprising (methyl) allyl, its molecular weight is preferably more than 195, more preferably more than 300, further preferably more than 400, more preferably more than 500.By being set as more than the above-mentioned lower limit, thereby there is the tendency that low dielectric properties, thermotolerance further improve.In addition, the molecular weight of the compound comprising (methyl) allyl is preferably below 3000, more preferably below 2000, further preferably below 1000, more preferably below 800.By being set as below the above-mentioned upper limit, thereby there is the tendency that low thermal expansion further improves.

[0396] When the resin combination of the present embodiment contains the compound comprising (meth) allyl, its content is preferably more than 1 mass part relative to 100 mass parts of the resin solids in the resin combination, more preferably more than 3 mass parts, more preferably more than 5 mass parts, and can also be more than 10 mass parts.By making the content of the compound comprising (meth) allyl as more than the above-mentioned lower limit, there is the tendency that excellent formability and heat resistance further improve.In addition, the upper limit of the content of the compound comprising (meth) allyl is preferably less than 40 mass parts relative to 100 mass parts of the resin solids in the resin combination, more preferably less than 30 mass parts, more preferably less than 20 mass parts.By making the content of the compound comprising (meth) allyl as less than the above-mentioned upper limit, there is the tendency that low thermal expansion further improves.

[0397] The resin composition of the present embodiment may contain only one compound containing a (meth)allyl group, or may contain two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0398] <<<(Meth)allyl isocyanurate compound>>>

[0399] As a (meth)allyl isocyanurate compound, as long as it is a compound having more than 2 (meth)allyl groups and having an isocyanurate ring (urate skeleton), there is no particular limitation. In the (meth)allyl isocyanurate compound, the number of (meth)allyl groups that become crosslinking points is large, so it is firmly cured with resin (A) and polyphenylene ether compound (B) and other resin components (such as other compounds (C)), and there is a tendency to obtain a cured product with low dielectric properties (Dk and / or Df) and excellent heat resistance. As a (meth)allyl isocyanurate compound, it is preferably a compound shown in formula (TA).

[0400] Formula (TA)

[0401]

[0402] (In formula (TA), R A represents a substituent).

[0403] In formula (TA), R A represents a substituent, and more preferably a substituent having a formula weight of 15 to 500.

[0404] R A The first example is an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms. By using an allyl compound having an alkyl group having 1 to 22 carbon atoms or an alkenyl group having 2 to 22 carbon atoms, a resin composition having excellent crosslinking properties and a cured product having high toughness can be provided. Thus, even when the resin composition does not contain a substrate such as glass cloth, cracking during etching treatment or the like can be suppressed.

[0405] From the viewpoint of improving workability, the carbon number of the alkyl group and / or alkenyl group is preferably 3 or more, more preferably 8 or more, further preferably 12 or more, and may be 18 or less. It is considered that, as a result, the resin fluidity of the resin composition becomes good, and the circuit filling property when a multilayer circuit substrate is produced using the resin composition of the present embodiment is more excellent.

[0406] R A A second example of is a group containing an allyl isocyanurate group. A When an allyl isocyanurate group is included, the compound represented by the formula (TA) is preferably a compound represented by the formula (TA-1).

[0407] Formula (TA-1)

[0408]

[0409] (In formula (TA-1), R A2 is a divalent linking group. )

[0410] In formula (TA-1), RA2 A divalent linking group having a formula weight of 54 to 250 is preferred, a divalent linking group having a formula weight of 54 to 250 and having carbon atoms at both ends is more preferred, and an aliphatic hydrocarbon group having 2 to 20 carbon atoms is further preferred (wherein the aliphatic hydrocarbon group may contain an ether group and may also have a hydroxyl group). More specifically, R A2 It is preferably a group represented by any one of the following formulae (i) to (iii).

[0411]

[0412] (In formulas (i) to (iii), p c1 represents the number of repeating units of the methylene group, which is an integer from 2 to 18. c2 represents the number of repeating units of oxyethylene, which is 0 or 1. * represents the bonding site. )

[0413] The aforementioned c1 It is preferably an integer of 2-10, more preferably an integer of 3-8, and even more preferably an integer of 3-5.

[0414] The aforementioned c2 It can be 0 or 1, preferably 1.

[0415] R A The third example is a phosphorus-based substituent.

[0416] R A2 The first example is preferred.

[0417] In the present embodiment, the reactive group (allyl group) equivalent of the compound represented by formula (TA) is preferably 1000 g / eq. or less. When the equivalent is 1000 g / eq. or less, it is considered that a high Tg can be obtained more reliably.

[0418] Examples of the aforementioned alkyl group having 1 to 22 carbon atoms include linear or branched alkyl groups, such as methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, and docosyl groups. Examples of the aforementioned alkenyl group having 2 to 22 carbon atoms include allyl and decenyl groups.

[0419] Specific examples of the compound represented by formula (TA) include triallyl isocyanurate, 5-octyl-1,3-diallyl isocyanurate, 5-dodecyl-1,3-diallyl isocyanurate, 5-tetradecyl-1,3-diallyl isocyanurate, 5-hexadecyl-1,3-diallyl isocyanurate, 5-octadecyl-1,3-diallyl isocyanurate, 5-eicosyl-1,3-diallyl isocyanurate, 5-docosyl-1,3-diallyl isocyanurate, 5-decenyl-1,3-diallyl isocyanurate, etc. These may be used alone or in combination of two or more, and may be used in the form of a prepolymer.

[0420] The method for producing the compound represented by formula (TA) is not particularly limited, and it can be obtained, for example, by the following method: diallyl isocyanurate and an alkyl halide are reacted in an aprotic polar solvent such as N,N'-dimethylformamide in the presence of an alkaline substance such as sodium hydroxide, potassium carbonate, triethylamine, etc. at a temperature of about 60°C to 150°C.

[0421] In addition, the compound represented by formula (TA) can also use commercial products. As commercial products, there are no particular limitations, and examples thereof include L-DAIC manufactured by Shikoku Chemical Industry Co., Ltd. and P-DAIC manufactured by Shikoku Chemical Industry Co., Ltd. having a phosphorus-based substituent. As triallyl isocyanurate, for example, TAIC manufactured by Shinryo Co., Ltd. can be listed. As the compound represented by formula (TA-1), for example, DD-1 manufactured by Shikoku Chemical Industry Co., Ltd. can be listed.

[0422] The molecular weight of the (meth)allyl isocyanurate compound (preferably the compound represented by formula (TA)) is preferably 200 or more, more preferably 300 or more, further preferably 400 or more, and further preferably 500 or more. By setting the molecular weight to the above lower limit value or more, there is a tendency that the low dielectric properties (Dk and / or Df) and heat resistance of the obtained cured product are further improved. In addition, the molecular weight of the (meth)allyl isocyanurate compound (preferably the compound represented by formula (TA)) is preferably 3000 or less, more preferably 2000 or less, further preferably 1000 or less, and further preferably 800 or less. By setting the molecular weight to the above upper limit value or less, there is a tendency that the low thermal expansion of the obtained cured product is further improved.

[0423] When the resin composition of the present embodiment includes (methyl) allyl isocyanurate compound, its content is preferably more than 1 mass part, more preferably more than 3 mass parts, more preferably more than 5 mass parts, and can also be more than 10 mass parts relative to 100 mass parts of resin solids in the resin composition.By setting the content of (methyl) allyl isocyanurate compound to more than the above-mentioned lower limit, there is a tendency that the excellent formability of the resin composition, the heat resistance of the obtained solidified material, and the low thermal expansion are further improved.In addition, the upper limit of the content of (methyl) allyl isocyanurate compound is preferably less than 40 mass parts relative to 100 mass parts of resin solids in the resin composition, more preferably less than 30 mass parts, and can also be less than 20 mass parts.By setting the content of (methyl) allyl isocyanurate compound to less than the above-mentioned upper limit, there is a tendency that the heat resistance of the obtained solidified material, low dielectric properties (Dk and / or Df) are further improved.

[0424] The resin composition of the present embodiment may contain only one (meth)allyl isocyanurate compound or two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0425] <<<(Meth)allyl-substituted nadic imide compounds>>>

[0426] The (meth)allyl-substituted nadic acid imide compound is not particularly limited as long as it is a compound having two or more (meth)allyl-substituted nadic acid imide groups in the molecule. Specific examples thereof include compounds represented by the following formula (AN).

[0427] Formula (AN)

[0428]

[0429] (In formula (AN), R1 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms, and R2 represents an alkylene group having 1 to 6 carbon atoms, a phenylene group, a biphenylene group, a naphthylene group, or a group represented by formula (AN-2) or (AN-3).

[0430] Formula (AN-2)

[0431]

[0432] (In formula (AN-2), R3 represents a methylene group, an isopropylidene group, a group represented by -C(=O)-, -O-, -S-, or -S(=O)2-.)

[0433] Formula (AN-3)

[0434]

[0435] (In formula (AN-3), R4 each independently represents an alkylene group having 1 to 4 carbon atoms or a cycloalkylene group having 5 to 8 carbon atoms.)

[0436] In addition, the compound shown in formula (AN) can also use commercial products. As commercial products, there are no particular limitations, and examples thereof include compounds shown in formula (AN-4) (BANI-M (made by Maruzen Petrochemical Co., Ltd.)), compounds shown in formula (AN-5) (BANI-X (made by Maruzen Petrochemical Co., Ltd.)), etc. These can be used alone or in combination of two or more.

[0437] Formula (AN-4)

[0438]

[0439] Formula (AN-5)

[0440]

[0441] The molecular weight of the (meth)allyl-substituted nadic imide compound (preferably the compound shown in formula (AN)) is preferably 400 or more, more preferably 500 or more, and may be 550 or more. By setting the molecular weight of the (meth)allyl-substituted nadic imide compound to above the above lower limit, there is a tendency for low dielectric properties, low thermal expansion, and heat resistance to be further improved. In addition, the molecular weight of the (meth)allyl-substituted nadic imide compound (preferably the compound shown in formula (AN)) is preferably 1500 or less, more preferably 1000 or less, further preferably 800 or less, and may be 700 or less, 600 or less. By setting the molecular weight of the (meth)allyl-substituted nadic imide compound to below the above upper limit, there is a tendency for formability and peel strength to be further improved.

[0442] When the resin composition of the present embodiment includes (methyl) allyl substituted nadic imide compound (preferably the compound shown in formula (AN)), its content is preferably more than 1 mass part relative to 100 mass parts of resin solids in the resin composition, more preferably more than 3 mass parts, more preferably more than 5 mass parts, and can also be more than 10 mass parts. By setting the content of (methyl) allyl substituted nadic imide compound to more than the above-mentioned lower limit, there is a tendency that excellent formability, low dielectric, low thermal expansion, and heat resistance are further improved. In addition, the upper limit of the content of (methyl) allyl substituted nadic imide compound (preferably the compound shown in formula (AN)) is preferably less than 40 mass parts relative to 100 mass parts of resin solids in the resin composition, more preferably less than 30 mass parts, more preferably less than 25 mass parts, and can also be less than 20 mass parts. By setting the content of (methyl) allyl substituted nadic imide compound to less than the above-mentioned upper limit, there is a tendency that formability and peel strength are further improved.

[0443] The resin composition of the present embodiment may contain only one (meth)allyl-substituted nadic acid imide compound, or may contain two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0444] <<<(Meth)allyl compounds having a glycoluril structure>>>

[0445] As the (meth) allyl compound with glycoluril structure, as long as it is a compound comprising glycoluril structure and more than 2 (meth) allyl groups, it is not particularly limited. When the (meth) allyl compound with glycoluril structure is mixed in the resin composition, the number of (meth) allyl groups can also be increased, that is, crosslinking points can also be increased. Therefore, similarly to the (meth) allyl isocyanurate compound, it is firmly cured with resin (A) and polyphenylene ether compound (B) and other resin components (such as other compounds (C)), and there is a tendency to obtain a cured product with low dielectric properties (Dk and / or Df) and excellent heat resistance.

[0446] In the present embodiment, the (meth)allyl compound having a glycoluril structure is preferably a compound represented by formula (GU).

[0447] Formula(GU)

[0448]

[0449] (In formula (GU), each R is independently a hydrogen atom or a substituent, and at least two Rs are groups containing a (meth)allyl group.)

[0450] In formula (GU), each R is independently preferably a hydrogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkenyl group having 2 to 5 carbon atoms, preferably an alkenyl group having 2 to 5 carbon atoms, more preferably a (meth)allyl group, and further preferably an allyl group.

[0451] In formula (GU), preferably 3 or 4 Rs are groups containing a (meth)allyl group, and more preferably 4 Rs are groups containing a (meth)allyl group.

[0452] Specific examples of the compound represented by formula (GU) include 1,3,4,6-tetraallyl glycoluril (a compound in which all R in formula (GU) are allyl groups).

[0453] In addition, a commercially available product may be used as the compound represented by the formula (GU). The commercially available product is not particularly limited, and an example thereof includes TA-G manufactured by Shikoku Chemicals Co., Ltd.

[0454] The molecular weight of the (meth) allyl compound (preferably the compound shown in formula (GU)) having a glycoluril structure is preferably 195 or more, more preferably 220 or more, further preferably 250 or more, and may be 300 or more, 400 or more. By setting the molecular weight of the (meth) allyl compound having a glycoluril structure to above the above lower limit, the heat resistance and low thermal expansion of the obtained solidified material tend to be further improved. In addition, the molecular weight of the (meth) allyl compound (preferably the compound shown in formula (GU)) having a glycoluril structure is preferably 1500 or less, more preferably 1000 or less, further preferably 800 or less, and may be 700 or less, 600 or less. By setting the molecular weight of the (meth) allyl compound having a glycoluril structure to below the above upper limit, the low dielectric properties (Dk and / or Df) and heat resistance of the obtained solidified material tend to be further improved.

