Adhesive agent and electronic device using the same

A polymerizable liquid crystal compound with multiple functionalities addresses the adhesion and dielectric challenges of low dielectric substrates, ensuring effective bonding and heat resistance for high-frequency electronic boards in 5G and 6G communication equipment.

JP2024167588APending Publication Date: 2024-12-04JNC CORP

Patent Information

Application Number
JP2023083768
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-22
Publication Date
2024-12-04

AI Technical Summary

Technical Problem

Conventional adhesives for low dielectric electronic substrates face challenges in achieving good adhesion to low dielectric constant resin sheets and low-roughness copper foils, while maintaining excellent dielectric properties and heat resistance, which is crucial for high-frequency electronic boards used in 5G and 6G communication equipment.

Method used

A polymerizable liquid crystal compound with two or more functionalities is used as an adhesive, combined with a curing component, to bond low dielectric electronic substrates and metal foils or resist layers, providing excellent adhesion and dielectric properties, even at lower curing temperatures.

Benefits of technology

The adhesive enables effective bonding of low dielectric electronic substrates to metal foils and resist layers using conventional equipment, reducing signal loss and heat damage, while offering high heat resistance and heat dissipation properties for advanced communication devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024167588000033
    Figure 2024167588000033
  • Figure 2024167588000034
    Figure 2024167588000034
  • Figure 2024167588000001
    Figure 2024167588000001
Patent Text Reader

Abstract

To realize an adhesive agent having excellent heat resistance which has excellent adhesiveness with a low dielectric constant resin sheet being a raw material of a low dielectric electronic substrate, and excellent adhesiveness with a low roughness copper foil or a low dielectric constant resist layer by using a polymerizable liquid crystal composition (PLC) which changes from a solid state to a liquid state at a curing temperature or lower, in order to solve problems that a conventional adhesive agent for low dielectric electronic substrate has.MEANS: An adhesive agent contains a bifunctional or higher polymerizable liquid crystal composition and a curing component polymerizable with the polymerizable liquid crystal composition, and is used for bonding a low dielectric electronic substrate with a metal foil or a resist layer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive for low dielectric electronic substrates using a polymerizable liquid crystal compound, which has good adhesion to low dielectric resin sheets and also good adhesion to smooth metal foils such as copper foils and resist layers such as low dielectric resist layers, enabling metal foils and low dielectric resist layers to be laminated on low dielectric electronic substrates used in electronic substrates handling high frequencies for 5G and 6G using conventional production equipment and processes, and which has excellent dielectric properties in the adhesive layer. The adhesive also relates to an electronic device using this adhesive. [Background technology]

[0002] In recent years, with the shift to 5G and beyond 5G and 6G in communication devices, the frequency of electrical signals on electronic boards and the frequency of radio waves transmitted and received by antennas have also increased, causing problems with signal loss due to signal processing circuit boards and antenna boards. For this reason, there is a demand for low dielectric constants and low dielectric loss tangents in resin materials used in printed wiring boards and 2D and 2.5D semiconductor module boards, and instead of conventional polyimide and epoxy resins, resins such as liquid crystal polymers (LCPs), polyphenylene ethers (PPEs), cycloolefin polymers (COPs), and fluororesins (PTFEs) have begun to be used as board materials (Non-Patent Document 1). The low dielectric constant resin sheets and resist layers used as the raw materials for these boards have a reduced resin polarity in order to keep the dielectric constant low, so they have poor adhesion to conventional epoxy adhesives, making it necessary to use a thermoplastic adhesive that is laminated at high temperatures of nearly 300°C, or to treat the surface of the low dielectric constant resin sheet or resist layer to make it easier to adhere to.In addition, the high temperatures can cause significant damage to the resin and copper foil that make up the low dielectric constant electronic board or resist layer due to thermal oxidation and differences in thermal expansion coefficients, so there is a need to develop an adhesive that can provide strong adhesion at temperatures below 200°C.

[0003] In addition, the copper foil used as the electrode or wiring must be as flat as possible to avoid deterioration of characteristics due to the skin effect. Copper is inherently a metal that is difficult to adhere to, and in order to improve adhesion, the adhesion surface is roughened or other metals are further deposited on the roughened surface before it is adhered to glass epoxy boards or polyimide flexible boards (Non-Patent Document 1). This high-frequency copper foil, which has a very thin adhesion treatment layer, has low adhesion to adhesives, so adhesives for low-dielectric electronic boards are also required to have adhesion to this smooth copper foil (Non-Patent Document 2).

[0004] Thus, adhesives for low dielectric electronic boards are required not only to have adhesion between a low dielectric constant resin sheet and a smooth copper foil or a low dielectric constant resist layer, but also to have important dielectric properties of the adhesive layer itself after the adhesive is cured, since the adhesive is in direct contact with a circuit pattern formed by etching the copper foil. For this reason, polyolefin-based thermocompression adhesive sheets with excellent dielectric properties are often used (Non-Patent Document 1). However, in order to withstand the fixing of electronic components by reflow soldering, the compression temperature is designed to be quite high. On the other hand, thermosetting adhesives using epoxy resins have also been developed, but they are mixed with various polymers and additives to adjust the dielectric properties, heat resistance, and adhesiveness (Patent Documents 1, 2, 3).

[0005] Furthermore, in the case of printed wiring boards, a resist film or coverlay film is often applied to the outermost layer, or a film or prepreg that serves as the substrate is often laminated, so there is often a demand for adhesion between the resist film or between substrates (Patent Documents 4 and 5).

[0006] Generally, adhesives containing many epoxy groups are used to achieve strong adhesion, but in adhesives for low dielectric electronic substrates that use maleimide residues or (meth)acrylic groups as raw materials, and in areas where adhesion between resins is important, such as areas where copper is not exposed much on the surface, it is possible to ensure adhesion using maleimide residues or (meth)acrylic groups, which are the main components of the resin, without using epoxy resins, which are difficult to make high dielectric properties, so selecting a polymerizable group that is suitable for the substrate to be used is also an important issue (Patent Documents 4 and 5).

[0007] Adhesives for low-dielectric electronic substrates are often required to have high heat resistance, especially a high glass transition temperature, in order to provide resistance to reflow ovens. One method for increasing the glass transition temperature is to introduce a mesogen moiety into the polymer chain, as in LCP, and increase the glass transition temperature through intermolecular interactions of the mesogen moiety. However, LCP is generally a thermoplastic resin with low adhesiveness and a high softening temperature, making it difficult to use it as an adhesive. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2023-32287 A [Patent Document 2] JP 2023-32286 A [Patent Document 3] JP 2022-133352 A [Patent Document 4] Special Publication No. 2015-515927 [Patent Document 5] International Publication No. 2011 / 111471 [Non-patent literature]

[0009] [Non-Patent Document 1] "Towards 5G / beyond 5G: Latest development trends in high-speed, high-frequency compatible materials," Technical Information Association, 2021, pp. 49, 50, 120, 121. [Non-Patent Document 2] "Latest technological trends and future prospects for next-generation communications and millimeter wave technology," AndTech, 2021, p.19, 28, 29. Summary of the Invention [Problem to be solved by the invention]

[0010] The problem that the present invention aims to solve is to realize an adhesive with excellent heat resistance, which has good adhesion to low dielectric constant resin sheets, which are the raw materials for low dielectric constant electronic substrates, and also has good adhesion to low roughness copper foils and low dielectric constant resist layers, by using a polymerizable liquid crystal compound (PLC) that changes from a solid to a liquid state below the curing temperature, in order to solve the problems of conventional adhesives for low dielectric constant electronic substrates. Furthermore, the cured product of the polymerizable liquid crystal compound has high thermal conductivity, and can also be given high heat dissipation as an added value. By using the adhesive of the present invention, it is possible to provide an adhesive suitable for producing substrates for next-generation communication devices and radars in the high-frequency range. [Means for solving the problem]

[0011] As a result of intensive research into solving the above problems, the inventors discovered that by using a bifunctional or higher functional polymerizable liquid crystal compound and a curing component as an adhesive component, an adhesive having both excellent dielectric properties and adhesive properties can be realized, thereby completing the present invention.

[0012] [1] An adhesive containing a bifunctional or higher functional polymerizable liquid crystal compound and a curable component that can polymerize with the polymerizable liquid crystal compound, used to bond low dielectric electronic substrates to metal foil or resist layers.

[0013] [2] The adhesive according to [1], wherein the bifunctional or higher functional polymerizable liquid crystal compound is a polymerizable liquid crystal compound represented by formula (1): R 1a -Z 1 -A 1 -Z 2 -A 2 -(Z 3 -A3 ) m1 -Z 4 -R 1b (1) In formula (1), A 1 , A 2 , and A 3 are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, bicyclo[2.2.2]octo-1,4-diyl, bicyclo[3.1.0]hex-3,6-diyl, or fluorene-2,7-diyl, and in these rings, at least one -CH 2 - may be replaced by -O-, at least one -CH= may be replaced by -N=, at least one hydrogen may be replaced by halogen or an alkyl having 1 to 12 carbon atoms in which at least one hydrogen may be replaced by halogen, and in this alkyl, at least one -CH 2 - may be replaced by -O-, -CO-, -COO-, -OCO-, or -C=C-; Z 1 , Z 2 , Z 3 , and Z 4 are independently a single bond or an alkylene having 1 to 20 carbon atoms, and in this alkylene, at least one -CH 2 - is -O-, -S-, -CO-, -COO-, -OCO-, -SO 2 -, -CH=CH-, -CF=CF-, -CH=N-, -N=CH-, or -N=N-, and at least one hydrogen may be replaced by a halogen; m1 is 0, 1, or 2; In the formula, Z 3 Or A 3 When there are multiple, they may be the same or different, R 1a and R 1b are independently a group selected from the polymerizable groups represented by formulas (PG-1) to (PG-5), TIFF2024167588000001.tif51116 formula (PG-1)~(PG-5), R bis hydrogen, halogen, -CF 3 or an alkyl group having 1 to 5 carbon atoms, q is 0 or 1, and there are multiple R b may be the same or different; A 1 and A 2 is 1,4-phenylene, and Z 2 is a single bond, m1 is 0, and R 1a and R 1b When the polymerizable group is represented by formula (PG-5), Z 1 and Z 4 is an alkylene having 3 to 20 carbon atoms, and in this alkylene, at least one -CH 2 - is -O-, -S-, -CO-, -COO-, -OCO-, -SO 2 may be replaced by -, -CH=CH-, -CF=CF-, -CH=N-, -N=CH-, or -N=N-, and at least one hydrogen may be replaced by a halogen.