[0455] When the resin composition of the present embodiment includes a (methyl) allyl compound (preferably a compound shown in formula (GU)) with a glycoluril structure, its content is preferably more than 1 mass part relative to 100 mass parts of the resin solids in the resin composition, more preferably more than 3 mass parts, more preferably more than 5 mass parts, and can also be more than 10 mass parts. By setting the content of the (methyl) allyl compound with glycoluril structure to more than the above-mentioned lower limit, there is a tendency that the formability of the resin composition is excellent, the heat resistance of the obtained cured product and the low thermal expansion are further improved. In addition, the upper limit of the content of the (methyl) allyl compound (preferably a compound shown in formula (GU)) with glycoluril structure is preferably less than 40 mass parts relative to 100 mass parts of the resin solids in the resin composition, more preferably less than 30 mass parts, more preferably less than 25 mass parts, and can also be less than 20 mass parts. By setting the content of the (methyl) allyl compound with glycoluril structure to less than the above-mentioned upper limit, there is a tendency that the low dielectric properties (Dk and / or Df) of the cured product obtained are further improved.

[0456] The resin composition of the present embodiment may contain only one (meth)allyl compound having a glycoluril structure, or may contain two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0457] <<Oxetane Resin>>

[0458] The resin composition of the present embodiment may contain an oxetane resin.

[0459] The oxetane resin is not particularly limited as long as it is a compound having one or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, further preferably 2 or 3, further preferably 2) oxetane groups, and a wide range of compounds commonly used in the field of printed wiring boards can be used.

[0460] Examples of the oxetane resin include oxetane, alkyloxetane (e.g., 2-methyloxetane, 2,2-dimethyloxetane, 3-methyloxetane, 3,3-dimethyloxetane, etc.), 3-methyl-3-methoxymethyloxetane, 3,3-bis(trifluoromethyl)oxetane, 2-chloromethyloxetane, 3,3-bis(chloromethyl)oxetane, biphenyl-type oxetane, OXT-101 (manufactured by Toagosei Co., Ltd.), and OXT-121 (manufactured by Toagosei Co., Ltd.).

[0461] The resin composition of the present embodiment preferably includes an oxetane resin within the scope of not damaging the effect of the present invention. In the case where the resin composition of the present embodiment includes an oxetane resin, its content is preferably 0.1 mass parts or more, more preferably 1 mass parts or more, and further preferably 2 mass parts or more relative to 100 mass parts of resin solids in the resin composition. By making the content of the oxetane resin more than 0.1 mass parts, there is a tendency that the metal foil peel strength and toughness of the obtained cured product are improved. In the case where the resin composition of the present embodiment includes an oxetane resin, the upper limit of the content of the oxetane resin is preferably 50 mass parts or less, more preferably 30 mass parts or less, further preferably 20 mass parts or less, further preferably 10 mass parts or less, and further preferably 8 mass parts or less relative to 100 mass parts of resin solids in the resin composition. By making the content of the oxetane resin less than 50 mass parts, there is a tendency that the electrical properties of the cured product obtained are improved.

[0462] The resin composition in the present embodiment may contain only one oxetane resin or two or more oxetane resins. When containing two or more oxetane resins, the total amount is preferably within the above range.

[0463] The resin composition in the present embodiment may be configured to contain substantially no oxetane resin. Substantially containing no oxetane resin means that the content of the oxetane resin is less than 0.1 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0464] <<Benzoxazine compounds>>

[0465] The resin composition of the present embodiment may contain a benzoxazine compound.

[0466] The benzoxazine compound is not particularly limited as long as it is a compound having two or more (preferably 2 to 12, more preferably 2 to 6, further preferably 2 to 4, further preferably 2 or 3, further preferably 2) dihydrobenzoxazine rings in one molecule, and compounds commonly used in the field of printed wiring boards can be widely used.

[0467] Examples of the benzoxazine compound include bisphenol A-type benzoxazine BA-BXZ (manufactured by Konishi Chemical Co., Ltd.), bisphenol F-type benzoxazine BF-BXZ (manufactured by Konishi Chemical Co., Ltd.), and bisphenol S-type benzoxazine BS-BXZ (manufactured by Konishi Chemical Co., Ltd.).

[0468] The resin composition of the present embodiment preferably contains a benzoxazine compound within a range that does not impair the effects of the present invention. When the resin composition of the present embodiment contains a benzoxazine compound, the content thereof is preferably 0.1 parts by mass or more and preferably 50 parts by mass or less relative to 100 parts by mass of the resin solid content in the resin composition.

[0469] The resin composition in the present embodiment may contain only one benzoxazine compound or two or more benzoxazine compounds. When containing two or more benzoxazine compounds, the total amount is preferably within the above range.

[0470] The resin composition in the present embodiment may also be configured to contain substantially no benzoxazine compound. Substantially containing no benzoxazine compound means that the content of the benzoxazine compound is less than 0.1 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

[0471] <<Aryl cyclobutene resin>>

[0472] The resin composition of the present embodiment may contain an arylcyclobutene resin.

[0473] The details thereof can be exemplified by the aryl cyclobutene resin described in paragraph 0042 of JP-A-2019-194312, and the contents thereof are incorporated into the present specification.

[0474] <<Polyamide resin>>

[0475] The resin composition of the present embodiment may contain a polyamide resin, or may contain a thermosetting polyamide resin.

[0476] For details, reference may be made to the polyamide described in paragraph 0065 of Japanese Patent Application Publication No. 2019-194312 and the polyamide described in paragraph 0063 of Japanese Patent Application No. 6951829, and the contents thereof are incorporated into this specification.

[0477] <<Polyimide resin>>

[0478] The resin composition of the present embodiment may contain a polyimide resin, or may contain a thermosetting polyimide resin.

[0479] For details, reference may be made to polyimide and the like described in paragraphs 0063 to 0064 of Japanese Patent No. 6951829, the contents of which are incorporated herein by reference.

[0480] <<Perfluorovinyl ether resin>>

[0481] The resin composition of the present embodiment may contain a perfluorovinyl ether resin, or may contain a perfluorovinyl benzyl ether resin.

[0482] The details thereof can be exemplified by the perfluorovinyl ether resin described in paragraph 0043 of JP-A-2019-194312, and the contents thereof are incorporated into the present specification.

[0483] <<Compounds Having a Styrene Group Other Than the Polyphenylene Ether Compound (B) Having a Carbon-Carbon Unsaturated Double Bond at the Terminal>>

[0484] The resin composition of the present embodiment may contain a compound having a styrene group other than the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal.

[0485] Their details include compounds having styrene at the end described in International Publication No. 2022 / 210095 (for example, compounds described in Synthesis Examples 12 to 16 of the publication), descriptions in paragraphs 0029 to 0038 of Japanese Patent Publication No. 2022-85610, and vinyl benzyl ether resins described in paragraph 0041 of Japanese Patent Publication No. 2019-194312, and the like, and these contents are incorporated into this specification.

[0486] <<Compounds having an isopropenyl group other than the resin (A) having an indane skeleton>>

[0487] The resin composition of the present embodiment may contain a compound having an isopropenyl group other than the resin (A) having an indane skeleton.

[0488] The details thereof include the resins having an isopropylene group described in International Publication No. 2022 / 210095 (for example, the compounds described in Synthesis Examples 1, 2, 7, and 8 of the publication), and the contents thereof are incorporated into the present specification.

[0489] <<Polyfunctional (meth)acrylate compounds other than the aforementioned polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal>>

[0490] The resin composition of the present embodiment may contain a multifunctional (meth)acrylate compound other than the aforementioned polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal. Here, the multifunctional (meth)acrylate compound refers to a compound containing two or more (meth)acryloyloxy groups in one molecule, preferably containing three or more (meth)acryloyloxy groups in one molecule.

[0491] The polyfunctional (meth)acrylate compound is preferably a compound having 3 to 5 (meth)acryloyloxy groups, more preferably a compound having 3 or 4 (meth)acryloyloxy groups, and further preferably a compound having 3 (meth)acryloyloxy groups. The (meth)acrylate compound is preferably a compound having a methacryloyloxy group.

[0492] In the multifunctional (meth)acrylate compound, the number of (meth)acrylate groups that serve as crosslinking points is large, so it is firmly cured with the resin (A), the polyphenylene ether compound (B), and other resin components (such as other compounds (C)), and there is a tendency to obtain a cured product with low dielectric properties (Dk and / or Df) and excellent heat resistance. As the multifunctional (meth)acrylate compound, a compound represented by formula (MA) is preferred.

[0493] Formula (MA)

[0494]

[0495] (In formula (MA), R 1 represents a hydrogen atom or a substituent, R 2 Each independently represents a hydrogen atom or a methyl group. )

[0496] In formula (MA), R 1 It represents a hydrogen atom or a substituent, more preferably a substituent having a formula weight of 15 to 500, more preferably a substituent having a formula weight of 15 to 300, further preferably a substituent having a formula weight of 15 to 100, and further preferably a substituent having a formula weight of 15 to 50.

[0497] R 1 It is preferably a hydrocarbon group or a (meth)acryloyloxy group, more preferably a hydrocarbon group with a carbon number of 22 or less, and further preferably an alkyl group with a carbon number of 1 to 22, or an alkenyl group with a carbon number of 2 to 22. By using a compound having an alkyl group with a carbon number of 1 to 22, or an alkenyl group with a carbon number of 2 to 22, a resin composition that can obtain a cured product with excellent crosslinking properties and high toughness can be provided. Thus, even if a substrate such as glass cloth is not included in the resin composition, cracking during etching treatment can be suppressed.

[0498] From the viewpoint of improving workability, the carbon number of the alkyl group and / or alkenyl group is preferably 2 or more, may be 8 or more, further may be 12 or more, and may be 18 or less. It is considered that, as a result, the resin fluidity of the resin composition becomes good, and the circuit filling property when a multilayer circuit substrate is produced using the resin composition of the present embodiment is more excellent.

[0499] In this embodiment, the (meth)acrylic acid group equivalent of the compound represented by formula (MA) is preferably 1000 g / eq. or less. When the equivalent is 1000 g / eq. or less, there is a tendency to more reliably obtain a high Tg. The lower limit of the (meth)acrylic acid group equivalent is, for example, 99 g / eq. or more.

[0500] As the aforementioned alkyl group having 1 to 22 carbon atoms, a linear or branched alkyl group having 1 to 22 carbon atoms is preferred, and examples thereof include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, dodecyl, tetradecyl, hexadecyl, octadecyl, eicosyl, and docosyl. In addition, as the aforementioned alkenyl group having 2 to 22 carbon atoms, an alkenyl group having 2 to 15 carbon atoms is preferred, and examples thereof include allyl and decenyl.

[0501] Specific examples of the compound represented by formula (MA) include trimethylolpropane trimethacrylate, trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, etc. These may be used alone or in combination of two or more, or may be used in the form of a prepolymer.

[0502] In addition, a commercially available product may be used as the compound represented by the formula (MA). The commercially available product is not particularly limited, and for example, trimethylolpropane trimethacrylate includes "NK ESTERTM PT" manufactured by Shin-Nakamura Chemical Industry Co., Ltd.

[0503] The molecular weight of the multifunctional (meth)acrylate compound is preferably 300 or more, more preferably 330 or more, 400 or more, or 500 or more. By setting the molecular weight to be above the lower limit, the low dielectric properties (Dk and / or Df) and heat resistance of the obtained cured product tend to be further improved. In addition, the molecular weight of the (meth)acrylate compound (preferably a compound represented by formula (MA)) is preferably 3000 or less, more preferably 2000 or less, further preferably 1000 or less, and further preferably 800 or less. By setting the molecular weight to be below the upper limit, the low thermal expansion of the obtained cured product tends to be further improved.

[0504] Their details include the resins having a (meth)acrylic group described in International Publication No. 2022 / 210095 (for example, the compounds described in Synthesis Examples 5 and 21 of the publication) and the resins having a (meth)acrylic group of Japanese Patent No. 6962507 (for example, the compounds described in Examples 1 to 9), and the contents thereof are incorporated into the present specification.

[0505] When the resin combination of the present embodiment includes multifunctional (meth) acrylate compound, its content is preferably more than 1 mass part relative to 100 mass parts of the resin solids in the resin combination, more preferably more than 3 mass parts, further preferably more than 5 mass parts, and can also be more than 10 mass parts.By setting the content of multifunctional (meth) acrylate compound as more than the above-mentioned lower limit, there is the tendency that the excellent formability of resin combination, the heat resistance of the cured product obtained, and the low thermal expansion are further improved.In addition, the upper limit of the content of (meth) acrylate compound is preferably less than 40 mass parts relative to 100 mass parts of the resin solids in the resin combination, more preferably less than 30 mass parts, and can also be less than 20 mass parts.By setting the content of multifunctional (meth) acrylate compound as less than the above-mentioned upper limit, there is the tendency that the heat resistance of the cured product obtained, low dielectric properties (Dk and / or Df) are further improved.

[0506] The resin composition of the present embodiment may contain only one type of polyfunctional (meth)acrylate compound, or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.

[0507] <<Elastomer>>

[0508] The resin composition of the present embodiment may contain an elastomer. The elastomer may be thermoplastic or thermosetting, or may not exhibit either thermoplasticity or thermosetting properties, but is preferably thermoplastic.

[0509] The elastomer in this embodiment is not particularly limited, and examples thereof include at least one selected from the group consisting of polyisoprene, polybutadiene, styrene butadiene, butyl rubber, ethylene propylene rubber, styrene butadiene ethylene, styrene butadiene styrene, styrene isoprene styrene, styrene ethylene butylene styrene, styrene propylene styrene, styrene ethylene propylene styrene, fluororubber, silicone rubber, their hydrogenated compounds, their alkyl compounds, and their copolymers.

[0510] In addition, examples of the elastomer include oligomers or polymers having a curable vinyl functional group and polybutadiene resins described in paragraphs 0044 and 0045 of JP-A-2019-194312, and the contents thereof are incorporated into the present specification.

[0511] The number average molecular weight of the elastomer (preferably thermoplastic elastomer) used in the present embodiment is preferably more than 1000. By setting the number average molecular weight to more than 1000, there is a tendency that the low dielectric properties (Dk and / or Df, particularly low dielectric loss tangent) of the cured product obtained are more excellent. The number average molecular weight is preferably more than 1500, more preferably more than 2000, and according to purposes, it can also be more than 600000, more than 700000, more than 800000. The upper limit of the number average molecular weight of elastomer is preferably less than 400000, more preferably less than 350000, and further preferably less than 300000. By being set to below the aforementioned upper limit value, there is a tendency that the solubility of the elastomer component in the resin combination improves.

[0512] When the resin composition of the present embodiment contains two or more elastomers, it is preferred that the number average molecular weight of the mixture thereof satisfy the above range.

[0513] The elastomer used in the present embodiment may include a resin containing a polybutadiene structure. The polybutadiene structure may be partially or completely hydrogenated. As specific examples, B-1000, B-2000, B-3000, BI-2000, BI-3000 manufactured by Nippon Soda Co., Ltd., Ricon100, Ricon130, Ricon131, Ricon142, Ricon150, Ricon181, Ricon184, etc. manufactured by Cray Valley Co., Ltd. may be included.

[0514] The elastomer used in the present embodiment may be a resin containing a poly(meth)acrylate structure, and specific examples thereof include Teisan Resin manufactured by Nagase ChemteX Co., Ltd., and ME-2000, W-197C, KG-15, and KG-3000 manufactured by Negami Industries, Ltd.

[0515] The elastomer used in the present embodiment can be listed as a resin containing a polycarbonate structure. Sometimes the resin containing a polycarbonate structure is referred to as a "polycarbonate resin". As such a resin, carbonate resins without reactive groups, carbonate resins containing hydroxyl groups, carbonate resins containing phenolic hydroxyl groups, carbonate resins containing carboxyl groups, carbonate resins containing anhydride groups, carbonate resins containing isocyanate groups, carbonate resins containing carbamate groups, and carbonate resins containing epoxy groups can be listed. Here, reactive groups refer to functional groups that can react with other components such as hydroxyl groups, phenolic hydroxyl groups, carboxyl groups, anhydride groups, isocyanate groups, carbamate groups, and epoxy groups.

[0516] Specific examples of the polycarbonate resin include FPC0220 and FPC2136 manufactured by Mitsubishi Gas Chemical Co., Ltd., and T6002 and T6001 (polycarbonate diol) manufactured by Asahi Kasei Chemicals Corporation.

[0517] Examples of the elastomer used in the present embodiment include resins containing a polysiloxane structure, and specific examples thereof include SMP-2006, SMP-2003PGMEA, SMP-5005PGMEA, KR-510, and SMP-7014-3S manufactured by Shin-Etsu Silicone Co., Ltd.

[0518] The elastomer used in the present embodiment may include a resin containing a polyalkylene structure and / or a polyoxyalkylene structure. The polyoxyalkylene structure is preferably a polyoxyalkylene structure having 2 to 15 carbon atoms, more preferably a polyoxyalkylene structure having 3 to 10 carbon atoms, and particularly preferably a polyoxyalkylene structure having 5 to 6 carbon atoms. Specific examples of the resin containing a polyalkylene structure and / or a polyoxyalkylene structure include PTXG-1000 and PTXG-1800 manufactured by Asahi Kasei Fibers Corporation.

[0519] The elastomer used in the present embodiment may be a resin containing a polyisoprene structure, and specific examples thereof include KL-610 and KL613 manufactured by Kuraray Co., Ltd.

[0520] The elastomer used in the present embodiment may be a resin containing a polyisobutylene structure, and specific examples thereof include SIBSTAR-073T (styrene-isobutylene-styrene triblock copolymer) and SIBSTAR-042D (styrene-isobutylene diblock copolymer) manufactured by Kaneka Corporation.

[0521] In this embodiment, the elastomer is preferably an elastomer comprising a styrene monomer unit and a conjugated diene monomer unit (hereinafter referred to as "elastomer (e)"). By using such an elastomer (e), the low dielectric properties (Dk and / or Df, especially low dielectric loss tangent) of the obtained cured product are more excellent.

[0522] The elastomer (e) contains styrene monomer units. By containing styrene monomer units, the solubility of the elastomer (e) in the resin composition is improved. As styrene monomers, styrene, α-methylstyrene, p-methylstyrene, divinylbenzene (vinyl styrene), N,N-dimethyl-p-aminoethylstyrene, N,N-diethyl-p-aminoethylstyrene, etc. can be exemplified. Among these, styrene, α-methylstyrene, and p-methylstyrene are preferred from the viewpoint of availability and productivity. Among these, styrene is particularly preferred.

[0523] The content of the styrene monomer unit in the elastomer (e) is preferably in the range of 10 to 50% by mass of all monomer units, more preferably in the range of 13 to 45% by mass, and further preferably in the range of 15 to 40% by mass. If the content of the styrene monomer unit is 50% by mass or less, the adhesion and adhesiveness to the substrate etc. will become better. In addition, if it is 10% by mass or more, there is a tendency that the adhesion is suppressed from being too strong, residual glue and retention marks are not easily generated, and the easy peelability between the bonding surfaces becomes good, so it is preferred.

[0524] The elastomer (e) may contain only one type of styrene monomer unit, or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.

[0525] The method for measuring the content of the styrene monomer unit in the elastomer (e) of the present embodiment can refer to the description of International Publication No. 2017 / 126469, the contents of which are incorporated into the present specification. The same applies to the conjugated diene monomer unit described later.

[0526] The elastomer (e) comprises a conjugated diene monomer unit. By comprising a conjugated diene monomer unit, the solubility of the elastomer (e) in the resin composition is improved. As a conjugated diene monomer, there is no particular limitation as long as it is a diene having one pair of conjugated double bonds. Examples of conjugated diene monomers include 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene and farnesene, preferably 1,3-butadiene and isoprene, more preferably 1,3-butadiene.

[0527] The elastomer (e) may contain only one type of conjugated diene monomer unit, or may contain two or more types.

[0528] In the above-mentioned elastomer (e), the mass ratio of styrene monomer units to conjugated diene monomer units is preferably in the range of styrene monomer units / conjugated diene monomer units = 5 / 95 to 80 / 20, more preferably in the range of 7 / 93 to 77 / 23, and further preferably in the range of 10 / 90 to 70 / 30. If the mass ratio of styrene monomer units to conjugated diene monomer units is in the range of 5 / 95 to 80 / 20, it is possible to suppress excessive adhesion and maintain high adhesion, and the easy peelability between the adhesive surfaces becomes good.

[0529] In the above-mentioned elastomer (e), the conjugated diene bonds of the elastomer may be all hydrogenated, partially hydrogenated, or unhydrogenated.

[0530] The elastomer (e) may or may not contain other monomer units in addition to the styrene monomer unit and the conjugated diene monomer unit. Examples of the other monomer units include aromatic vinyl compound units other than the styrene monomer unit.

[0531] In the elastomer (e), the total content of styrene monomer units and conjugated diene monomer units is preferably 90% by mass or more of all monomer units, more preferably 95% by mass or more, further preferably 97% by mass or more, and further preferably 99% by mass or more.

[0532] As described above, the elastomer (e) may contain only one type of each of the styrene monomer unit and the conjugated diene monomer unit, or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.

[0533] The elastomer (e) used in this embodiment may be a block polymer or a random polymer. In addition, it may be a hydrogenated elastomer in which the conjugated diene monomer units are hydrogenated, an unhydrogenated elastomer that is not hydrogenated, or a partially hydrogenated elastomer, preferably an unhydrogenated elastomer or a partially hydrogenated elastomer.

[0534] In one embodiment of the present embodiment, the elastomer (e) is a hydrogenated elastomer. Here, the hydrogenated elastomer refers to an elastomer in which the double bonds based on the conjugated diene monomer unit are hydrogenated, and includes elastomers with a hydrogenation rate of 100% and elastomers with a hydrogenation rate of 80% or more. The hydrogenation rate of the hydrogenated elastomer is preferably 85% or more, more preferably 90% or more, and further preferably 95% or more. In the present embodiment, the hydrogenation rate is 1 The measurement results of H-NMR spectrum measurement were calculated.

[0535] In one embodiment of the present embodiment, the elastomer (e) is an unhydrogenated elastomer. Here, the unhydrogenated elastomer refers to an elastomer in which the ratio of double bonds based on conjugated diene monomer units in the elastomer that are hydrogenated, i.e., the hydrogenation rate, is 20% or less. The hydrogenation rate is preferably 15% or less, more preferably 10% or less, and further preferably 5% or less.

[0536] On the other hand, the partially hydrogenated elastomer refers to an elastomer in which a part of the double bonds based on the conjugated diene monomer units in the elastomer are hydrogenated, and generally refers to an elastomer in which the hydrogenation rate is lower than 80% and higher than 20%.

[0537] Examples of commercially available products of the elastomer (e) used in this embodiment include SEPTON (registered trademark) 2104, V9461, and S8104 manufactured by Kuraray Co., Ltd., SOE (registered trademark) S1606, S1613, S1609, and S1605 manufactured by Asahi Kasei Corporation, H1041, H1043, P2000, and MP10 of TUFTEC (registered trademark) manufactured by Asahi Kasei Corporation, and DYNARON (registered trademark) 9901P and TR2250 manufactured by JSR Corporation.

[0538] In addition, the elastomer used in this embodiment may also be a liquid diene. Liquid diene refers to a liquid elastomer containing a conjugated diene monomer unit. As conjugated diene monomers, 1,3-butadiene, 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene and farnesene can be listed, preferably 1,3-butadiene and isoprene, more preferably 1,3-butadiene.

[0539] Examples of the liquid diene used in the present embodiment include liquid polybutadiene, liquid polyisoprene, modified products of liquid polybutadiene, modified products of liquid polyisoprene, liquid acrylonitrile-butadiene copolymers, and liquid styrene-butadiene copolymers.

[0540] The number average molecular weight of the liquid diene is not particularly limited as long as it is liquid at 20°C, but is preferably 500 or more and 10,000 or less.

[0541] When the resin combination of the present embodiment includes elastomer (preferably elastomer (e)), its content is preferably more than 1 mass part, more preferably more than 5 mass parts, more preferably more than 8 mass parts, according to purposes etc., it can also be more than 10 mass parts, more than 12 mass parts.By being set to more than the aforementioned lower limit, there is a tendency that dielectric properties (low dielectric loss tangent) are further improved.In addition, the upper limit of the content of elastomer is preferably less than 45 mass parts, more preferably less than 40 mass parts, more preferably less than 35 mass parts, more preferably less than 32 mass parts, more preferably less than 28 mass parts.By being set to less than the above-mentioned upper limit, there is a tendency that heat resistance is further improved.

[0542] The resin composition of the present embodiment may contain only one type of elastomer, or may contain two or more types. When containing two or more types, the total amount is preferably within the above range.

[0543] In addition, the resin composition in the present embodiment may be configured to contain substantially no elastomer, which means that the content of the elastomer is less than 1 part by mass, preferably less than 0.1 part by mass, and more preferably less than 0.01 part by mass, relative to 100 parts by mass of the resin solid content in the resin composition.

[0544] <<Petroleum Resin>>

[0545] The resin composition of this embodiment may contain a petroleum resin. By containing a petroleum resin, the melt viscosity can be reduced.

[0546] Petroleum resin is a resin obtained by polymerizing the remaining components after thermally decomposing naphtha and taking necessary fractions without separating unsaturated hydrocarbons, in the absence of a catalyst or in the presence of a catalyst. The remaining fractions are mainly fractions containing C5 fractions (isoprene, piperylene, cyclopentadiene, pentenes, pentanes, etc.) or C9 fractions (vinyl toluene, indene, dicyclopentadiene, etc.).

[0547] The catalyst used for the manufacture of petroleum resin is preferably an acidic catalyst. Specifically, solid acids such as Lewis acids such as boron trifluoride phenol complex, boron trifluoride ether complex, aluminum chloride, aluminum bromide, iron chloride (III), iron bromide (III), zeolite, silicon dioxide, montmorillonite, aluminum oxide, fluorine resin containing sulfonic acid group, ion exchange resins such as polystyrene resin containing sulfonic acid group, sulfuric acid, hydrochloric acid, acetic acid, phosphoric acid, oxalic acid, nitric acid, p-toluenesulfonic acid, protonic acids such as trifluoroacetic acid, etc. can be used. Among these, it is preferred to use Lewis acids and solid acids that are not prone to side reactions and have fast response speed, and from the aspect of the ease of acquisition and high reactivity, various complexes and aluminum chloride of boron trifluoride are more preferred.