[0014] [3] A of the bifunctional or higher polymerizable liquid crystal compound 1 From the right end A 3 The mesogen portion up to is a biphenyl structure, and the biphenyl structure and R 1a and R 1b A linear Z having 3 or more carbon atoms is placed between the epoxy groups. 1 and Z 4 The adhesive described in [2], wherein

[0015] [4] The adhesive according to [2], wherein the mesogen moiety of the difunctional or higher functional polymerizable liquid crystal compound has a bicyclohexyl structure.

[0016] [5] The adhesive according to any one of [2] to [4], wherein the polymerizable group of the di- or higher functional polymerizable liquid crystal compound is a polymerizable group represented by formula (PG-5).

[0017] [6] The adhesive according to any one of [1] to [5], wherein the curing component comprises at least one selected from the group consisting of a curing agent, a polymerization initiator, a curing accelerator, and a crosslinking agent.

[0018] [7] The adhesive according to [6], wherein the curing agent comprises at least one selected from the group consisting of a polyphenylene ether oligomer having at least two hydroxyl groups, an active ester curing agent, and an alkyl ether having at least two hydroxyl groups.

[0019] [8] The adhesive according to any one of [1] to [7], further comprising 1 to 30 volume % of an inorganic filler.

[0020] [9] The adhesive according to [8], wherein the inorganic filler is at least one selected from the group consisting of silicon oxide compounds such as spherical silica, crushed silica, hollow silica and fumed silica, carbon nanotubes, graphene, silicon carbide, and metal oxides such as magnesium oxide and zinc oxide.

[0021]

[10] The adhesive according to [8], wherein the inorganic filler is a nitride filler, and a cured product of the adhesive has a thermal conductivity of 1 W / m K or more.

[0022]

[11] The adhesive according to any one of the items [1] to

[10] , wherein the adhesive is a solid adhesive.

[0023]

[12] The adhesive according to any one of [1] to

[11] , wherein the low dielectric substrate includes at least one layer selected from the group consisting of liquid crystal polymer resin, modified polyimide resin, polyphenylene ether resin, polyphenylene sulfide resin, cycloolefin resin, and fluororesin.

[0024]

[13] An electronic device using the adhesive according to any one of [1] to

[12] . Effect of the Invention

[0025] In the present invention, by using an adhesive for low dielectric electronic substrates using a polymerizable liquid crystal compound, a laminate obtained by laminating a low dielectric electronic substrate and a metal foil or a resist layer can be produced by using conventional production equipment with a set temperature of 200°C or less to bond a low dielectric electronic substrate made of a low dielectric constant resin to a metal foil such as a low roughness copper foil or a resist layer such as a low dielectric constant resist layer, and the resin part where the adhesive of the present invention is cured has excellent dielectric properties, and the laminate can be produced with high heat resistance. As a result, an electronic device can be realized that has little signal loss in the electronic substrate as frequencies go beyond 5G and 6G, can withstand high temperatures associated with increased heat generation from semiconductor chips, and has heat dissipation properties. [Brief description of the drawings]

[0026] [Figure 1] Fig. 1 is a schematic diagram of a sample prepared to measure the peel strength between a low dielectric film and copper foil in [Examples] and [Comparative Examples]. A 7 cm x 1 cm copper foil with an adhesive component coating layer was placed on a 5 cm square low dielectric film as shown in Fig. 1, and then the adhesive of the present invention (adhesive component coating layer) was cured using a heat press to bond the low dielectric film and the copper foil, so that the 2 cm protruding portion could be held by a tensile tester (autograph). [Diagram 2] Figure 2 is a schematic diagram of the jig used to attach the sample in Figure 1 to the tensile tester. The sample in Figure 1 was attached to a 2 mm thick aluminum plate as shown in Figure 2 and measured. The JIS standard requires a sample with a bonding length of 10 cm, but with the simplified method shown in Figure 2, the angle between the copper foil and the low dielectric film substrate becomes smaller as the measurement progresses, causing the measured value to deviate from that when perpendicular, so the bonding length was halved to 5 cm. With this length, there is also the length of the load cell of the tensile tester, so there is no significant difference in the angle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The following provides a detailed description of the bifunctional or higher polymerizable liquid crystal compound used in the present invention, a curable component (hereinafter sometimes referred to as the curable component) that can polymerize with this polymerizable liquid crystal compound, an adhesive containing these and used for bonding a low dielectric electronic substrate to a metal foil or a resist layer, an electronic device of the present invention using the adhesive, and methods for producing these. The terms used in this specification are as follows. "Liquid crystal compound" is a general term for compounds having a liquid crystal phase such as a nematic phase or a smectic phase, and compounds that do not have a liquid crystal phase but have physical properties specific to liquid crystals such as dielectric anisotropy, refractive index anisotropy, magnetic susceptibility anisotropy, etc., and are useful as components of liquid crystal compositions. In the liquid crystal temperature range, alignment treatment becomes easy, and the molecular alignment can be controlled like the stretching treatment of thermoplastic resins. "Compound (1)" means a polymerizable liquid crystal compound represented by the formula (1) as a bifunctional or higher functional polymerizable liquid crystal compound, and may also mean at least one of the compounds represented by the formula (1). The same applies to "compound (1-1)" and the like, and compounds (1-1), (1-2) and (1-3) may also be collectively referred to as "compound (1)". One compound (1) may contain multiple A 3 When we have, any two A 3 may be the same or different. b When any two R b may be the same or different. This rule also applies to other symbols, groups, etc., such as q and X. The term "polymer (1)" refers to at least one type of polymer obtained by polymerizing the compound (1). As with the term "compound (1)," the polymers of the compounds (1-1), (1-2), and (1-3) may be collectively referred to as "polymer (1)." "Adhesive (1)" refers to an adhesive containing a difunctional or higher polymerizable liquid crystal compound, preferably at least one selected from the compounds (1) as a difunctional or higher polymerizable liquid crystal compound, and a curing component polymerizable with the polymerizable liquid crystal compound, and is an adhesive for bonding a low dielectric electronic substrate and a metal foil or a resist layer, i.e., the adhesive of the present invention.

[0028] [glue] The adhesive of the present invention is an adhesive containing a bifunctional or higher functional polymerizable liquid crystal compound and a curable component polymerizable with this polymerizable liquid crystal compound, and is an adhesive for bonding a low dielectric electronic substrate to a metal foil or a resist layer.

[0029] 1) Compound (1) As the bifunctional or higher polymerizable liquid crystal compound used in the present invention, the polymerizable liquid crystal compound (1) represented by the above formula (1) (hereinafter, sometimes referred to as compound (1)) is a preferred compound, which has a liquid crystal skeleton (rod-shaped mesogenic skeleton) and a polymerizable group, and preferably has few conjugated or polar groups, high molecular linearity and symmetry, high polymerization reactivity, a wide liquid crystal phase temperature range, good miscibility, etc. This compound (1) can be easily made homogeneous when mixed with other liquid crystal compounds or polymerizable compounds. The melting point of compound (1) is preferably 200°C or lower, more preferably 180°C or lower, and even more preferably 160°C or lower, from the viewpoint of adhesion and curing temperatures. The transition temperature of compound (1) from a nematic phase to a liquid is preferably 200°C or lower, more preferably 180°C or lower, and even more preferably 160°C or lower, from the viewpoint of molding and curing temperatures. The bifunctional or higher polymerizable liquid crystal compound used in the present invention is a compound (1) represented by the formula (1) and composed of a ring structure, a bonding group, a terminal group, and other groups. 1a or R 1b , ring structure A 1 , A 2 Or A 3 and the bonding group Z 1 , Z 2 , Z 3 or Z 4By appropriately selecting these, physical properties such as the liquid crystal phase expression region can be adjusted as desired. The effects of the types of terminal group, ring structure and bonding group on the physical properties of compound (1), as well as preferred examples of these compounds (1) defined by the above formula (1), are explained below. The ring structure, bonding group and terminal group are referred to as "ring structure A", "bonding group Z" and "terminal group R", respectively. 1 " is sometimes referred to collectively. In addition, "at least one -CH 2 The meaning of phrases such as "- may be replaced by -O-" is shown below as an example. 4 H 9 At least one -CH 2 As a group in which - is replaced by -O-, there is C 3 H 7 O-, CH 3 -O-(CH 2 ) 3 -, CH 3 -O-CH 2 -O-, etc. In this way, the term "at least one" means "at least one selected without distinction." In addition, in consideration of the stability of the compound, it is preferable that oxygen and oxygen are not adjacent to each other. 3 -OO-CH 2 - is a CH group with no adjacent oxygens. 3 -O-CH 2 -O- is preferred.