[0548] The weight average molecular weight of the petroleum resin is not particularly limited, but is preferably 500 to 10,000, and more preferably 500 to 5,000. By setting it below the upper limit, it tends to be compatible with other resins and to have higher solubility in solvents. By setting it above the lower limit, the heat resistance and mechanical strength of the obtained cured product tend to be further improved.

[0549] The softening point of the petroleum resin is not particularly limited, but is preferably higher, preferably 80° C. or higher, and more preferably 100° C. or higher. When the softening point is equal to or higher than the above lower limit, the heat resistance of the obtained cured product tends to be improved.

[0550] Examples of the petroleum resin include aliphatic petroleum resins, aromatic petroleum resins, copolymer petroleum resins, and dicyclopentadiene petroleum resins, and dicyclopentadiene petroleum resins are preferred.

[0551] Examples of the dicyclopentadiene petroleum resin include resins obtained by polymerizing dicyclopentadiene fractions such as dicyclopentadiene, isopropenylnorbornene, dimethyldicyclopentadiene, and tricyclopentadiene; and resins obtained by polymerizing dicyclopentadiene fractions with other monomers having an unsaturated bond, preferably unsaturated cyclic olefins.

[0552] Examples of the unsaturated cyclic olefins include cyclopentadiene; norbornene monomers such as 2-norbornene, 5-methyl-2-norbornene, 5-ethylidene-2-norbornene, 5-phenylnorbornene, 5-propenyl-2-norbornene, and 5-ethylidene-2-norbornene; and tricyclic or higher norbornene monomers such as diethyldicyclopentadiene, dihydrodicyclopentadiene, and other tricyclic monomers excluding dicyclopentadiene fractions, tetracyclic monomers such as tetracyclododecene, pentacyclic monomers such as tricyclopentadiene, heptacyclic monomers such as tetracyclopentadiene, and alkyl-substituted, alkylidene-substituted, and aryl-substituted products of these polycyclic monomers. As the alkyl substitution body of the above-mentioned polycyclic body, for example, methyl, ethyl, propyl, butyl substitution body and the like can be listed. In addition, as the alkylidene substitution body of the above-mentioned polycyclic body, for example, ethylidene substitution body and the like can be listed. Furthermore, as the aryl substitution body of the above-mentioned polycyclic body, for example, phenyl, tolyl, naphthyl substitution body and the like can be listed.

[0553] Furthermore, as monomers having an unsaturated bond other than unsaturated cyclic olefins, olefins having 3 to 12 carbon atoms may be copolymerized, for example, α-olefins such as propylene, butene-1, pentene-1, 1,3-pentadiene, hexene-1, heptene-1, octene-1, diisobutylene, nonene-1, decene-1, 4-phenylbutene-1, 6-phenylhexene-1, 3-methylbutene-1, 4-methylpentene-1, 3-methylpentene-1, 3-methylhexene-1, 4-methylhexene-1, 5-methylhexene-1, 3,3-dimethylpentene-1, 3,4-dimethylpentene-1, 4,4-dimethylpentene-1, vinylcyclohexane, and vinylcyclohexene; and halogen-substituted α-olefins such as hexafluoropropylene, 2-fluoropropylene, 3-fluoropropylene, and 3,4-dichlorobutene-1.

[0554] Examples of monomers having unsaturated bonds other than the above monomers include ethylene, tetrafluoroethylene, vinyl fluoride, vinylidene fluoride, and trifluoroethylene; alkyl styrenes such as styrene, p-methylstyrene, o-methylstyrene, m-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, and p-tert-butylstyrene; halogenated styrenes such as p-chlorostyrene, m-chlorostyrene, o-chlorostyrene, p-bromostyrene, m-bromostyrene, o-bromostyrene, p-fluorostyrene, m-fluorostyrene, o-fluorostyrene, and o-methyl-p-fluorostyrene; maleic anhydride, maleic acid, fumaric acid, allyl alcohol, 3-butene-2-ol, methylbutene-1-ol, vinyl acetate, and vinyl chloride.

[0555] The above-mentioned monomers may be used alone or in combination of two or more.

[0556] As the petroleum resin, commercially available products can be used as appropriate. Examples of the aliphatic petroleum resin include Quintone A100, Quintone B170, Quintone K100, Quintone M100, Quintone R100, and Quintone C200S manufactured by Nippon Zeon Co., Ltd., and MARUKAREZ T-100AS and MARUKAREZ R-100AS manufactured by Maruzen Petrochemical Co., Ltd.; and examples of the aromatic petroleum resin include Neopolymer L-90, Neopolymer 120, Neopolymer 130, Neopolymer 140, Neopolymer 150, Neopolymer 170S, Neopolymer 160, Neopolymer E-100, Neopolymer E-130, Neopolymer 130S, and Neopolymer S manufactured by JXTG Energy Corporation, and Petcoal LX, Petcoal LX-HS, and Petcoal Examples of the copolymer petroleum resin include Quintone D100, Quintone N180, Quintone P195N, Quintone S100, Quintone S195, Quintone U185, Quintone G100B, Quintone G115, Quintone D200, Quintone E200SN, Quintone N295 manufactured by Nippon Zeon Co., Ltd., and Petrotack 60, Petrotack 70, Petrotack 90, Petrotack 90V, Petrotack 100, Petrotack 100V, Petrotack 90HM. DCPD (dicyclopentadiene)-based petroleum resins include MARUKAREZ M-890A and MARUKAREZ M-845A manufactured by Maruzen Petrochemical Co., Ltd., Quintone 1325, Quintone 1345, Quintone 1500, Quintone 1525L, and Quintone 1700 manufactured by Nippon Zeon Co., Ltd., and HA085, HA103, HA105, HA125, HB103, and HB125 manufactured by ENEOS Corporation.

[0557] In addition, as the petroleum resin, resins described in Synthetic Organic Chemistry, Vol. 25, No. 6 (1967) can also be used.

[0558] When the resin combination of the present embodiment includes petroleum resin, the lower limit of its content is preferably more than 1 mass part relative to 100 mass parts of the resin solids in the resin combination, more preferably more than 5 mass parts, further preferably more than 10 mass parts, more preferably more than 20 mass parts, more preferably more than 25 mass parts.By being set to more than the aforementioned lower limit, there is a tendency that melt viscosity reduces.In addition, the upper limit of the content of petroleum resin is preferably less than 70 mass parts relative to 100 mass parts of the resin solids in the resin combination, more preferably less than 50 mass parts, and also can be less than 40 mass parts.By being set to less than the aforementioned upper limit, there is a tendency that Df reduces.

[0559] The resin composition in the present embodiment may contain only one petroleum resin or two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0560] In addition, the resin composition in the present embodiment may be configured to contain substantially no petroleum resin. Substantially containing no petroleum resin means that the content of petroleum resin is less than 1 part by mass, preferably less than 0.1 part by mass, and more preferably less than 0.01 part by mass, relative to 100 parts by mass of the resin solid content in the resin composition.

[0561] <Filling material (D)>

[0562] The resin composition of this embodiment preferably contains a filler (D). By containing a filler (D), the physical properties such as low dielectric properties (Dk and / or Df), flame resistance, and low thermal expansion of the resin composition and its cured product can be further improved.

[0563] In addition, the filler material (D) used in the present embodiment is more preferably excellent in low dielectric properties (Dk and / or Df). For example, the relative dielectric constant (Dk) of the filler material (D) used in the present embodiment at 10 GHz measured by the cavity resonator perturbation method is preferably 8.0 or less, more preferably 6.0 or less, and further preferably 4.0 or less. In addition, the lower limit of the relative dielectric constant is, for example, 2.0 or more, which is practical. In addition, the dielectric loss tangent (Df) at 10 GHz measured by the cavity resonator perturbation method of the filler material (D) used in the present embodiment is preferably 0.05 or less, and more preferably 0.01 or less. In addition, the lower limit of the dielectric loss tangent is, for example, 0.0001 or more, which is practical.

[0564] The filler (D) used in the present embodiment is not particularly limited in type, and fillers commonly used in the technical field can be suitably used. Specifically, natural silica, fused silica, synthetic silica, amorphous silica, AEROSIL, hollow silica and other silicas; metal oxides such as aluminum oxide, white carbon, titanium dioxide, titanium oxide, zinc oxide, magnesium oxide, zirconium oxide and other metal oxides; composite oxides such as zinc borate, zinc stannate, forsterite, barium titanate, strontium titanate, calcium titanate and other metal oxides; nitrides such as boron nitride, aggregated boron nitride, silicon nitride, aluminum nitride and other metal hydroxides (including hydrates) such as aluminum hydroxide, aluminum hydroxide heat-treated product (a material obtained by heating aluminum hydroxide and reducing a portion of crystal water), boehmite, magnesium hydroxide and other metal hydroxides; molybdenum oxide, Molybdenum compounds such as zinc molybdate; inorganic fillers such as barium sulfate, clay, kaolin, talc, calcined clay, calcined kaolin, calcined talc, mica, E-glass, A-glass, NE-glass, NER-glass, C-glass, L-glass, D-glass, S-glass, M-glass G20, short glass fibers (including glass micropowders such as E glass, T glass, D glass, S glass, Q glass, etc.), hollow glass, spherical glass; and organic fillers such as styrene-type, butadiene-type, acrylic-type rubber powders, core-shell rubber powders, silicone resin powders, silicone rubber powders, silicone composite powders, etc.

[0565] In the present embodiment, preferably inorganic filling material, more preferably including more than one selected from the group consisting of silicon dioxide, aluminum hydroxide, aluminum nitride, boron nitride, forsterite, titanium oxide, barium titanate, strontium titanate and calcium titanate, from the viewpoint of low dielectric properties (Dk and / or Df), more preferably including more than one selected from the group consisting of silicon dioxide and aluminum hydroxide, further preferably including silicon dioxide. By using these inorganic filling materials, the heat resistance of the cured product of resin combination, low dielectric properties (Dk and / or Df), thermal expansion characteristics, dimensional stability, flame retardancy and other characteristics are further improved.

[0566] The content of the filler (D) in the resin combination of the present embodiment can be appropriately set according to desired characteristics, is not particularly limited, and is preferably more than 10 mass parts relative to 100 mass parts of the resin solids in the resin combination, more preferably more than 20 mass parts, more preferably more than 40 mass parts, more preferably more than 60 mass parts, more preferably more than 80 mass parts.By being set to more than the aforementioned lower limit, so that the heat resistance, low thermal expansion, and low dielectric loss tangent of the cured product obtained are further improved.In addition, the upper limit of the content of the filler (D) is preferably less than 1000 mass parts relative to 100 mass parts of resin solids, more preferably less than 500 mass parts, more preferably less than 300 mass parts, more preferably less than 250 mass parts, and can also be less than 200 mass parts, less than 120 mass parts.By being set to less than the aforementioned upper limit, so that the formability of the resin combination is further improved.

[0567] In the resin composition of the present embodiment, as an example of a preferred embodiment, there can be illustrated an embodiment in which the content of the filler (D) is 30% by mass to 90% by mass of the components excluding the solvent.

[0568] The resin composition of the present embodiment may contain only one filler (D) or two or more fillers. When containing two or more fillers, the total amount is preferably within the above range.

[0569] In the resin composition of the present embodiment, when a filler (D), especially an inorganic filler, is used, a silane coupling agent may be further included. By including a silane coupling agent, there is a tendency to further improve the dispersibility of the filler (D) and the bonding strength between the resin component and the filler (D) and the substrate described later.

[0570] The silane coupling agent is not particularly limited, and examples thereof include silane coupling agents commonly used in surface treatment of inorganic substances, such as aminosilane compounds (e.g., γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, etc.), epoxysilane compounds (e.g., γ-glycidoxypropyltrimethoxysilane, etc.), vinylsilane compounds (e.g., vinyltrimethoxysilane, etc.), styrylsilane compounds, acrylic silane compounds (e.g., γ-acryloxypropyltrimethoxysilane, etc.), cationic silane compounds (e.g., N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane hydrochloride, etc.), and phenylsilane compounds. The silane coupling agent may be used alone or in combination of two or more.

[0571] The content of the silane coupling agent is not particularly limited, but may be 0.1 to 5.0 parts by mass based on 100 parts by mass of the resin solid content.

[0572] <Monomer or oligomer having ethylenically unsaturated groups>

[0573] In the resin composition of the present embodiment, in order to improve the thermosetting property and the curing property based on active energy rays (for example, the photocuring property based on ultraviolet rays, etc.), a monomer or oligomer having an ethylenically unsaturated group may also be used in combination. The oligomer or monomer having an ethylenically unsaturated group used in the present embodiment is not particularly limited as long as it is an oligomer or monomer having one or more ethylenically unsaturated groups in one molecule, and for example, monomers or oligomers having vinyl, isopropenyl, allyl, (meth)acryloyl, etc. may be cited, preferably monomers or oligomers having vinyl.

[0574] In addition, in this specification, the compound which is a compound which is a monomer or oligomer which has an ethylenically unsaturated group and which also belongs to a polyphenylene ether compound (B) is regarded as a polyphenylene ether compound (B).

[0575] More specifically, examples of the monomer having an ethylenically unsaturated group include compounds (F1) having a molecular weight of less than 1,000 and containing one organic group having an ethylenically unsaturated bond in the molecule (compound (F1)).

[0576] The ethylenic unsaturated bonds constituting the aforementioned organic groups containing ethylenic unsaturated bonds do not include ethylenic unsaturated bonds contained as part of an aromatic ring. On the other hand, ethylenic unsaturated bonds contained as part of a non-aromatic ring are included. Examples of ethylenic unsaturated bonds contained as part of a non-aromatic ring include cyclohexenyl in a molecule, etc. In addition, the portion other than the end of a straight or branched organic group, i.e., the ethylenic unsaturated bonds contained in a straight or branched chain, are also included.