[0030] <Ring structure A :A 1 , A 2 and A 3 > Ring structure A of compound (1) 1 is a group selected from a benzene ring bonded at the para position, a cyclohexane ring bonded at the para position, ring structures represented by the following formulae (R1-1) to (R1-8), and ring structures represented by the following formulae (R2-1) to (R2-8). TIFF2024167588000002.tif4699 TIFF2024167588000003.tif4699 In equations (R1-1) to (R1-8) and equations (R2-1) to (R2-8), X 1is halogen or alkyl having 1 to 6 carbon atoms. Ring structure A of compound (1) 1 Preferred examples of the formula (R1-1), (R1-2), (R1-3), (R2-1), (R2-2), and (R2-3) are those in which X 1 When the aryl group is fluorine or methyl, the aryl group has a low melting point, exhibits fluidity at about room temperature, and exhibits high solubility in organic solvents. Ring structure A 2 and A 3 is 1,4-phenylene or 1,4-cyclohexylene, and in these rings, at least one hydrogen may be replaced by halogen or alkyl having 1 to 6 carbon atoms in which at least one hydrogen may be replaced by halogen. In the case of these ring structures, they have the characteristics of a high clearing point, a very low relative dielectric constant, a low dielectric loss, and a low viscosity. Furthermore, they often have a low melting point and exhibit fluidity around room temperature, so that it is possible to easily prepare an adhesive that can be formed into a film by a coating method using no solvent or a small amount of organic solvent. For manufacturing reasons, the ring structure A 1 is a group selected from the ring structures represented by formulae (R1-1) to (R1-8), the ring structure A 2 Or A 3 is preferably 1,4-phenylene in which at least one hydrogen may be replaced by halogen or alkyl having 1 to 6 carbon atoms, 1 is a group selected from the ring structures represented by formulae (R2-1) to (R2-8), the ring structure A 2 Or A 3 and 1,4-cyclohexylene in which at least one hydrogen may be replaced by halogen or alkyl having 1 to 6 carbon atoms.

[0031] Ring structure A of compound (1) 2 Or A 3Particularly preferred examples of the aromatic ring structures are 1,4-phenylene, 2-methyl-1,4-phenylene, 3-methyl-1,4-phenylene, 2,3-dimethyl-1,4-phenylene, 2,5-dimethyl-1,4-phenylene, 2,6-dimethyl-1,4-phenylene, 3,5-dimethyl-1,4-phenylene, 2-fluoro-1,4-phenylene, 3-fluoro-1,4-phenylene, 2,3-difluoro-1,4-phenylene, 2,5-difluoro-1,4-phenylene, 2,6-difluoro-1,4-phenylene, and 3,5-difluoro-1,4-phenylene, as well as The alicyclic structures are 1,4-cyclohexylene, 2-methyl-1,4-cyclohexylene, 3-methyl-1,4-cyclohexylene, 2,3-dimethyl-1,4-cyclohexylene, 2,5-dimethyl-1,4-cyclohexylene, 2,6-dimethyl-1,4-cyclohexylene, 3,5-dimethyl-1,4-cyclohexylene, 2-fluoro-1,4-cyclohexylene, 3-fluoro-1,4-cyclohexylene, 2,3-difluoro-1,4-cyclohexylene, 2,5-difluoro-1,4-cyclohexylene, 2,6-difluoro-1,4-cyclohexylene, and 3,5-difluoro-1,4-cyclohexylene.

[0032] The configuration of 1,4-cyclohexylene may be either cis or trans. In the case of the cis form, the melting point is low, while in the case of the trans form, the linearity is high and the dielectric constant is low.

[0033] When at least one ring in the ring structure A is 1,4-phenylene, the orientational order parameter and magnetic anisotropy are large, and when at least two rings are 1,4-phenylene, the clearing point is high. Preferred examples of the 1,4-phenylene ring in which at least one hydrogen atom may be replaced include fluorine, alkyl having 1 to 6 carbon atoms, or -CF 3 It has a low melting point and high solubility. It also has a low dielectric constant due to its small molecular polarizability. Furthermore, it has low dielectric loss due to its suppressed molecular motion. When at least one ring in the ring structure A is 1,4-cyclohexylene, the clearing point is high, the dielectric constant is very low, the dielectric loss is low, and the viscosity is small. When at least two rings are trans-1,4-cyclohexylene, the clearing point is high, the dielectric constant is very low, the dielectric loss is low, and the viscosity is small. In the case of cis-1,4-cyclohexylene, the melting point is low, and in the case of trans-1,4-cyclohexylene, the linearity is high and the dielectric constant is low.

[0034] <Binding group Z :Z 1 , Z 2 , Z 3 and Z 4 > Preferred examples of the bonding group Z in compound (1) include a single bond, -(CH 2 ) a -, -O(CH 2 ) b -, -(CH 2 ) b O- or -O(CH 2 ) c O-, where a is an integer from 1 to 20, b is an integer from 1 to 19, and c is an integer from 1 to 18. The bonding group Z is a single bond, -(CH 2 ) a -, -(CH 2 ) b O-, -O(CH 2 ) b - or -O(CH 2 ) c When the bonding group Z is -(CH 2 ) a -, -(CH 2 ) b O-, -O(CH 2 ) b - or -O(CH 2 ) c When the formula is O-, a is an integer of about 2 to 12, b is an integer of about 1 to 11, and c is an integer of about 1 to 10, the molecular length is long, the melting point is low, the solubility in organic solvents is high, and the dielectric tangent is small.

[0035] <Terminal group R 1:R 1a and R 1b > End group R of compound (1) 1 is a polymerizable group represented by any one of formulas (PG-1) to (PG-5).

[0036] TIFF2024167588000004.tif51116

[0037] In formulas (PG-1) to (PG-5), R b is hydrogen, halogen, -CF 3 Or it is alkyl having 1 to 5 carbon atoms, and q is 0 or 1. There are also multiple R b They may be the same or different.

[0038] End group R of compound (1) 1 Preferred examples include polymerizable groups represented by formulae (PG-1a) to (PG-1d), (PG-2a), (PG-3a), (PG-4a), and (PG-5a) to (PG-5d).

[0039] TIFF2024167588000005.tif51135

[0040] Among these preferred polymerizable groups, (PG-1a) to (PG-1d), (PG-2a), and (PG-4a) have an α,β-unsaturated ketone structure, and therefore can be polymerized by various means to be changed into a polymer having a larger molecular weight. (PG-3a) has a vinyl adjacent to an electron donating group, and therefore can be polymerized by various means to be changed into a polymer having a larger molecular weight. (PG-5a) to (PG-5d) have a strained cyclic ether, and therefore can be polymerized by various means to be changed into a polymer having a larger molecular weight.

[0041] The polymerizable groups represented by the formulae (PG-1) to (PG-5) can be appropriately selected depending on the production conditions of the adhesive. When preparing a thermosetting adhesive for low dielectric electronic substrates, the maleimide residue represented by formula (PG-2a), the oxiranyl represented by formula (PG-5a), and the oxetanyl represented by formula (PG-5b) are preferred from the viewpoints of heat resistance, heat dissipation, etc. When preparing a photocurable adhesive that is typically used in the adhesive for low dielectric electronic substrates of the present invention, the acrylic or methacrylic represented by formula (PG-1) are preferred from the viewpoints of high curability, solubility in organic solvents, ease of handling, etc.

[0042] As described above, the ring structure A, the bonding group Z, and the terminal group R 1 By appropriately selecting the type of ring, the number of rings, etc., a compound (1) having the desired physical properties can be obtained. Preferred examples of compound (1) include compounds represented by formulas (1-1) to (1-6).

[0043] TIFF2024167588000006.tif6693

[0044] TIFF2024167588000007.tif6793 formula (1-1)~(1-6), Z 1 , Z 2 , and Z 4 are independently a single bond, -(CH 2 ) a -, -O(CH 2 ) b -, -(CH 2 ) b O- or -O(CH 2 ) c O-, where a is an integer from 1 to 20, b is an integer from 1 to 19, and c is an integer from 1 to 18; X is fluorine or methyl, Me is methyl, n is an integer of 0 to 4 including the case where n is 2 or more, and when there are a plurality of X in the formula, they may be the same or different, R 1a and R 1b are independently a polymerizable group represented by formula (PG-1) or (PG-5).

[0045] TIFF2024167588000008.tif2041 Formula (PG-1) and (PG-5), R b is hydrogen, halogen, -CF 3 or an alkyl group having 1 to 5 carbon atoms, q is 0 or 1, and there are multiple R b They may be the same or different.

[0046] Preferred specific examples of the compounds (1-1) to (1-6) are shown below. TIFF2024167588000009.tif11894

[0047] TIFF2024167588000010.tif130100

[0048] TIFF2024167588000011.tif12497

[0049] TIFF2024167588000012.tif11897

[0050] TIFF2024167588000013.tif12399

[0051] TIFF2024167588000014.tif12496

[0052] In formulas (1-1-1) to (1-6-7), Z 2 is a single bond, -(CH 2 ) a -, -O(CH 2 ) b -, -(CH 2 ) b O- or -O(CH 2 ) cO-, where a is an integer of 1 to 20, b is an integer of 1 to 19, c is an integer of 1 to 18, m is an integer of 0 to 20, M is a single bond or oxygen, X is fluorine or methyl, and when there are multiple X in the formula, they may be the same or different, and Me is methyl, and in the formula, multiple m or M may be the same or different. However, in view of the definitions of the formulae of more preferred specific examples of compound (1), the formulae (1-1-5) and (1-2-3), the formulae (1-1-7) and (1-3-3), the formulae (1-4-5) and (1-5-3), and the formulae (1-4-7) and (1-6-3) each include partially overlapping compound (1).

[0053] [Method for synthesizing compound (1)] Compound (1) can be synthesized by combining known methods in organic synthetic chemistry. Methods for introducing the desired terminal groups, ring structures, and bonding groups into starting materials are described in books such as Houben-Wyle, Methods of Organic Chemistry, Georg Thieme Verlag, Stuttgart, Organic Syntheses, John Wily & Sons, Inc., Organic Reactions, John Wily & Sons Inc., Comprehensive Organic Synthesis, Pergamon Press, and New Experimental Chemistry Lectures (Maruzen).

[0054] The method for introducing the bonding group Z is described in the following schemes 1 to 4. 1 and MSG 2 represents a monovalent organic group having at least one ring, and Hal represents a halogen. 1 (or MSG 2) may be the same or different. Compounds (1A) to (1F) in the following scheme correspond to the above-mentioned compound (1). These methods can be applied to the synthesis of optically active compound (1) and optically inactive compound (1).

[0055] (Scheme 1) Compounds where Z is a single bond As shown below, arylboronic acid (S1) is reacted with compound (S2) synthesized by a known method in the presence of an aqueous carbonate solution and a catalyst such as tetrakis(triphenylphosphine)palladium to obtain MSG. 1 and MSG 2 Compound (1A) can be synthesized in which a single bond is introduced between the compound (S3) and the compound (S4). Compound (1A) can also be synthesized by reacting compound (S3), which is synthesized by a known method, with n-butyllithium and then with zinc chloride, and then further reacting compound (S2) in the presence of a catalyst such as dichlorobis(triphenylphosphine)palladium.

[0056] TIFF2024167588000015.tif53137

[0057] (Scheme 2) Z is -(CH 2 ) 2 - Compound As shown below, the compound (1B) obtained as above is hydrogenated in the presence of a catalyst such as palladium on carbon to give MSG. 1 and MSG 2 Between -(CH 2 ) 2 Compound (1C) having the formula (1C) can be synthesized.

[0058] TIFF2024167588000016.tif25130

[0059] (Scheme 3) Z is -(CF 2 ) 2 - Compound As shown below, MSG can be obtained by fluorinating diketone (S6) with sulfur tetrafluoride in the presence of a fluorinating agent according to the method described in J. Am. Chem. Soc., 2001, 123, 5414. 1 and MSG 2 Between -(CF 2 ) 2 Compound (1D) having the formula (1D) can be synthesized.

[0060] TIFF2024167588000017.tif35122

[0061] (Scheme 4) Z is -(CH 2 ) 4 - Compound As shown below, according to the method of Scheme 1, a phosphonium salt (S7) was used to prepare -(CH 2 ) 2 A compound having -CH=CH- was synthesized and catalytically hydrogenated in the same manner as in Scheme 2 to obtain MSG. 1 and MSG 2 Between -(CH 2 ) 4 Compound (1E) having - introduced therein can be synthesized.

[0062] TIFF2024167588000018.tif34151

[0063] (Scheme 5) Z is -CH 2 O- or -OCH 2 - Compound As shown below, compound (S4) is reduced with a reducing agent such as sodium borohydride to obtain compound (S8). Compound (S8) is halogenated with hydrobromic acid to obtain compound (S9). Compound (S9) is reacted with compound (S10) in the presence of potassium carbonate to obtain MSG. 1 and MSG 2 Between -OCH 2 -(or -CH 2 O-) can be introduced into compound (1F).

[0064] TIFF2024167588000019.tif55148

[0065] 2) Polymer (1) The compound (1) used in the present invention has a polymerizable group (terminal group R 1 ), it can be easily polymerized. The polymer (1) in the present invention is at least one type of polymer obtained by polymerizing the compound (1). In the adhesive (1) described in the next section, the polymer (1) constituted by a combination of at least one other component may be an oligomer of the compound (1). This oligomer means a low polymer having a small number (degree of polymerization) of constitutional units of the compound (1) constituting the polymer (1). Depending on the number of constitutional units, the oligomer may be called a dimer, trimer, tetramer, etc.

[0066] 3) Adhesive (1) The adhesive (1) in the present invention is an adhesive containing a bifunctional or higher polymerizable liquid crystal compound and a curing component polymerizable with the polymerizable liquid crystal compound, and is preferably an adhesive containing at least one compound (1) as the bifunctional or higher polymerizable liquid crystal compound. The adhesive (1) may preferably be composed of two or more compounds (1) as the compound (1), or may be composed of at least one compound (1) in combination with at least one other component other than the bifunctional or higher polymerizable liquid crystal compound including the polymer (1). The component of such at least one other component is not particularly limited, but may include polymer (1), a polymerizable compound other than the bifunctional or higher polymerizable liquid crystal compound (hereinafter sometimes referred to as "other polymerizable compound"), an organic solvent, a non-polymerizable liquid crystal compound, an inorganic filler, and a fibrous reinforcing agent. Preferred examples of the adhesive (1) include an adhesive composed of at least one compound (1), a curing component, and a polymer (1), an adhesive composed of at least one compound (1), a curing component, and other polymerizable compounds, and an adhesive composed of at least one compound (1), a curing component, a polymer (1), and other polymerizable compounds.

[0067] 4) Other polymerizable compounds The adhesive (1) may contain a polymerizable compound (other polymerizable compound) other than the difunctional or higher polymerizable liquid crystal compound. The polymerizable compound other than the difunctional or higher polymerizable liquid crystal compound is composed of at least one of the following polymerizable liquid crystal compounds other than the difunctional or higher polymerizable liquid crystal compounds (hereinafter sometimes referred to as "other polymerizable liquid crystal compounds") and at least one of the following polymerizable non-liquid crystal compounds other than the difunctional or higher polymerizable liquid crystal compounds (hereinafter sometimes referred to as "other polymerizable non-liquid crystal compounds"). 4-1) Other polymerizable liquid crystal compounds The adhesive (1) may contain at least one polymerizable liquid crystal compound other than the difunctional or higher functional polymerizable liquid crystal compound, that is, at least one monofunctional polymerizable liquid crystal compound.

[0068] 4-2) Other polymerizable non-liquid crystal compounds The adhesive (1) may contain at least one other polymerizable non-liquid crystal compound as a component. As such other polymerizable non-liquid crystal compounds, compounds that do not reduce film-forming properties and mechanical strength are preferred. These polymerizable non-liquid crystal compounds are classified as compounds that do not have liquid crystal properties. Examples of other polymerizable non-liquid crystal compounds that are polymerizable compounds that do not have liquid crystal properties include derivatives such as vinyl derivatives, styrene derivatives, (meth)acrylic acid derivatives, sorbic acid derivatives, fumaric acid derivatives, and itaconic acid derivatives, modified polyimide oligomers, modified maleimide oligomers, modified polyphenylene ether oligomers, modified polyphenylene sulfide oligomers, and modified polybutadiene elastomers, and modified engineering plastic oligomers and modified elastomers, i.e., macromers, which mean high molecular weight compounds having polymerizable functional groups such as addition polymerizable double bonds. Preferred examples of these derivatives are shown below. In the text, "(meth)acryloyloxy" means acryloyloxy or methacryloyloxy, "(meth)acrylate" means acrylate or methacrylate, and "(meth)acrylic acid" means acrylic acid or methacrylic acid.

[0069] Preferred vinyl derivatives include vinyl chloride, vinyl fluoride, vinyl acetate, vinyl pivalate, vinyl 2,2-dimethylbutanoate, vinyl 2,2-dimethylpentanoate, vinyl 2-methyl-2-butanoate, vinyl propionate, vinyl stearate, vinyl 2-ethyl-2-methylbutanoate, N-vinylacetamide, vinyl pt-butylbenzoate, vinyl N,N-dimethylaminobenzoate, vinyl benzoate, ethyl vinyl ether, hydroxybutyl monovinyl ether, t-amyl vinyl ether, cyclohexanedimethanol methyl vinyl ether, α,β-vinyl naphthalene, methyl vinyl ketone, and isobutyl vinyl ketone.

[0070] Preferred styrene derivatives include styrene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, o-chloromethylstyrene, m-chloromethylstyrene, p-chloromethylstyrene, and α-methylstyrene.

[0071] Preferred (meth)acrylic acid derivatives include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, phenyl (meth)acrylate, 1,4-butanediol diacrylate, 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, neopentyl glycol diacrylate, triethylene glycol diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, tetraethylene glycol diacrylate, trimethylolpropane triacrylate, trimethylol EO-added triacrylate, pentaerythritol triacrylate, tris(meth)acryloyloxyethyl phosphate, bisphenol A EO-added diacrylate, bisphenol A glycidyl diacrylate (trade name: "Viscoat 700" manufactured by Osaka Organic Chemical Industry Co., Ltd.), polyethylene glycol diacrylate dimethyl itaconate, and the like.