[0577] The organic group containing an ethylenically unsaturated bond is more preferably one selected from the group consisting of a vinyl group, an isopropenyl group, an allyl group, an acryloyl group, and a methacrylic group, and is still more preferably a vinyl group.

[0578] In addition, in this specification, a compound which is a monomer or oligomer having an ethylenically unsaturated group and is also a silane coupling agent is regarded as a silane coupling agent.

[0579] In addition, the compound (F1) used in this embodiment is preferably composed only of atoms selected from carbon atoms, hydrogen atoms, oxygen atoms, nitrogen atoms and silicon atoms, more preferably composed only of atoms selected from carbon atoms, hydrogen atoms, oxygen atoms and silicon atoms, and further preferably composed only of atoms selected from carbon atoms, hydrogen atoms, oxygen atoms and oxygen atoms.

[0580] The compound (F1) used in this embodiment may or may not have a polar group. The compound (F1) used in this embodiment preferably has no polar group. Examples of the polar group include an amino group, a carboxyl group, a hydroxyl group, and a nitro group.

[0581] In the present embodiment, the molecular weight of the compound (F1) is preferably 70 or more, more preferably 80 or more, and further preferably 90 or more. By setting it to be above the aforementioned lower limit, there is a tendency to suppress the volatilization of the compound (F1) from the resin composition of the present embodiment, its cured product, etc. The upper limit of the molecular weight of the aforementioned compound (F1) is preferably 500 or less, more preferably 400 or less, further preferably 300 or less, further preferably 200 or less, and may be 150 or less. By setting it to be below the aforementioned upper limit, there is a tendency to further improve the effect of improving the reactivity with other resin components.

[0582] When the resin composition of the present embodiment contains two or more compounds (F1), the average molecular weight value of the compound (F1) is preferably within the above range, and the molecular weight of each compound is more preferably within the above preferred range.

[0583] In the present embodiment, the compound (F1) preferably has a boiling point of 110°C or more, more preferably 115°C or more, and further preferably 120°C or more. By setting it to be above the aforementioned lower limit, the volatilization of the compound (F1) during the thermal curing of the resin composition can be suppressed, and the other compound (C) and the compound (F1) can be reacted. The boiling point of the aforementioned compound (F1) is preferably 300°C or less, more preferably 250°C or less, and further preferably 200°C or less. By setting it to be below the aforementioned upper limit, it can be made less likely to remain in the cured product as a residual solvent.

[0584] When the resin composition of the present embodiment contains two or more compounds (F1), the average value of the boiling points may fall within the above range, and the boiling point of each compound is preferably within the above preferred range.

[0585] Examples of the compound (F1) include (meth)acrylate compounds, aromatic vinyl compounds (preferably styrene compounds), isopropenyl-containing compounds, saturated fatty acid vinyl ester compounds, vinyl cyanide compounds, ethylenically unsaturated carboxylic acids, ethylenically unsaturated carboxylic acid anhydrides, ethylenically unsaturated dicarboxylic acid monoalkyl esters, ethylenically unsaturated carboxylic acid amides, maleic anhydride, and unsaturated polyester compounds based on fumaric acid, itaconic acid and citraconic acid; unsaturated epoxy (meth)acrylate compounds containing an acryloyl group or a methacryloyl group; and unsaturated epoxy (meth)acrylate compounds containing a vinyl group or a (meth) Allyl unsaturated epoxy compounds, carbamate (meth) acrylate compounds, polyether (meth) acrylate compounds; polyol (meth) acrylate compounds, alkyd acrylate compounds, polyester acrylate compounds, spiroacetal acrylate compounds, diallyl phthalate compounds, diallyl tetrabromophthalate compounds, diethylene glycol bisallyl carbonate and polyethylene polythiol, etc., preferably at least one selected from the group consisting of (meth) acrylate compounds, aromatic vinyl compounds and saturated fatty acid vinyl ester compounds. More preferably, it is an aromatic vinyl compound.

[0586] Specific examples of compound (F1) include methylstyrene (e.g., 4-methylstyrene), ethylvinylbenzene, diethyl 4-vinylbenzylphosphonate, 4-vinylbenzyl glycidyl ether, α-methylstyrene, etc. In addition, as specific examples of compound (F1), reference may be made to paragraphs 0046 and 0049 of Japanese Patent Application Publication No. 2019-194312, the contents of which are incorporated into this specification.

[0587] On the other hand, in order to improve the low dielectric constant and low dielectric loss tangent, the resin composition of the present embodiment also preferably contains a styrene oligomer (F2). The styrene oligomer (F2) of the present embodiment is preferably polymerized by at least one selected from the group consisting of styrene and the above-mentioned styrene derivatives and vinyl toluene. The number average molecular weight of the styrene oligomer (F2) is preferably above 178, and is preferably below 1600. In addition, the styrene oligomer (F2) is preferably a compound having an average number of aromatic rings of 2 to 14, a total amount of 2 to 14 aromatic rings of 50% by mass or more, a boiling point of 300°C or more, and no branched structure.

[0588] As the styrene oligomer (F2) used in the present embodiment, for example, styrene polymers, vinyl toluene polymers, α-methyl styrene polymers, vinyl toluene-α-methyl styrene polymers, styrene-α-styrene polymers, etc. can be listed. As styrene polymers, commercially available products can be used, for example, Piccolastic A5 (Eastman Chemical Co., Ltd.), Piccolastic A-75 (Eastman Chemical Co., Ltd.), Piccotex 75 (Eastman Chemical Co., Ltd.), FTR-8100 (Mitsui Chemicals, Inc.), FTR-8120 (Mitsui Chemicals, Inc.) can be listed. In addition, as vinyl toluene-α-methyl styrene polymers, Piccotex LC (Eastman Chemical Co., Ltd.) can be listed. In addition, examples of α-methylstyrene polymers include Kristalex 3070 (manufactured by Eastman Chemical Co., Ltd.), Kristalex 3085 (manufactured by Eastman Chemical Co., Ltd.), Kristalex (3100), Kristalex 5140 (manufactured by Eastman Chemical Co., Ltd.), FMR-0100 (manufactured by Mitsui Chemicals, Inc.), and FMR-0150 (manufactured by Mitsui Chemicals, Inc.). In addition, examples of styrene-α-styrene polymers include FTR-2120 (manufactured by Mitsui Chemicals, Inc.). These styrene oligomers may be used alone or in combination of two or more.

[0589] Among the resin compositions of the present embodiment, α-methylstyrene oligomers are preferred because they are well thermally cured, have good embedding properties for fine wiring, and are excellent in solder heat resistance, low relative dielectric constant, and low dielectric loss tangent.

[0590] In order to improve low dielectric constant and low dielectric loss tangent, the resin composition of the present embodiment preferably further contains a divinyl compound (F3) as a monomer having an ethylenically unsaturated group.

[0591] Divinyl compound is a low molecular compound with 2 vinyl groups. By making vinyl group 2, thus becoming a good cross-linking density of the degree that will not be too high, as a result, the free volume of molecule becomes large, therefore the dielectric loss tangent (Df) of the cured product obtained can be suppressed to be less. And then it can be considered that divinyl compound (F3) is used as a replacement of a part of resin (A) and polyphenylene oxide compound (B) and other compounds (C), therefore the content reduction of the composition with polar groups itself also contributes to the reduction of dielectric loss tangent (Df). In addition, it can be considered that by making 2 functional groups possessed by divinyl compound be vinyl, thus becoming good with the reactivity of resin (A) and polyphenylene oxide compound (B), as a result, there is a tendency that heat resistance is easily improved.

[0592] It should be noted that the divinyl compound (F3) herein refers to a compound having a molecular weight of less than 600, preferably less than 300, and more preferably less than 195. In addition, the lower limit of the molecular weight is practically 54. Examples of the divinyl compound (F3) include divinylbenzene, 1-ethynyl-4-[2-(4-ethynylphenyl)ethyl]benzene (BVPE), and 1,3-vinyltetramethylsiloxane.

[0593] Moreover, as the monomer or oligomer having an ethylenically unsaturated group, 1,3-diisopropenylbenzene and 1,4-diisopropenylbenzene are also preferably used.

[0594] In addition, for details of the monomer or oligomer having an ethylenically unsaturated group, reference can be made to the description in paragraphs 0069 to 0087 of International Publication No. 2017 / 135168 and paragraphs 0065 to 0067 of International Publication No. 2019 / 230945, the contents of which are incorporated into the present specification.

[0595] In the case where the resin combination of the present embodiment includes a monomer or oligomer with an ethylenically unsaturated group, its content is preferably more than 0.5 mass parts relative to 100 mass parts of the resin solids in the resin combination, more preferably more than 1 mass part, more preferably more than 2 mass parts, more preferably more than 3 mass parts, and then can also be more than 5 mass parts. By being set to more than the aforementioned lower limit, there is a tendency for the low dielectric properties (Dk and / or Df) of the cured product obtained to be further improved. In addition, the upper limit of the content of the monomer or oligomer with an ethylenically unsaturated group is preferably less than 30 mass parts relative to 100 mass parts of the resin solids in the resin combination, more preferably less than 25 mass parts, more preferably less than 20 mass parts, more preferably less than 15 mass parts, and more preferably less than 10 mass parts. By being set to less than the aforementioned upper limit, there is a tendency for the heat resistance of the cured product obtained to be further improved. In addition, there is a tendency for low dielectric constant, low dielectric loss tangent and chemical resistance to be further improved.

[0596] The resin composition of the present embodiment may contain only one monomer or oligomer having an ethylenically unsaturated group, or may contain two or more. When containing two or more monomers or oligomers, the total amount is preferably within the above range.

[0597] <Flame retardant>

[0598] The resin composition of the present embodiment may contain a flame retardant. Examples of the flame retardant include phosphorus-based flame retardants, halogen-based flame retardants, inorganic-based flame retardants, and silicone-based flame retardants, and phosphorus-based flame retardants are preferred.

[0599] As the flame retardant, known flame retardants can be used, for example, brominated epoxy resin, brominated polycarbonate, brominated polystyrene, brominated styrene, brominated phthalimide, tetrabromobisphenol A, pentabromobenzyl (meth)acrylate, pentabromotoluene, tribromophenol, hexabromobenzene, decabromodiphenyl ether, bis-1,2-pentabromophenylethane, chlorinated polystyrene, chlorinated paraffin and other halogen flame retardants; red phosphorus, tricresyl phosphate, triphenyl phosphate, toluene diphenyl phosphate, triphenyl phosphate, trimethylol phosphate, triphenyl ... Phosphorus-based flame retardants such as (xylene esters), trialkyl phosphates, dialkyl phosphates, tri(chloroethyl) phosphate, phosphazene, 1,3-phenylenebis(2,6-bis(xylene) phosphate), 10-(2,5-dihydroxyphenyl)-10H-9-oxa-10-phosphaphenanthrene-10-oxide; inorganic flame retardants such as aluminum hydroxide, magnesium hydroxide, some boehmite, boehmite, zinc borate, antimony trioxide; silicone-based flame retardants such as silicone rubber and silicone resin.

[0600] In the present embodiment, among these, 1,3-phenylenebis(2,6-bis(xylyl)phosphate) is preferred because it does not impair the low dielectric properties (Dk and / or Df) of the obtained cured product.

[0601] When the resin composition of the present embodiment includes a flame retardant, its content is preferably 1 mass part or more, more preferably 5 mass parts or more relative to 100 mass parts of the resin solid content in the resin composition. In addition, the lower limit of the content of the aforementioned flame retardant is preferably 30 mass parts or less, more preferably 25 mass parts or less.

[0602] The flame retardant may be used alone or in combination of two or more. When two or more flame retardants are used, the total amount is within the above range.

[0603] <Active ester compound>

[0604] The resin composition of the present embodiment may contain an active ester compound. The active ester compound is not particularly limited, and for example, reference may be made to the description in paragraphs 0064 to 0066 of International Publication No. 2021 / 172317, the contents of which are incorporated into this specification.

[0605] When the resin composition of the present embodiment contains an active ester compound, the amount thereof is preferably 1 part by mass or more, and is preferably 90 parts by mass or less, and may be 50 parts by mass or less, based on 100 parts by mass of the resin solid content in the resin composition.

[0606] The resin composition in the present embodiment may contain only one active ester compound or two or more thereof. When containing two or more thereof, the total amount is preferably within the above range.

[0607] In addition, the resin composition in the present embodiment may also be configured to contain substantially no active ester compound. Substantially containing no active ester compound means that the content of the active ester compound is less than 1 part by mass, preferably less than 0.1 part by mass, and more preferably less than 0.01 part by mass, relative to 100 parts by mass of the resin solid content in the resin composition.

[0608] <Dispersant>

[0609] The resin composition of the present embodiment may also contain a dispersant. As the dispersant, a dispersant commonly used for coating applications can be suitably used, and its type is not particularly limited. The dispersant is preferably a wetting dispersant for the copolymer matrix or a fluorine-containing fluorine-based dispersant.

[0610] Specific examples of the dispersant include DISPERBYK (registered trademark)-110, 111, 161, 180, 2009, 2152, 2155, BYK (registered trademark)-W996, W9010, W903, and W940 manufactured by BYK Japan Co., Ltd., Ftergent manufactured by NEOS Co., Ltd., and MPT manufactured by Mitsubishi Pencil Co., Ltd.