[0072] Preferred sorbic acid derivatives include sodium sorbate, potassium sorbate, lithium sorbate, 1-naphthylmethylammonium sorbate, benzylammonium sorbate, dodecylammonium sorbate, octadecylammonium sorbate, methyl sorbate, ethyl sorbate, propyl sorbate, isopropyl sorbate, butyl sorbate, t-butyl sorbate, hexyl sorbate, octyl sorbate, octadecyl sorbate, cyclopentyl sorbate, cyclohexyl sorbate, vinyl sorbate, allyl sorbate, and propargyl sorbate.

[0073] Preferred fumaric acid derivatives include dimethyl fumarate, diethyl fumarate, diisopropyl fumarate, dibutyl fumarate, dicyclopentyl fumarate, and dicyclohexyl fumarate.

[0074] Preferred itaconic acid derivatives include diethyl itaconate, dibutyl itaconate, and diisopropyl itaconate. In addition to these, many polymerizable non-liquid crystal compounds such as butadiene, isoprene, and maleimide can be used.

[0075] 5) Curing component The curing component preferably includes at least one selected from the group consisting of a curing agent, a polymerization initiator, a curing accelerator, and a crosslinking agent. Of these, the curing agent more preferably includes at least one selected from the group consisting of a polyphenylene ether oligomer having at least two hydroxyl groups, an active ester curing agent, and an alkyl ether having at least two hydroxyl groups.

[0076] 6) Polymerization initiator The adhesive (1) may contain a polymerization initiator as a component. The polymerization initiator may be a thermal radical polymerization initiator, a photoradical polymerization initiator, a photocationic polymerization initiator, or the like, depending on the curing method (polymerization method) of the adhesive (1). When the bifunctional or higher polymerizable liquid crystal compound used in the present invention is composited with an inorganic filler to increase thermal conductivity, it is preferable to use a thermal radical polymerization initiator because the inorganic filler absorbs light. When a composite material with an inorganic filler is used as a thin film with a thickness of several μm, it is also possible to increase the amount of polymerization initiator or use a strong polymerization initiator to cure by photopolymerization.

[0077] Preferred thermal radical polymerization initiators include benzoyl peroxide, diisopropyl peroxydicarbonate, t-butyl peroxy-2-ethylhexanoate, t-butyl peroxypivalate, di-t-butyl peroxide (DTBPO), t-butyl peroxydiisobutyrate, lauroyl peroxide, dimethyl 2,2'-azobisisobutyrate (MAIB), azobisisobutyronitrile (AIBN), azobiscyclohexanecarbonitrile (ACN), dimethyl 2,2'-azobis(isobutyrate), and the like. Commercially available peroxide polymerization initiators include benzoyl peroxide, which is available from various companies, as well as "Dicumyl Peroxide" (trade name) manufactured by Tokyo Chemical Industry Co., Ltd., and "Percumyl D, Niper BMT, Perhexa 25Z" (trade names) manufactured by NOF Corp. Examples of azo polymerization initiators include AIBN, which is available from various companies, as well as "V-40, V-50, V-59, V-65, V-70, V-501, V-601" (trade names) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. In general, azo polymerization initiators can be suitably used for both thermal radical polymerization and photoradical polymerization.

[0078] The photoradical polymerization initiator is not particularly limited, and any known photoradical polymerization initiator can be used. 4-Methoxyphenyl-2,4-bis(trichloromethyl)triazine, 2-(4-butoxystyryl)-5-trichloromethyl-1,3,4-oxadiazole, 9-phenylacridine, 9,10-benzphenazine, benzophenone / Michler's ketone mixture, hexaarylbiimidazole / mercaptobenzimidazole mixture, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, benzyl dimethyl ketal, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2,4-diethylxanthone / methyl p-dimethylaminobenzoate mixture, benzophenone / methyltriethanolamine mixture, etc. Commercially available products include those manufactured by Chiba Specialty Co., Ltd., marketed under the trade names "Darocur Series 1173, 4265," and "Irgacure Series 184, 369, 500, 651, 784, 819, 907, 1300, 1700, 1800, 1850, 2959."

[0079] The photocationic polymerization initiator is not particularly limited, and known ones can be used, and examples of commercially available products include those manufactured by UCC under the trade names "Syracure UVI-6990, 6974", those manufactured by ADEKA CORPORATION under the trade names "ADEKA OPTOMER SP-150, 152, 170, 172", those manufactured by Rhodia under the trade name "Photoinitiator 2074", those manufactured by Chiba Specialty Corporation under the trade name "Irgacure 250", and those manufactured by Midori Chemical Industry Co., Ltd. under the trade name "DTS-102".

[0080] Preferred polymerization initiators for anionic, coordination and living polymerization include nC 4 H 9 Li, tC 4 H 9 Li-R 3 Examples of the metal include an alkyl compound of an alkali metal such as Al, an aluminum compound, and a transition metal compound.

[0081] 7) Hardener The curing agent preferably includes at least one selected from the group consisting of a polyphenylene ether oligomer having at least two hydroxyl groups, an active ester curing agent, and an alkyl ether having at least two hydroxyl groups. When the adhesive (1) contains a cyclic ether, which is a cyclic compound having an ether bond, as a constituent element, the adhesive (1) may contain a curing agent as a constituent element. Preferred examples of the curing agent are shown below.

[0082] Amine-based hardeners include diethylenetriamine, triethylenetetramine, tetraethylenepentamine, o-xylenediamine, m-xylenediamine, p-xylenediamine, trimethylhexamethylenediamine, 2-methylpentamethylenediamine, diethylaminopropylamine, isophoronediamine, 1,3-bisaminomethylcyclohexane, bis(4-amino-3-methylcyclohexyl)methane, bis(4-aminocyclohexyl)methane, norbornene diamine, 1,2 -diaminocyclohexane, 3,9-dipropanamine-2,4,8,10-tetraoxaspiro[5,5]undecane, 4,4'-diaminodiphenylmethane, 4,4'-diamino-1,2-diphenylethane, o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylsulfone, polyoxypropylenediamine, polyoxypropylenetriamine, polycyclohexylpolyamine, and N-aminoethylpiperazine.

[0083] Examples of acid anhydride curing agents include tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylhexahydrophthalic anhydride, methylnadic anhydride, hydrogenated methylnadic anhydride, trialkyltetrahydrophthalic anhydride, methylcyclohexenetetracarboxylic dianhydride, phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, benzophenonetetracarboxylic dianhydride, ethylene glycol bisanhydrotrimethylate, glycerin bis(anhydrotrimellitate) monoacetate, dedecenylsuccinic anhydride, and chlorendic anhydride.

[0084] Examples of phenol-based curing agents include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 2,5-xylenol, 2,6-xylenol, 3,4-xylenol, 3,5-xylenol, m-ethylphenol, p-ethylphenol, 2,3,5-trimethylphenol, 2,3,6-trimethylphenol, o-isopropylphenol, p-tert-butylphenol, o-sec-butylphenol, p-octylphenol, 2,6-di-tert-butylphenol, resorcinol, 1-naphthol, 2-naphthol, bisphenol A, phenol novolac, xylylene novolac, and bisphenol A novolac. In addition to the above, the curing agents described in JP-A-2004-256687, JP-A-2002-226550, etc. can also be used.

[0085] The active ester curing agent is not particularly limited, and known active ester curing agents can be used. Examples of commercially available products include an active ester compound containing a dicyclopentadiene-type diphenol structure, manufactured by DIC Corporation under the trade name "HPC-8000H-65T," an active ester compound containing a naphthalene structure, manufactured by DIC Corporation under the trade name "EXB-8150-65T," an active ester compound containing an acetylated product of phenol novolac, manufactured by Mitsubishi Chemical Corporation under the trade name "DC808," an active ester compound containing a benzoylated product of phenol novolac, manufactured by Mitsubishi Chemical Corporation under the trade name "YLH1026," an active ester curing agent which is an acetylated product of phenol novolac, manufactured by Mitsubishi Chemical Corporation under the trade name "DC808," and an active ester curing agent which is a benzoylated product of phenol novolac, manufactured by Mitsubishi Chemical Corporation under the trade name "YLH1026."

[0086] In addition, examples of the curing accelerator include cycloamidine compounds such as 1,8-diazabicyclo[5.4.0]-7-undecene (DBU), 1,5-diazabicyclo[4.3.0]-5-nonene, and 5,6-dibutylamino-1,8-diazabicyclo[5.4.0]-7-undecene; and the like, when added to the cycloamidine compounds, maleic anhydride, 1,4-benzoquinone, 2,5-toluquinone, 1,4-naphthoquinone, 2,3-dimethylbenzoquinone, 2,6-dimethylbenzoquinone, and 2,3-dimethoxy-5-methylbenzoquinone. quinone compounds such as phenyl-1,4-benzoquinone, 2,3-dimethoxy-1,4-benzoquinone, and the like, compounds having intramolecular polarization obtained by adding compounds having a π bond such as diazophenylmethane and phenol resin; tertiary amine compounds such as benzyldimethylamine, triethanolamine, dimethylaminoethanol, and tris(dimethylaminomethyl)phenol; derivatives of the tertiary amine compounds; 2-methylimidazole, 2-phenylimidazole, 2-phenylimidazole, derivatives of the imidazole compounds; organic phosphine compounds such as tributylphosphine, methyldiphenylphosphine, triphenylphosphine, tris(4-methylphenyl)phosphine, diphenylphosphine, and phenylphosphine; phosphorus compounds having intramolecular polarization obtained by adding a compound having a π bond such as maleic anhydride, the above-mentioned quinone compounds, diazophenylmethane, and a phenol resin to the organic phosphine compounds; tetraphenylboron salts such as tetraphenylphosphonium tetraphenylborate, triphenylphosphine tetraphenylborate, 2-ethyl-4-methylimidazole tetraphenylborate, and N-methylmorpholine tetraphenylborate; derivatives of the tetraphenylboron salts; and adducts of phosphine compounds such as triphenylphosphonium-triphenylborane and N-methylmorpholine tetraphenylphosphonium-tetraphenylborate with the tetraphenylboron salts.