[0611] When the resin composition of the present embodiment includes a dispersant, the lower limit of its content is preferably 0.01 mass parts or more, more preferably 0.1 mass parts or more, or 0.3 mass parts or more relative to 100 mass parts of the resin solid components in the resin composition. In addition, the upper limit of the content of the dispersant is preferably 10 mass parts or less, more preferably 5 mass parts or less, and further preferably 3 mass parts or less relative to 100 mass parts of the resin solid components in the resin composition.

[0612] The dispersants may be used alone or in combination of two or more. When two or more are used, the total amount is within the above range.

[0613] <Curing Accelerator>

[0614] The resin composition of the present embodiment may further include a curing accelerator. The curing accelerator is not particularly limited, and examples thereof include imidazoles such as 2-ethyl-4-methylimidazole and triphenylimidazole; organic peroxides such as benzoyl peroxide, bis(1-methyl-1-phenylethyl)peroxide, di-tert-butyl peroxide, lauroyl peroxide, acetyl peroxide, p-chlorobenzoyl peroxide, di-tert-butyl peroxyphthalate, α,α'-di(tert-butylperoxy)diisopropylbenzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexyne-3; azo compounds such as azobisisobutyronitrile; N,N-dimethylbenzylamine, N,N-dimethylaniline, N,N-dimethyltoluidine, 2 -N-ethylanilinoethanol, tri-n-butylamine, pyridine, quinoline, N-methylmorpholine, triethanolamine, triethylenediamine, tetramethylbutylenediamine, N-methylpiperidine and other tertiary amines; phenols such as phenol, xylenol, cresol, resorcinol, catechol and other phenols; pyrolysis-type free radical generators such as 2,3-dimethyl-2,3-diphenylbutane; organic metal salts such as lead naphthenate, lead stearate, zinc naphthenate, zinc octoate, manganese octoate, tin oleate, dibutyltin maleate, manganese naphthenate, cobalt naphthenate, ferric acetylacetonate, etc.; substances obtained by dissolving these organic metal salts in hydroxyl-containing compounds such as phenol and bisphenol; inorganic metal salts such as tin chloride, zinc chloride, aluminum chloride; organic tin compounds such as dioctyltin oxide, other alkyl tins, alkyl tin oxides, etc.

[0615] The curing accelerator is preferably at least one selected from the group consisting of imidazoles, organic peroxides, and organic metal salts, more preferably at least one selected from the group consisting of imidazoles and organic metal salts, and still more preferably imidazoles.

[0616] In addition, in the present embodiment, the composition may be such that the polymerization initiator such as organic peroxide or azo compound is substantially not included. Substantially not included means that the content of the polymerization initiator is less than 0.1 parts by mass, preferably less than 0.01 parts by mass, and more preferably less than 0.001 parts by mass, relative to 100 parts by mass of the resin solid content in the resin composition.

[0617] In particular, when a polyphenylene ether compound represented by formula (OP-1) is used as the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond, sufficient curing can be achieved even in a configuration that substantially contains no polymerization initiator (including a curing accelerator).

[0618] When the resin combination of the present embodiment includes a curing accelerator, the lower limit of its content is preferably 0.005 mass parts or more relative to 100 mass parts of the resin solids in the resin combination, more preferably 0.01 mass parts or more, and further preferably 0.1 mass parts or more. In addition, the upper limit of the content of the curing accelerator is preferably 10 mass parts or less relative to 100 mass parts of the resin solids in the resin combination, more preferably 5 mass parts or less, and further preferably 2 mass parts or less.

[0619] The curing accelerator may be used alone or in combination of two or more. When two or more are used, the total amount is within the above range.

[0620] <Solvent>

[0621] The resin combination of the present embodiment can contain a solvent, preferably an organic solvent. When containing a solvent, the resin combination of the present embodiment is at least a portion of the above-mentioned various resin solid components, preferably all dissolved or compatible with the form (solution or varnish) of the solvent. As a solvent, as long as it is a polar organic solvent or a non-polar organic solvent that can make at least a portion of the above-mentioned various resin solid components, preferably all dissolved or compatible, there is no particular limitation, as a polar organic solvent, for example, ketones (such as acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.), cellosolves (such as propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, etc.), esters (such as ethyl lactate, methyl acetate, ethyl acetate, butyl acetate, isoamyl acetate, ethyl lactate, methyl methoxypropionate, methyl hydroxyisobutyrate, etc.), amides (such as dimethoxyacetamide, dimethylformamide, etc.), as a non-polar organic solvent, aromatic hydrocarbons (such as toluene, xylene, etc.) can be listed.

[0622] The solvent may be used alone or in combination of two or more. When two or more solvents are used, the total amount is within the above range.

[0623] <Other ingredients>

[0624] The resin composition of the present embodiment may contain various polymer compounds and various additives such as resin and oligomer thereof in addition to the above-mentioned components. As additives, ultraviolet light absorbers, antioxidants, photopolymerization initiators, fluorescent whitening agents, photosensitizers, dyes, pigments, thickeners, flow regulators, lubricants, defoamers, leveling agents, brighteners, polymerization inhibitors, etc. These additives may be used alone or in combination of two or more.

[0625] In addition, the resin composition in the present embodiment may also be configured to be substantially free of polymerization inhibitors. Substantially free of polymerization inhibitors means that the resin composition does not contain a polymerization inhibitor, or the content of the polymerization inhibitor in the resin composition is, for example, less than 0.008 mass parts relative to 100 mass parts of the resin solids, preferably less than 0.007 mass parts, more preferably less than 0.001 mass parts, and even more preferably less than 0.0001 mass parts.

[0626] <Purpose>

[0627] The resin composition of the present embodiment can be used in the form of a cured product. Specifically, the resin composition of the present embodiment can be used as a material with low dielectric properties (Dk and / or Df) and is suitably used as an insulating layer of a printed circuit board, a semiconductor package material and other electronic material resin composition. The resin composition of the present embodiment can be suitably used as a prepreg, a metal foil laminated plate using a prepreg, a resin composite sheet and a printed circuit board material.

[0628] The resin composition of this embodiment preferably has a minimum melt viscosity of 100,000 Pa·s or less, and more preferably 20,000 Pa·s or less. The lower limit of the minimum melt viscosity is not particularly limited, and it is practical to be 10 Pa·s or more. Such a low melt viscosity can be achieved by using a resin (A) and a polymer having a structural unit represented by formula (V).

[0629] In addition, the resin composition of the present embodiment preferably has a viscosity of (minimum melting temperature + 10°C) ÷ minimum melting viscosity of 80 times or less, and more preferably 20 times or less. When the viscosity of (minimum melting temperature + 10°C) ÷ minimum melting viscosity is low, there is a tendency that the curing reaction proceeds gently and the formation of voids can be effectively suppressed.

[0630] The minimum melt viscosity is measured by the method described in the examples described later.

[0631] The lowest melting temperature of the resin composition of the present embodiment is preferably 210° C. or lower, more preferably 200° C. or lower, further preferably 190° C. or lower, further preferably 180° C. or lower, further preferably 175° C. or lower. It is practical that the lower limit is, for example, 120° C. or higher.

[0632] The minimum melting temperature is measured by the method described in Examples below.

[0633] The resin composition of the present embodiment preferably has a glass transition temperature of 130°C or higher, more preferably 150°C or higher, further preferably 165°C or higher, further preferably 175°C or higher, and may also be 180°C or higher or 190°C or higher, as determined by DMA (dynamic mechanical analysis) of its cured product.

[0634] Such a high glass transition temperature is achieved mainly by using the polyphenylene ether compound (B). It is practical that the upper limit of the glass transition temperature is, for example, 350° C. or less.

[0635] The glass transition temperature is measured by the method described in Examples below.

[0636] The resin composition of the present embodiment preferably has a low relative dielectric constant (Dk) of its cured product. Specifically, the relative dielectric constant (Dk) at a frequency of 10 GHz measured by the cavity resonator perturbation method is preferably 2.50 or less, more preferably less than 2.45, and further preferably less than 2.44. There is no particular limitation on the lower limit of the relative dielectric constant (Dk), and for example, 0.01 or more is practical.

[0637] In addition, the dielectric loss tangent (Df) of the resin composition of the present embodiment is preferably low for its cured product. Specifically, the dielectric loss tangent (Df) at a frequency of 10GHz measured according to the cavity resonator perturbation method is preferably less than 0.0022, more preferably less than 0.0021, further preferably less than 0.0020, and may be less than 0.0018, less than 0.0015, less than 0.0014, less than 0.0013. About the lower limit of dielectric loss tangent (Df), it is not particularly limited, for example, it is practical to be more than 0.0001.

[0638] Such low dielectric properties can be achieved mainly by using the resin (A) and a polymer having a structural unit represented by the formula (V).

[0639] The relative dielectric constant (Dk) and the dielectric loss tangent (Df) were measured by the method described in the examples described later.

[0640] The resin composition of the present embodiment can be used as a prepreg, a resin composite sheet or other layered material (including a film, a sheet, etc.) that becomes the insulating layer of a printed circuit board. When making the layered material, the thickness is preferably 5 μm or more, and more preferably 10 μm or more. As the upper limit of the thickness, it is preferably 200 μm or less, and more preferably 180 μm or less. It should be noted that the thickness of the above-mentioned layered material, for example, when the resin composition of the present embodiment is impregnated in glass cloth, refers to the thickness including the glass cloth.

[0641] The material formed from the resin composition of the present embodiment may be used for applications where a pattern is formed by exposure and development, or may be used for applications where exposure and development are not performed. The material is particularly suitable for applications where exposure and development are not performed.

[0642] <<Prepreg>>

[0643] The prepreg of the present embodiment is formed by a substrate (prepreg substrate) and a resin composition of the present embodiment. The prepreg of the present embodiment can be obtained, for example, by applying (e.g., impregnating and / or coating) the resin composition of the present embodiment to the substrate, and semi-curing it by heating (e.g., a method of drying at 120 to 220°C for 2 to 15 minutes, etc.). At this time, the amount of the resin composition attached to the substrate, that is, the amount of the resin composition relative to the total amount of the semi-cured prepreg (including the filler (D)) is preferably in the range of 20 to 99% by mass, more preferably in the range of 20 to 80% by mass.

[0644] The substrate is not particularly limited as long as it is a substrate used for various printed circuit board materials. As the material of the substrate, for example, glass fiber (such as E-glass, D-glass, L-glass, S-glass, T-glass, Q-glass, UN-glass, NE-glass, NER-glass, spherical glass, etc.), inorganic fibers other than glass (such as quartz, etc.), organic fibers (such as polyimide, polyamide, polyester, liquid crystal polyester, polytetrafluoroethylene, etc.) can be listed. The form of the substrate is not particularly limited, and woven fabrics, non-woven fabrics, coarse yarns, short glass fiber mats, surface mats, etc. can be listed. These substrates can be used alone or in combination of two or more. Among these substrates, from the viewpoint of dimensional stability, woven fabrics that have been subjected to super fiber opening treatment and caulking treatment are preferred. From the viewpoint of strength and low water absorption, the substrate is preferably 200 μm or less in thickness and 250 g / m in mass. 2 The following glass woven fabrics are preferably glass woven fabrics that have been surface treated with a silane coupling agent such as epoxysilane or aminosilane from the viewpoint of moisture absorption and heat resistance. From the viewpoint of electrical properties, low dielectric glass fabrics formed of glass fibers having low relative dielectric constants and low dielectric loss tangents such as L-glass, NE-glass, NER-glass, and Q-glass are more preferred.

[0645] The substrate with low relative dielectric constant can be exemplified by a substrate with a relative dielectric constant of 5.0 or less (preferably 3.0 to 4.9). The substrate with low dielectric loss tangent can be exemplified by a substrate with a dielectric loss tangent of 0.006 or less (preferably 0.001 to 0.005). The relative dielectric constant and dielectric loss tangent are values ​​measured using a perturbation method cavity resonator at a frequency of 10 GHz.

[0646] <<Metal foil clad laminate>>

[0647] The metal foil clad laminate of the present embodiment comprises: at least one layer formed by the prepreg of the present embodiment, and a metal foil disposed on one or both sides of the layer formed by the aforementioned prepreg. As a method for making the metal foil clad laminate of the present embodiment, for example, the following method can be cited: at least one (preferably overlapping two or more) prepreg of the present embodiment is disposed, and a metal foil is disposed on one or both sides thereof and laminated. In more detail, it can be made by disposing a metal foil of copper, aluminum, etc. on one or both sides of the prepreg and laminating. As the number of sheets of the prepreg, it is preferably 1 to 10 sheets, more preferably 2 to 10 sheets, and further preferably 2 to 9 sheets. The metal foil is not particularly limited as long as it is a metal foil used for printed circuit board materials, and for example, copper foils such as rolled copper foil and electrolytic copper foil can be cited. The thickness of the metal foil (preferably copper foil) is not particularly limited and can be about 1.5 to 70 μm. When copper foil is used as the metal foil, the roughness Rz of the copper foil surface measured according to JIS B0601:2013 is preferably adjusted to 0.2 to 4.0 μm. By setting the roughness Rz of the copper foil surface to 0.2 μm or more, there is a tendency that the roughness of the copper foil surface becomes a moderate size and the peel strength of the copper foil is further improved. On the other hand, by setting the roughness Rz of the copper foil surface to 4.0 μm or less, there is a tendency that the roughness of the copper foil surface becomes a moderate size and the dielectric loss tangent characteristics are further improved. From the viewpoint of reducing the dielectric loss tangent, the roughness Rz of the copper foil surface is more preferably 0.5 μm or more, more preferably 0.6 μm or more, and particularly preferably 0.7 μm or more. In addition, it is more preferably 3.5 μm or less, more preferably 3.0 μm or less, and particularly preferably 2.0 μm or less.

[0648] As the lamination forming method, there can be cited the method generally used when forming a laminated board or a multilayer board for a printed circuit board. More specifically, there can be cited the method of using a multistage press, a multistage vacuum press, a continuous forming machine, an autoclave forming machine, etc. at a temperature of about 180 to 350° C., a heating time of about 100 to 300 minutes, a surface pressure of 20 to 100 kg / cm 2A method for laminating and forming about. In addition, a multilayer board can also be made by combining the prepreg of the present embodiment with a separately prepared inner layer circuit board and laminating and forming. As a method for making a multilayer board, for example, a copper foil of about 35 μm can be arranged on both sides of a prepreg of the present embodiment, and an inner layer circuit is formed after laminating and forming by the above-mentioned forming method, and the circuit is subjected to blackening treatment to form an inner layer circuit board, and then, the inner layer circuit board and the prepreg of the present embodiment are alternately arranged with one each, and copper foil is further arranged in the outermost layer, and laminating and forming is performed under the above-mentioned conditions, preferably under vacuum, thereby making a multilayer board. The metal foil-clad laminate of the present embodiment can be suitably used as a printed circuit board.

[0649] As described above, the resin composition for electronic materials obtained using the resin composition of the present embodiment (a resin composition comprising a combination of specific components) can have the moldability of the resin composition, the low dielectric properties of its cured product (Dk and / or Df, especially low dielectric loss tangent), as well as low relative dielectric constant, crack resistance, appearance of the cured product, low thermal expansion, and excellent moisture absorption and heat resistance.

[0650] <<Printed Circuit Board>>

[0651] The printed circuit board of the present embodiment comprises an insulating layer and a conductor layer disposed on the surface of the aforementioned insulating layer, wherein the aforementioned insulating layer comprises at least one of a layer formed by the resin composition of the present embodiment and a layer formed by the prepreg of the present embodiment. Such a printed circuit board can be manufactured according to a conventional method, and its manufacturing method is not particularly limited. Below, an example of a method for manufacturing a printed circuit board is shown. First, a metal foil-clad laminate such as the above-mentioned copper-clad laminate is prepared. Next, an etching treatment is applied to the surface of the metal foil-clad laminate, and an inner layer circuit is formed to make an inner layer substrate. On the surface of the inner layer circuit of the inner layer substrate, a surface treatment for improving the bonding strength is performed as needed, and then the required number of prepregs are overlapped on the surface of the inner layer circuit, and the metal foil for the outer layer circuit is further stacked on its outer side, and heated and pressed to form it in one piece. In this way, a multilayer laminate having an insulating layer formed by a cured product of a substrate and a resin composition is manufactured between the metal foil for the inner layer circuit and the outer layer circuit. Then, after the multilayer laminate is subjected to hole opening processing for through holes and conductive holes, a metal-plated coating is formed on the wall surface of the hole to connect the metal foil used for the inner layer circuit and the outer layer circuit, and then the metal foil used for the outer layer circuit is etched to form the outer layer circuit, thereby manufacturing a printed circuit board.

[0652] The printed circuit board obtained in the above manufacturing example has the following structure: it has an insulating layer and a conductor layer formed on the surface of the insulating layer, and the insulating layer contains the resin composition of the present embodiment and / or its cured product. That is, the layer formed by the prepreg of the present embodiment (for example, a prepreg formed by a substrate and the resin composition of the present embodiment impregnated or coated on the substrate) and the resin composition of the metal foil-clad laminate of the present embodiment becomes the insulating layer of the present embodiment.

[0653] In addition, this embodiment also relates to a semiconductor device including the printed circuit board. For details of the semiconductor device, reference can be made to paragraphs 0200 to 0202 of Japanese Patent Application Laid-Open No. 2021-021027, the contents of which are incorporated into this specification.

[0654] In addition, the insulating layer formed by the cured product of the resin composition of the present embodiment preferably reduces the surface roughness of the insulating layer after the roughening treatment. Specifically, the arithmetic mean roughness Ra of the insulating layer surface after the roughening treatment is preferably less than 200nm, more preferably less than 150nm, and particularly preferably less than 100nm. The lower limit of the arithmetic mean roughness Ra is not particularly limited, for example, it can be more than 10nm. The determination of the arithmetic mean roughness Ra on the insulating layer surface uses a non-contact surface roughness meter, and is measured and obtained using a VSI mode and a 50x lens.

[0655] As a non-contact surface roughness meter, WYKONT3300 manufactured by Veeco Instruments Inc. was used.

[0656] <<Resin composite sheet>>

[0657] The resin composite sheet of the present embodiment includes: a support body, and a layer formed by the resin composition of the present embodiment arranged on the surface of the aforementioned support body. The resin composite sheet can be used as a laminated film or a dry film solder resist. There is no particular limitation on the method for manufacturing the resin composite sheet, and for example, a method for obtaining a resin composite sheet by dissolving the resin composition of the present embodiment in a solvent and applying (coating) the solution obtained on the support body and drying it can be cited.

[0658] Examples of the support used herein include polyethylene film, polypropylene film, polycarbonate film, polyethylene terephthalate film, ethylene tetrafluoroethylene copolymer film, release film obtained by coating a release agent on the surface of these films, organic film substrates such as polyimide film, conductor foil such as copper foil and aluminum foil, glass plate, SUS (Steel Use Stainless Steel) plate, FRP (Fiber-Reinforced Plastics) and other plate-shaped supports, without particular limitation.

[0659] As a coating method (coating method), for example, the following method can be cited: using a rod coater, a die coater, a scraper, a Baker coater, etc., the solution obtained by dissolving the resin composition of the present embodiment in a solvent is applied to the support. In addition, the support can be peeled off or etched from the resin composite sheet formed by laminating the support and the resin composition after drying, thereby making a single-layer sheet. It should be noted that the solution obtained by dissolving the resin composition of the present embodiment in a solvent can also be supplied to a mold having a sheet-shaped cavity and dried, thereby forming a sheet without using a support.

[0660] It should be noted that in the preparation of the single-layer sheet or resin composite sheet of the present embodiment, the drying conditions when removing the solvent are not particularly limited. From the perspective that the solvent is likely to remain in the resin composition at low temperatures and the curing of the resin composition is accelerated at high temperatures, it is preferably at a temperature of 20°C to 200°C for 1 to 90 minutes. In addition, the single-layer sheet or resin composite sheet can be used in an uncured state after only the solvent is dried, or it can be used in a semi-cured (B-stage) state as needed. Furthermore, the thickness of the resin layer in the single-layer sheet or resin sheet of the present embodiment can be adjusted by the concentration of the solution of the resin composition of the present embodiment used for coating (applying) and the coating thickness. It is not particularly limited. Generally, if the coating thickness becomes thicker, the solvent becomes easy to remain during drying, so it is preferably 0.1 to 500 μm.

[0661] Example

[0662] The present invention is further specifically described by enumerating examples below. The materials, usage amounts, ratios, processing contents, processing steps etc. shown in the following examples can be appropriately changed as long as they do not depart from the gist of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below.

[0663] When the measuring equipment used in the examples is difficult to obtain due to discontinuation of production or the like, other equipment having equivalent performance may be used for measurement.

[0664] <Determination of Weight Average Molecular Weight and Number Average Molecular Weight>

[0665] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the resin (A) having an indane skeleton and a terminal group represented by formula (T1), the polyphenylene ether compound (B1) having a carbon-carbon unsaturated double bond at the terminal, and the polymer having a structural unit represented by formula (V) were measured by gel permeation chromatography (GPC). A liquid delivery pump (LC-20AD manufactured by Shimadzu Corporation), a differential refractive index detector (RID-10A manufactured by Shimadzu Corporation), and a GPC column (GPC KF-801, 802, 803, 804 manufactured by Showa Denko K.K.) were used, tetrahydrofuran was used as the solvent, the flow rate was 1.0 mL / min, the column temperature was 40°C, and a calibration curve based on monodisperse polystyrene was used.

[0666] <Measurement of parameters α and β>

[0667] The parameters α and β of resin (A) are determined by 1 The synthesized resin was dissolved in a mixed solvent of heptane and methanol and dried to solid. This operation was repeated to remove the residual solvent contained in the recovered solid. Thereafter, the recovered solid was dissolved in CDCl3 and 1 H-NMR measurement. 1 In H-NMR, parameters α and β of each resin were calculated using the formula shown below.

[0668]

[0669]

[0670] (The brackets in formula (α) and formula (β) represent 1 The integral value between corresponding chemical shift values ​​in H-NMR. )

[0671] <Synthesis Example 1 Synthesis of Resin (A) Having a Terminal Group Represented by Formula (T1) and Having an Indane Skeleton>

[0672] In a three-necked flask equipped with a thermometer and a cooling tube, 520 g of toluene, 3 g of activated clay and a stirrer were added, and the mixture was heated to an internal temperature of 70°C while stirring. Thereafter, the dropping rate was controlled so that the internal temperature did not exceed 80°C, and 150 g of 1,3-diisopropenylbenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise. After the addition, the mixture was stirred until the internal temperature dropped to 70°C. Then, 150 g of 1,3-diisopropenylbenzene (manufactured by Tokyo Chemical Industry Co., Ltd.) was added dropwise in the same manner, and the mixture was further reacted for 2 hours after the addition was completed. At the end of the reaction, 433 g of toluene was added, and the activated clay was removed by filtration. The filtrate was distilled under heating and reduced pressure to remove the solvent, thereby obtaining 231 g of solid resin.

[0673] The obtained resin (A) had an Mw of 2674, an Mn of 1153, and an Mw / Mn of 2.3. In the formula (Tx), the parameter α was 0.71, the parameter β was 0.50, and n+o+p was 6.3. The structures in brackets shown in (a), (b), and (c) all had the same molecular weight, and n+o+p was calculated by assuming the Mn of the synthesized resin as the average molecular weight. In addition, the residual monomer was confirmed to be less than 1% by mass by GPC analysis.

[0674] Regarding the obtained resin, Figure 1 An NMR spectrum is shown.

[0675] <Synthesis Example 2 Polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal>

[0676] <<Synthesis of Bifunctional Phenylene Ether Oligomer>>

[0677] In a 12L vertical reactor equipped with a stirring device, a thermometer, an air inlet pipe and a baffle, 9.64g (43.2mmol) of CuBr, 1.86g (10.8mmol) of N,N'-di-tert-butylethylenediamine, 69.83g (690.1mmol) of n-butyldimethylamine and 2600g of toluene were added, and stirred at a reaction temperature of 40°C while a mixed gas of nitrogen and air adjusted to an oxygen concentration of 8% by volume was introduced at a flow rate of 5.2L / min. While bubbling, a mixed solution of 129.3 g (0.48 mol) of 2,2',3,3',5,5'-hexamethyl-(1,1'-biphenol)-4,4'-diol, 878.4 g (7.2 mol) of 2,6-dimethylphenol, 1.26 g (7.3 mmol) of N,N'-di-tert-butylethylenediamine, and 27.19 g (268.7 mmol) of n-butyldimethylamine dissolved in 2300 g of methanol was added dropwise over 230 minutes and stirred. After the addition was completed, 1500 g of an aqueous solution in which 48.06 g (126.4 mmol) of tetrasodium ethylenediaminetetraacetate was dissolved was added to stop the reaction. The aqueous layer and the organic layer were separated, and the organic layer was washed with a 1N aqueous hydrochloric acid solution and then washed with pure water. The obtained solution was concentrated to 50% by mass using an evaporator to obtain 1980 g of a toluene solution of a bifunctional phenylene ether oligomer (resin "B0"). The number average molecular weight of resin "B0" based on polystyrene conversion by GPC method was 2100, the weight average molecular weight based on polystyrene conversion by GPC method was 3740, and the hydroxyl equivalent was 1070.

[0678] <<Synthesis of modified polyphenylene ether compounds>>

[0679] After 792 g of a 50% by mass toluene solution of a bifunctional phenylene ether oligomer (B0) was dried by an evaporator, 2772 g of N,N-dimethylacetamide was added and concentrated to a solid content of 20% by mass, to obtain 1980 g of a 79.80% by mass N,N-dimethylacetamide and 0.20% by mass toluene solution (B0) of a bifunctional phenylene ether oligomer. Next, 1980 g (0.37 mol in terms of OH equivalent) of the bifunctional phenylene ether oligomer solution (B0) and 67.78 g (0.44 mol) of chloromethylstyrene (CMS-P) were added to a reactor equipped with a stirring device, a thermometer, and a reflux tube, and heated and stirred at 50°C. While the reaction temperature was maintained at 50°C, 84.48 g (0.44 mol) of a methanol solution of sodium methoxide (concentration: 28.4% by mass) was added dropwise, and stirred for 1 hour. 9.75 g (0.05 mol) of a methanol solution of sodium methoxide (concentration: 28.4 mass%) was further added dropwise, and the mixture was stirred for 2 hours. Then, 5.91 g (0.05 mol) of an 85 mass% phosphoric acid aqueous solution was added, and after removing the generated inorganic salt, the reaction solution was added dropwise to 1975 g of water to solidify the mixture. After solid-liquid separation was performed by a centrifugal separator, the mixture was washed with pure water and methanol, and then dried under reduced pressure to obtain 381.87 g of the target polyphenylene ether compound (B). The number average molecular weight of the modified polyphenylene ether compound based on the polystyrene conversion by the GPC method was 2350, the weight average molecular weight was 3880, and the vinyl equivalent was 1220 g / vinyl.