[0087] The crosslinking agent may contain a polymerizable compound having three or more functionalities. Three-dimensional crosslinking is expected to improve the glass transition temperature, reduce the dielectric tangent, and improve the mechanical strength. Examples of crosslinking agents having three or more functionalities include isocyanuric acid derivatives having 0 to 3 epoxy groups and 3 to 0 allyl groups, tetraglycidyldiaminodiphenylmethane (TGDDM), and TECHMORE VG3101L (trade name) manufactured by Printec Co., Ltd.

[0088] 8) Organic Solvents The adhesive (1) may contain an organic solvent. The adhesive (1) may be cured in an organic solvent or without a solvent. The adhesive (1) containing an organic solvent may be applied to a low dielectric substrate by spin coating or the like, and then the organic solvent may be removed before photocuring. After photocuring, the adhesive may be heated to an appropriate temperature for post-treatment by thermal curing.

[0089] Preferred organic solvents include benzene, toluene, xylene, mesitylene, hexane, heptane, octane, nonane, decane, tetrahydrofuran, γ-butyrolactone, N-methylpyrrolidone, N,N-dimethylformamide, dimethylsulfoxide, cyclohexane, methylcyclohexane, cyclopentanone, cyclohexanone, 2-methoxy-1-methylethyl acetate (propylene glycol methyl ether acetate: PGMEA), etc. The above organic solvents may be used alone or in combination of two or more. It is not particularly meaningful to limit the proportion of the organic solvent used during curing, and the proportion may be determined for each individual case, taking into consideration the curing efficiency, solvent cost, energy cost, and the like.

[0090] The adhesive (1) of the present invention preferably contains 70 wt% or less of an organic solvent based on the total weight, and is particularly preferably a solvent-free composition. A solvent-free composition is a composition that can be prepared into a varnish-like form that maintains fluidity at room temperature without using an organic solvent, or that exhibits high fluidity when melted. By using a composition that contains 70 wt% or less of an organic solvent based on the total weight, or a solvent-free composition, the concentration of the cured product is increased, and the function of the cured product can be effectively expressed. The adhesive (1) before curing is in a liquid state at around room temperature and retains its fluidity, and can be used as is as a varnish containing no solvent or 70 wt% or less of an organic solvent based on the total weight. In other words, it can be used as is for applications such as coating or adhesion, and does not require a process of volatilizing the solvent at high temperature. In addition, examples of organic solvents that can be used here include acetone, methyl ethyl ketone, toluene, xylene, methyl isobutyl ketone, ethyl acetate, ethylene glycol monomethyl ether, N,N-dimethylformamide, methanol, ethanol, etc., which are relatively less toxic from the viewpoint of environmental load. The adhesive (1) of the present invention is capable of forming a high adhesive layer and has high heat resistance in a non-organic solvent system, and therefore can provide insulating materials for various electronic components used in the electronic device of the present invention, such as laminates for printed wiring boards, interlayer insulating materials for boards, adhesive films, semiconductor sealants, and conductive adhesives.

[0091] 9) Non-polymerizable liquid crystal compounds The adhesive (1) may contain a liquid crystal compound without a polymerizable group as a component. Examples of such non-polymerizable liquid crystal compounds are listed in LiqCryst, a database of liquid crystal compounds (LCI Publisher GmbH, Hamburg, Germany). By curing the adhesive (1) containing the non-polymerizable liquid crystal compound, a composite material of a polymer of the compound (1) and the non-polymerizable liquid crystal compound can be obtained. In such a composite material, for example, the non-polymerizable liquid crystal compound exists in a polymer network such as a polymer-dispersed liquid crystal.

[0092] 10) Inorganic fillers and fibrous reinforcing agents An inorganic filler can be added to the adhesive (1) in order to improve thermal conductivity, improve mechanical strength, adjust viscosity, etc. In this specification, the inorganic filler may be referred to as inorganic filler. In order to suppress dielectric loss, the silica may be a silicon oxide compound such as spherical silica, pulverized silica, hollow silica, or fumed silica, a metal oxide such as magnesium oxide, zinc oxide, or titanium oxide, or a metal salt such as potassium titanate. Spherical silica, hollow silica, magnesium oxide, or potassium titanate is preferable, and hollow silica is more preferable. The adhesive (1) of the present invention used for bonding low dielectric electronic substrates and resin parts can use a fibrous reinforcing agent as a fibrous or whisker-like filler to increase the strength of the adhesive layer formed by curing the adhesive (1). Preferred are inorganic fibers such as glass cloth, low dielectric glass cloth, carbon fiber, carbon nanotubes, and graphene, and inorganic whiskers such as silicate whiskers, alumina whiskers, magnesium oxide whiskers, zinc oxide whiskers, and aluminum nitride whiskers, and more preferred are low dielectric glass cloth, aluminum oxide whiskers, and aluminum nitride whiskers. In order to increase the mechanical strength, it is preferable to have a large amount of filler, but if there is too much, the resin may not be able to fill the gaps in the filler. Also, if there is too much resin, the effect of increasing the mechanical strength may not be achieved. In addition, since increasing the filler tends to increase the dielectric constant and decrease the dielectric tangent, it is preferable to determine the composition while balancing the two. In addition to inorganic fibers, organic fibers can also be used. Examples of organic fibers with high mechanical strength include polyamide fibers, aramid fibers, polyparaphenylene benzobisoxazole fibers, and liquid crystalline polyester fibers. Since organic fibers are lighter than inorganic fibers, they are preferable as fibrous reinforcing agents used in adhesives (1) for bonding low-dielectric electronic boards of portable devices. Fillers with high thermal conductivity may be metal nitrides such as powdered aluminum nitride, boron nitride, silicon nitride, etc., carbides such as diamond, graphite, silicon carbide, etc., metal oxides such as magnesium oxide, aluminum oxide, zinc oxide, silicon oxide, titanium oxide, tin oxide, holmium oxide, calcium oxide, etc., metal hydroxides such as magnesium hydroxide, aluminum hydroxide, etc., and silicate compounds such as cordierite or mullite, and metal fillers such as gold, silver, copper, platinum, iron, tin, lead, nickel, aluminum, magnesium, tungsten, molybdenum, and stainless steel. Preferably, boron nitride and silicon oxide, which have a low dielectric constant, are preferred, and in particular, hexagonal boron nitride (h-BN) is preferred because it has a low dielectric constant and high thermal conductivity. The more inorganic filler is used, the higher the thermal conductivity, etc., but generally, inorganic fillers have a high relative dielectric constant and a small dielectric tangent compared to resin components, so the dielectric constant increases when the filling amount is increased. Therefore, it is preferable to fill the required amount within a range that does not exceed the desired dielectric constant. The adhesive (1) of the present invention has high transparency and low dielectric constant, and when used for low refractive index optical materials, the refractive index can be adjusted by adding powders of hollow silica, spherical silica, titanium oxide, zirconium oxide, etc.

[0093] The shape of the filler may be spherical, amorphous, fibrous, whisker-like, cylindrical, plate-like, etc. The type, shape, size, and amount of the filler may be appropriately selected depending on the purpose. When the adhesive layer obtained by curing the adhesive (1) requires insulation, the filler may be conductive as long as it maintains the desired insulation, mechanical strength, dielectric constant, and dielectric loss.

[0094] The average particle size of the spherical or irregular filler is preferably 0.1 to 200 μm. More preferably, it is 1 to 100 μm. If it is 0.1 μm or more, the thermal conductivity is good, and if it is 200 μm or less, the filling rate can be increased. As for the fibrous filler, the longer the fiber length, the higher the tensile strength is, but it may not be possible to knead or disperse it, so it is preferable to select it according to the application. When dispersing, the average particle size of the fibrous filler is preferably 0.01 to 200 μm. More preferably, it is 0.1 to 100 μm. If it is 0.01 μm or more, the thermal conductivity is good, and if it is 200 μm or less, the mechanical strength can be increased. The amount of filler is preferably 20 to 95 wt% in the adhesive layer after the adhesive (1) has hardened. More preferably, it is 50 to 95 wt%. If it is 20 wt% or more, the thermal conductivity becomes high, which is preferable. If it is 95 wt% or less, the adhesive layer does not become brittle, which is preferable.

[0095] As the filler, commercially available products that have been surface-treated, such as affinity-treated, adhesion-facilitating, dispersing, waterproofing, etc., may be used as they are, or the commercially available products from which the surface treatment agents have been removed may be used. Also, untreated fillers may be used after being treated with a silane coupling agent, affinity agent, surface tension adjuster, anti-settling agent, anti-aggregation agent, etc.

[0096] 11) Other additives Since the compound (1) and the adhesive (1) have high polymerizability, a stabilizer may be added to the adhesive (1) to facilitate handling. As such a stabilizer, any known stabilizer can be used without limitation, and examples thereof include hydroquinone, 4-ethoxyphenol, and 3,5-di-t-butyl-4-hydroxytoluene (BHT). In applications requiring a low dielectric tangent (low tan δ) and a high glass transition temperature, it is preferable to add a crosslinking agent. The crosslinking agent is preferably one that chemically bonds with the polymerizable group of the compound (1) having a polymerizable group at its end used in the present invention to form a three-dimensional crosslink.

[0097] In order to adjust the properties of the cured product, the adhesive (1) of the present invention may contain other resins that do not react with the compound (1) used in the present invention. Examples of such resins include polyphenylene ether resins (PPE resins), polystyrene resins, polycarbonate resins, polyimide resins, polyamide resins, polyester resins, polybutadiene copolymers, polyvinyl acetal resins, natural rubber, synthetic rubber, synthetic elastomers, epoxy resins that have a different skeleton from the liquid crystal compound of the compound (1) used in the present invention, oxetane resins, acrylic resins, methacrylic resins, maleimide resins, oxazine resins, and oxazoline resins. In particular, when dielectric properties are important, polyphenylene ether resins (PPE resins), polystyrene resins, and polycarbonate resins are preferred. There are unreacted sites in these resins, which may react with the compound (1) used in the present invention, but in that case, a cross-linked structure is formed, so that the properties can be expected to be improved compared to when the reaction is not complete.

[0098] 12) The adhesive layer formed by hardening the adhesive (1) The adhesive layer formed by curing the adhesive (1), which is another embodiment of the present invention, has a low dielectric constant because it is a cured product of the adhesive (1), and is also excellent in thermal conductivity, heat resistance, rigidity, elasticity, molding flow, chemical resistance, dimensional stability, and the like.

[0099] When the adhesive layer formed by curing adhesive (1) exhibits liquid crystallinity, the molecular orientation can be controlled by an orientation treatment prior to curing. The dielectric constant and thermal conductivity exhibit anisotropy depending on the molecular orientation direction. When designing the dielectric constant and thermal design of low-dielectric electronic substrates, more advanced material design becomes possible, such as designing the area directly below the heat-generating IC to have high thermal conductivity in the thickness direction, and orienting the area other than directly below the IC in the lateral direction to spread the heat over a wide area. The orientation method can be controlled by the following methods. Methods for controlling the alignment of the mesogen moieties of the liquid crystal molecules in the adhesive (1) include a method of treating the inorganic filler surface with a silane coupling agent or an alignment agent having alignment ability, and a method of aligning by the self-alignment restraining force of the adhesive (1) itself. These methods may be performed alone or in combination of two or more. The alignment state controlled by such an alignment control method may be homogeneous, twisted, homeotropic, hybrid, bend, or spray alignment, and may be appropriately determined depending on the application and the alignment control method. In addition, during film formation or molding, shear stress may be applied to the liquid crystal state before curing to physically align it.

[0100] The orientation temperature is in the range of room temperature to 250°C, preferably room temperature to 200°C, more preferably room temperature to 180°C. The heat treatment time is in the range of 5 seconds to 2 hours, preferably 10 seconds to 60 minutes, more preferably 20 seconds to 30 minutes. If the heat treatment time is shorter than the above range, the temperature of the layer made of the adhesive (1) may not be raised to a predetermined temperature, and if it is longer than the above range, the productivity may decrease. Note that the above heat treatment conditions vary depending on the type and composition ratio of the components used in the adhesive (1), the presence or absence and the content of the polymerization initiator, etc., and therefore only show approximate ranges. In particular, if the temperature is higher than the polymerization initiation temperature of the polymerizable component used in the adhesive (1), the adhesive will harden before it is oriented, and an adhesive layer in which the molecular chains are oriented in a certain direction cannot be obtained.

[0101] The curing method (polymerization method) of the adhesive (1) includes radical polymerization of polymerizable groups (polymerizable components), anionic polymerization, cationic polymerization, and coordination polymerization. However, to fix the molecular arrangement or the helical structure, thermal polymerization or photopolymerization using light or heat such as electron beams, ultraviolet rays, visible light, or infrared rays (heat rays) is suitable. Thermal polymerization is preferably carried out in the presence of a radical polymerization initiator, and photopolymerization is preferably carried out in the presence of a photoradical polymerization initiator. A polymer in which the arrangement of liquid crystal molecules is fixed can be obtained by a polymerization method in which ultraviolet rays or an electron beam are irradiated in the presence of a photoradical polymerization initiator. The obtained polymer may be a homopolymer, a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer, and may be appropriately selected depending on the application.

[0102] When the orientation of the adhesive (1) is fixed by photopolymerization, ultraviolet light or visible light is usually used. The wavelength of the light used for light irradiation is in the range of 150 to 500 nm, preferably 250 to 450 nm, and more preferably 300 to 400 nm. Examples of light sources for light irradiation include low-pressure mercury lamps (germicidal lamps, fluorescent chemical lamps, black lights), high-pressure discharge lamps (high-pressure mercury lamps, metal halide lamps), short arc discharge lamps (ultra-high-pressure mercury lamps, xenon lamps, mercury xenon lamps), ultraviolet light-emitting diodes, and the like. Among these, metal halide lamps, xenon lamps, ultraviolet light-emitting diodes, and high-pressure mercury lamps are preferred.

[0103] A filter or the like may be placed between the light source and the adhesive (1) to allow only a specific wavelength range to pass, thereby selecting the wavelength range of the irradiation light source. The amount of light emitted from the light source is 2 to 5000 mJ / cm. 2 , preferably 10 to 3000 mJ / cm 2 , more preferably 100 to 2000 mJ / cm 2 The temperature condition during the light irradiation is preferably set to the same range as the above-mentioned heat treatment temperature.

[0104] Conditions for fixing the orientation of the adhesive (1) by thermal polymerization include a heat curing temperature in the range of room temperature to 350°C, preferably room temperature to 250°C, and more preferably 50°C to 200°C, and a curing time in the range of 5 seconds to 10 hours, preferably 1 minute to 5 hours, and more preferably 5 minutes to 1 hour. After curing, it is preferable to slowly cool the product to suppress stress distortion, etc. Also, a reheating treatment may be performed to relieve distortion, etc.

[0105] The orientation of the cured product or the adhesive (1) in the curing process that has been orientation-controlled as described above may be further controlled in any direction by a mechanical operation such as stretching. The isolated polymer (1) may be dissolved in an organic solvent together with other components to prepare an adhesive (1), which may then be aligned and cured on an alignment-treated substrate to be processed into a film or the like. In this case, two polymers may be mixed and processed, or multiple polymers may be laminated. As the organic solvent, N-methyl-2-pyrrolidone, dimethyl sulfoxide, N,N-dimethylacetamide, N,N-dimethylformamide, N,N-dimethylacetamide dimethyl acetal, tetrahydrofuran, chloroform, 1,4-dioxane, bis(methoxyethyl)ether, γ-butyrolactone, tetramethylurea, trifluoroacetic acid, ethyl trifluoroacetate, hexafluoro-2-propanol, 2-methoxyethyl acetate, methyl ethyl ketone, cyclopentanone, cyclohexanone, and the like are preferred. These may be mixed with a small amount of a general organic solvent such as acetone, benzene, toluene, heptane, or methylene chloride.

[0106] When a highly linear adhesive (1) exhibits a liquid crystal phase in a very narrow range, if the crystallinity is high, it forms domains with axes aligned in a certain direction, resulting in a higher thermal conductivity in the orientation direction compared to polymerizable compounds such as bisphenol A structures. Orientation and crystallinity can also be controlled by slowly curing from an isotropic liquid state with the surface of a polymer sheet with aligned orientation or crystalline resin filler present as a core for crystal growth. However, if the crystallinity is made too high, flexibility tends to decrease, so it is necessary to use an adhesive (1) with appropriate crystallinity.

[0107] 13) A laminate obtained by bonding a low dielectric electronic substrate and a metal foil or a resist layer with the adhesive (1) A laminate obtained by bonding a low dielectric electronic substrate and a metal foil or a resist layer using the adhesive (1) of the present invention is a laminate containing an adhesive layer that is a cured product of the adhesive (1), and can also be used as a film-shaped, sheet-shaped, plate-shaped, fibrous, or three-dimensional electronic component. When used in a thin film, film, sheet, plate, fiber, or three-dimensional laminate, the preferred shapes are a film and a thin film. A film and a thin film can be obtained by applying the adhesive (1) to a low dielectric electronic substrate or the like and curing the applied adhesive. Alternatively, the adhesive (1) containing an organic solvent can be applied to an orientation-treated low dielectric electronic substrate and cured after removing the organic solvent. In this specification, the thickness of the sheet is 1 mm or more, the thickness of the film is 5 μm or more and less than 1 mm, preferably 10 to 500 μm, and more preferably 20 to 300 μm, and the thickness of the thin film is less than 5 μm.

[0108] Hereinafter, a method for producing a film as a laminate using the adhesive (1) containing an organic solvent will be specifically described. First, the adhesive (1) is applied onto a release-treated low dielectric electronic substrate, and the organic solvent is dried and removed to form a coating layer with a uniform thickness. Coating methods include spin coating, roll coating, curtain coating, flow coating, printing, microgravure coating, gravure coating, wire bar coating, dip coating, spray coating, and meniscus coating.