[0680] <Synthesis Example 3 Synthesis of a polymer (va) having a structural unit represented by formula (V)>

[0681] 2.25 mol (292.9 g) of divinylbenzene, 1.32 mol (172.0 g) of ethylvinylbenzene, 11.43 mol (1190.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were placed in a reactor, and 600 mmol of a diethyl ether complex of boron trifluoride was added at 70°C to react for 4 hours. After the polymerization reaction was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and decompressed and devolatilized at 60°C to recover a polymer (va) having a structural unit represented by formula (V). The polymer (va) having a structural unit represented by formula (V) obtained was weighed, and it was confirmed that 860.8 g of a polymer (va) having a structural unit represented by formula (V) was obtained.

[0682] The obtained polymer (va) having a structural unit represented by formula (V) had a number average molecular weight Mn of 2060, a weight average molecular weight Mw of 30700, and a monodispersity Mw / Mn of 14.9. 13 C-NMR and 1In the H-NMR analysis, resonance lines derived from each monomer unit used as a raw material were observed in the polymer (va) having a structural unit represented by formula (V). Based on the NMR measurement results and GC analysis results, the ratio of each monomer unit (structural unit derived from each raw material) in the polymer (va) having a structural unit represented by formula (V) was calculated as follows.

[0683] Structural units derived from divinylbenzene: 20.9 mol% (24.3 mass%)

[0684] Structural units derived from ethylvinylbenzene: 9.1 mol% (10.7 mass%)

[0685] Structural unit derived from styrene: 70.0 mol% (65.0 mass%)

[0686] The content of structural units having residual vinyl groups derived from divinylbenzene was 16.7 mol% (18.5 mass%).

[0687] Example 1

[0688] 20 parts by mass of the resin (A) obtained in Synthesis Example 1, 40 parts by mass of the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal obtained in Synthesis Example 2, and 40 parts by mass of the polymer (va) having a structural unit represented by formula (V) obtained in Synthesis Example 3 were dissolved and mixed in methyl ethyl ketone and toluene to obtain a varnish. The compounding amount of each component is expressed as a value based on the solid content.

[0689] <Manufacturing of Test Specimens of Cured Plates with a Thickness of 1.0 mm>

[0690] The resin composition powder is obtained by evaporating the solvent from the obtained varnish. The obtained resin composition powder is used to make a cured plate as described below. 4.5 g of the resin composition powder is spread in a stainless steel mold 100 mm × 30 mm × 1.0 mm high frame, set in a vacuum press (Kitagawa Seiki Co., Ltd.), kept at 200 ° C for 1.5 hours, and pressed with a surface pressure of 1.9 MPa.

[0691] The powder or cured plate of the obtained resin composition was used to evaluate the minimum melt viscosity, viscosity (minimum melt temperature + 10°C) ÷ minimum melt viscosity, moldability, minimum melt temperature, glass transition temperature, relative dielectric constant (Dk), and dielectric loss tangent (Df). The evaluation results are shown in Table 1.

[0692] <Measurement Method and Evaluation Method>

[0693] (1) Minimum melt viscosity and viscosity (minimum melt temperature + 10°C) ÷ minimum melt viscosity

[0694] For the powder of the obtained resin composition, after confirming that the residual solvent amount is less than 1 mass% by GC measurement (GC-2025, manufactured by Shimadzu Corporation), 1 g is taken and formed into tablets with a diameter of 25 mm to prepare a measurement sample. The sample is measured using a viscoelasticity measuring device (ARES-G2, manufactured by TA Instruments Co., Ltd.) under the conditions of a heating temperature of 2°C / min and a frequency of 10 rad / s to determine the minimum melt viscosity (Pa·s) and the viscosity (minimum melt temperature + 10°C).

[0695] The minimum melt viscosity was evaluated as follows.

[0696] A: 20000Pa·s or less

[0697] B: more than 20000Pa·s and less than 100000Pa·s

[0698] C: more than 100000Pa·s

[0699] In addition, the value of viscosity (lowest melting temperature + 10° C.) ÷ lowest melting viscosity was calculated. Evaluation was performed as follows.

[0700] A: Less than 20 times

[0701] B: More than 20 times and less than 80 times

[0702] C: More than 80 times

[0703] (2) Formability

[0704] The formability was evaluated as follows.

[0705] A: The evaluation results of both the minimum melt viscosity and the value of viscosity (minimum melt viscosity+10° C.) ÷ minimum melt viscosity were A.

[0706] B: The evaluation result of the minimum melt viscosity and the value of viscosity (minimum melt viscosity+10° C.) ÷ minimum melt viscosity is A or B, and at least one of them is B.

[0707] C: C is included in the evaluation results of the minimum melt viscosity and the value of viscosity (minimum melt viscosity+10° C.) ÷ minimum melt viscosity.

[0708] (3) Minimum melting temperature

[0709] The temperature at which the minimum melt viscosity is reached is taken as the minimum melting temperature.

[0710] The unit is expressed in °C.

[0711] (4) Glass transition temperature

[0712] The sample obtained by miniaturizing the cured plate to 12.7 mm×30 mm was measured by DMA (Dynamic Mechanical Analysis) bending method according to JIS C6481 5.17.2 using a dynamic viscoelasticity measuring apparatus, and the peak temperature of the loss modulus obtained was defined as the glass transition temperature, expressed in °C.

[0713] As a dynamic viscoelasticity analyzer, DMA Q800 manufactured by TA Instruments, Inc. was used.

[0714] (5) Relative dielectric constant (Dk) and dielectric loss tangent (Df)

[0715] The cured plate was miniaturized to 1.0 mm in width and dried at 120°C for 60 minutes, and then the relative dielectric constant (Dk) and dielectric loss tangent (Df) after drying were measured at a frequency of 10 GHz using a perturbation cavity resonator. The measurement temperature was set at 23°C.

[0716] Agilent 8722ES manufactured by Agilent Technologies was used as the perturbation method cavity resonator.

[0717] Example 2

[0718] In Example 1, the same procedures were followed except that the content of the resin (A) was changed to 25 parts by mass, the content of the polyphenylene ether compound (B) was changed to 50 parts by mass, and the content of the polymer (va) having the structural unit represented by the formula (V) was changed to 25 parts by mass.

[0719] Comparative Example 1

[0720] In Example 1, the same procedures were carried out except that the resin (A) and the polymer (va) having the structural unit represented by the formula (V) were not used and the content of the polyphenylene ether compound (B) was changed to 100 parts by mass.

[0721] Comparative Example 2

[0722] In Example 1, the same procedures were carried out except that the resin (A) and the polyphenylene ether compound (B) were not used and the content of the polymer (va) having the structural unit represented by the formula (V) was changed to 100 parts by mass.

[0723] [Table 1]

[0724]

Claims

1. A resin composition, in, 100 parts by mass of a resin (A) having an indane skeleton and a terminal group represented by formula (T1), 10 to 300 parts by mass of a polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at a terminal and 10 to 300 parts by mass of a polymer having a structural unit represented by formula (V), In formula (T1), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, y represents an integer of 0 to 4, and * represents a bonding position to another site. In formula (V), Ar represents an aromatic hydrocarbon linking group, and * represents a bonding position.

2. The resin composition according to claim 1, in, The resin (A) comprises a resin represented by formula (T1-1), In formula (T1-1), R is a group containing a structural unit represented by formula (Tx), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, y is an integer of 0 to 4, In formula (Tx), n, o and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, 1.0≤n+o+p≤20.0, Ma each independently represents a hydrocarbon group having 1 to 12 carbon atoms optionally substituted by a halogen atom, x represents an integer from 0 to 4, and the structural units (a), (b), (c) are each bonded to the structural units (a), (b), (c), or other groups at *, and each structural unit is optionally randomly bonded.

3. The resin composition according to claim 1 or 2, in, The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal includes a polyphenylene ether compound represented by formula (OP), In formula (OP), X represents an aromatic group, -(YO) n1 - represents a polyphenylene ether structure, n1 represents an integer of 1 to 100, n2 represents an integer of 1 to 4, Rx is a group represented by formula (Rx-1) or formula (Rx-2), In formula (Rx-1) and formula (Rx-2), R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group, or an alkynyl group, * is a bonding site to an oxygen atom, Mc each independently represents a hydrocarbon group having 1 to 12 carbon atoms, z represents an integer of 0 to 4, and r represents an integer of 1 to 6.

4. The resin composition according to claim 1 or 2, in, The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal includes a polyphenylene ether compound represented by formula (OP-1), In formula (OP-1), X represents an aromatic group, -(YO)n 2 - represents the polyphenylene ether structure, R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group, n 1 Integer from 1 to 6, n 2 Integer from 1 to 100, n 3 Indicates an integer from 1 to 4.

5. The resin composition according to claim 1 or 2, in, The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal has a number average molecular weight (Mn) of 500 to 3,000 and a weight average molecular weight (Mw) of 800 to 6,000.

6. The resin composition according to claim 1 or 2, in, The number average molecular weight (Mn) of the resin (A) is 400-3000.

7. The resin composition according to claim 1 or 2, in, The mass ratio of the resin (A) is 10 to 50 parts by mass relative to 100 parts by mass of the total of the resin (A) and the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal. The resin composition according to claim 1 or 2, which does not substantially contain a polymerization inhibitor.

9. The resin composition according to claim 1 or 2, further comprising other compounds (C) other than the resin (A), the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal, and the polymer having the structural unit represented by formula (V).

10. The resin composition according to claim 9, in, The other compound (C) includes one or more selected from the group consisting of a maleimide compound, a cyanate compound, an epoxy compound, a phenol compound, a compound containing a (meth)allyl group, an oxetane resin, a benzoxazine compound, an arylcyclobutene resin, a polyamide resin, a polyimide resin, a perfluorovinyl ether resin, a compound having a styrene group other than the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal, a compound having an isopropenyl group other than the resin (A) having an indane skeleton, a multifunctional (meth)acrylate compound other than the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal, an elastomer, and a petroleum resin.

11. The resin composition according to claim 1 or 2, in, The total content of the resin (A) and the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond is 40 parts by mass or more based on 100 parts by mass of the resin solid content in the resin composition. 12 . The resin composition according to claim 1 , further comprising a filler (D).

13. The resin composition according to claim 12, in, The content of the filler (D) is 10 to 1000 parts by mass based on 100 parts by mass of the resin solid content in the resin composition.

14. The resin composition according to claim 1, in, The resin (A) comprises a resin represented by formula (T1-1), The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal includes a polyphenylene ether compound represented by formula (OP-1), The polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal has a number average molecular weight (Mn) of 500 to 3000 and a weight average molecular weight (Mw) of 800 to 6000, The number average molecular weight (Mn) of the resin (A) is 400 to 3000, The mass ratio of the resin (A) is 10 to 50 parts by mass relative to 100 parts by mass of the total of the resin (A) and the polyphenylene ether compound (B) having a carbon-carbon unsaturated double bond at the terminal. The resin composition contains substantially no polymerization inhibitor, The total content of the resin (A) and the polyphenylene ether compound (B) having a terminal carbon-carbon unsaturated double bond is 40 parts by mass or more relative to 100 parts by mass of the resin solid content in the resin composition, In formula (T1-1), R is a group containing a structural unit represented by formula (Tx), Mb each independently represents a hydrocarbon group having 1 to 12 carbon atoms which may be substituted with a halogen atom, y is an integer of 0 to 4, In formula (Tx), n, o and p are the average number of repeating units, n represents a number greater than 0 and less than 20, o and p each independently represent a number from 0 to 20, 1.0≤n+o+p≤20.0, Ma each independently represents a hydrocarbon group having 1 to 12 carbon atoms which is optionally substituted by a halogen atom, x represents an integer from 0 to 4, and each of the structural units (a), (b), (c) is bonded to the structural unit (a), (b), (c), or other groups at *, and each structural unit is optionally randomly bonded, In formula (OP-1), X represents an aromatic group, -(YO)n 2 - represents the polyphenylene ether structure, R 1 , R 2 and R 3 Each independently represents a hydrogen atom, an alkyl group, an alkenyl group or an alkynyl group, n 1 Integer from 1 to 6, n 2 Integer from 1 to 100, n 3 Indicates an integer from 1 to 4.

15. A cured product of the resin composition according to claim 1, 2 or 14.

16. A prepreg comprising a substrate and the resin composition according to claim 1, 2 or 14. 17 . A metal foil-clad laminate comprising: at least one layer formed of the prepreg according to claim 16 ; and a metal foil disposed on one or both sides of the layer formed of the prepreg. 18 . A resin composite sheet comprising: a support, and a layer formed from the resin composition according to claim 1 , 2 or 14 and disposed on a surface of the support. 19 . A printed wiring board comprising an insulating layer and a conductor layer disposed on a surface of the insulating layer, wherein the insulating layer comprises a layer formed from the resin composition according to claim 1 .

20. A semiconductor device comprising the printed circuit board according to claim 19.

Citation Information

Patent Citations

  • Curable resin composition

    JP2006070136A

  • Flame retardant resin composition

    JP2006089683A

  • Curable resin composition

    JP2008248001A

  • Soluble polyfunctional vinyl aromatic copolymer, method for producing the same, curable resin composition, and cured product of the same

    JP2018039995A

  • Phenylene ether oligomer, curable composition comprising phenylene ether oligomer, and thermoset composition derived therefrom

    JP2019194312A

Cited By

  • Low dielectric resin composition

    TWI907297B