[0109] The organic solvent can be removed by drying at room temperature, drying on a hot plate, drying in a drying oven, blowing warm or hot air, or the like. The conditions for removing the organic solvent are not particularly limited, and the coating layer may be dried until the organic solvent is mostly removed and the fluidity of the coating layer disappears. Depending on the type and composition ratio of the compound used in the adhesive (1), the molecular orientation of the liquid crystal molecules in the coating layer may be completed during the drying process. In such a case, the coating layer that has been subjected to the drying process can be subjected to the polymerization process (curing process) without passing through the above-mentioned heat treatment process. However, in order to make the orientation of the liquid crystal molecules in the coating layer more uniform, it is preferable to heat the coating layer that has been subjected to the drying process to a liquid crystal phase expression temperature to align it in the liquid crystal state, and then fix the orientation by photopolymerization or thermal polymerization treatment.

[0110] In addition, when using the adhesive (1), it is also preferable to perform an alignment treatment on the surface of the low dielectric electronic substrate before coating. The alignment treatment method may be a method of simply forming an alignment film on the substrate, a method of forming an alignment film on the low dielectric electronic substrate and then rubbing the substrate with a rayon cloth, a method of directly rubbing the low dielectric electronic substrate with a rayon cloth, a method of obliquely depositing silicon oxide, a method of rubbing free alignment using a stretched film, a photoalignment film, or an ion beam, etc. In addition, there are cases where a desired alignment state can be formed without performing a treatment on the surface of the low dielectric electronic substrate. In many cases, a surface treatment such as a rubbing treatment is not performed when forming a homeotropic alignment, but a rubbing treatment may be performed in order to achieve a higher alignment. In addition, in a normal coating method, a shear stress in a direction parallel to the substrate is applied to the adhesive solution, so that in the absence of any treatment, the liquid crystal molecules are often weakly aligned in a direction parallel to the substrate.

[0111] The alignment film is not particularly limited as long as it can control the alignment of the adhesive (1), and any known alignment film can be used, and for example, polyimide, polyamide, polyvinyl alcohol, alkylsilane, alkylamine or lecithin-based alignment films are suitable. In the case of vertical alignment, a silane coupling agent is also suitable.

[0112] Any method can be used for the rubbing treatment. Usually, a method is used in which a rubbing cloth made of a material such as rayon, cotton, or polyamide is wrapped around a metal roll and the like, and the roll is moved while rotating in a state in which the roll is in contact with the low dielectric electronic substrate or the alignment film, or a method is used in which the roll is fixed and the low dielectric electronic substrate is moved.

[0113] In order to obtain a more uniform alignment, an alignment control additive may be contained in the adhesive (1). Examples of such alignment control additives include imidazoline, quaternary ammonium salts, alkylamine oxides, polyamine derivatives, polyoxyethylene-polyoxypropylene condensates, polyethylene glycol and its esters, sodium lauryl sulfate, ammonium lauryl sulfate, lauryl sulfate amines, alkyl-substituted aromatic sulfonates, alkyl phosphates, aliphatic or aromatic sulfonic acid formalin condensates, lauryl amidopropyl betaine, lauryl aminoacetate betaine, polyethylene glycol fatty acid esters, polyoxyethylene alkylamines, perfluoroalkyl sulfonates, perfluoroalkyl carboxylates, perfluoroalkyl ethylene oxide adducts, perfluoroalkyl trimethyl ammonium salts, oligomers having perfluoroalkyl and hydrophilic groups, oligomers having perfluoroalkyl and lipophilic groups, urethanes having perfluoroalkyl, and organosilicon compounds having primary amino groups (alkoxysilane type, linear siloxane type, and three-dimensional condensation type silsesquioxane type organosilicon compounds).

[0114] Examples of the low dielectric electronic substrate include plastic film substrates and glass-reinforced resin substrates such as polyimide, polyamideimide, polyamide, polyetherimide, polyetheretherketone, polyetherketone, polyketone sulfide, polyethersulfone, polysulfone, polyphenylene sulfide, polyphenylene oxide, polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyacetal, polycarbonate, polyarylate, acrylic resin, polyvinyl alcohol, polypropylene, cellulose, triacetyl cellulose or a partially saponified product thereof, epoxy resin, phenol resin, and norbornene resin, as well as glass substrates such as alkali glass, borosilicate glass, and flint glass; metal substrates such as aluminum, iron, and copper; and inorganic substrates such as silicon.

[0115] The film substrate may be a uniaxially stretched film or a biaxially stretched film. The film substrate may be previously subjected to a surface treatment such as saponification, corona treatment, or plasma treatment. A protective layer that is not affected by the organic solvent contained in the adhesive (1) may be formed on the film substrate. An example of a material used for the protective layer is polyvinyl alcohol. Furthermore, an anchor coat layer may be formed to enhance adhesion between the protective layer and the low dielectric electronic substrate made of the film substrate. Such an anchor coat layer may be made of either an inorganic or organic material as long as it enhances adhesion between the protective layer and the low dielectric electronic substrate made of the film substrate.

[0116] 14) Electronic components and devices A laminate obtained by bonding a low dielectric electronic substrate and a metal foil or a resist layer using the adhesive of the present invention can be used as various electronic components. Furthermore, various electronic components obtained using the adhesive of the present invention are useful for applications as various electronic devices.

[0117] [Manufacturing method] Hereinafter, a method for producing the adhesive of the present invention for bonding low dielectric electronic substrates, and a method for producing a laminate obtained by bonding a low dielectric electronic substrate and a metal foil or a resist layer using the adhesive, and an electronic device of the present invention will be specifically described.

[0118] The adhesive of the present invention can be used as a semi-cured solid adhesive sheet, or as a liquid adhesive in a temperature range where the adhesive exhibits a liquid crystal phase or an isotropic phase, or can be dissolved in an organic solvent to be used as a liquid adhesive in the form of a solution or slurry. The adhesive is prepared by adding an organic solvent, an inorganic filler, the above-mentioned various additives, etc. to a bifunctional or higher polymerizable liquid crystal compound and a curing component as necessary, and stirring and degassing the mixture using a stirrer until there is no compositional unevenness. For example, a rotation-revolution mixer is used to stir the mixture at a rotation speed of 2000 rpm for 10 minutes, and then degassing the mixture at a rotation speed of 2200 rpm for 10 minutes. In addition to the rotation-revolution mixer, a stirring motor, a mortar, a three-roll mill, a ball mill, a rotation-revolution mill, a planetary mill, a bead mill, a jet mill, etc. can be used to disperse the mixture.

[0119] A method for producing a laminate or an electronic device of the present invention by bonding a low dielectric electronic substrate and a metal foil or a resist layer using the adhesive of the present invention will be described below. In order to bond a low dielectric electronic substrate to a metal foil or a resist layer, the adhesive of the present invention is applied to the surfaces where the low dielectric electronic substrate and the metal foil or the resist layer are to be bonded. The adhesive may be applied to all of the surfaces to be bonded, or to only one of the surfaces, for example, the surface of the low dielectric electronic substrate to be bonded, and not to the surface where the metal foil or the resist layer is to be bonded. For the application method of the adhesive to the surfaces to be bonded, it is preferable to use a wet coating method in order to uniformly coat the adhesive of the present invention for the low dielectric electronic substrate. Among the wet coating methods, when the laminate or the electronic device of the present invention is produced in small quantities, a spin coating method that can easily form a homogeneous film is preferable. When productivity is important, gravure coating, die coating, bar coating, reverse coating, roll coating, slit coating, dipping, spray coating, kiss coating, reverse kiss coating, air knife coating, curtain coating, inkjet printing, flexographic printing, screen printing, rod coating, etc. are preferable. The wet coating method can be appropriately selected from these methods depending on the required film thickness, viscosity, curing conditions, etc. On the other hand, if you want to print the adhesive only in the necessary areas, you can adjust the viscosity by adjusting the amount of organic solvent or silica, and pattern it using the inkjet method, flexographic printing method, screen printing method, or dispenser method. The adhesive of the present invention is used to apply the adhesive to the surfaces to be bonded, and then the low dielectric electronic substrate and the metal foil or resist layer are bonded together by a known method to produce a laminate or the electronic device of the present invention.

[0120] When manufacturing an adhesive sheet that is a solid adhesive, a resin molding method such as a cast molding method can be used in which the liquid adhesive is coated on a release-treated substrate using the above-mentioned application method and then peeled off. A transferable adhesive sheet can also be formed by semi-curing the adhesive using the cast molding method. Using the obtained adhesive sheet, a low-dielectric electronic substrate and a metal foil or resist layer can be bonded together using a known method (see, for example, "The Easy Book of Printed Wiring Boards, 2nd Edition, Nikkan Kogyo Shimbun, 2018, p.106") to manufacture a laminate or the electronic device of the present invention. EXAMPLES

[0121] The present invention will be described in more detail by way of examples (including production examples of compounds, adhesives, polymers (cured products), laminates, etc.). The present invention is not limited by these examples.

[0122] [Synthesis Example of Compound (1)] Compound (1) was synthesized according to the procedures shown in Synthesis Example 1 and other synthesis examples. Unless otherwise specified, the reaction was carried out under a nitrogen atmosphere. The synthesized compound was identified by methods such as NMR analysis. The properties of Compound (1), the adhesive, the polymer (cured product), the laminate, etc. were measured by the following methods.

[0123] [NMR Analysis] For the measurement, JNM-ECZR manufactured by JEOL Ltd. was used. 1 In the measurement of 1H-NMR, the sample was dissolved in a deuterated solvent such as CDCl 3 and the measurement was carried out at room temperature under the conditions of 500 MHz and 16 integration times. Tetramethylsilane was used as an internal standard. 19 In the measurement of 19F-NMR, CFCl 3 was used as an internal standard and the measurement was carried out under the condition of 32 integration times. In the description of the nuclear magnetic resonance spectrum, s means singlet, d means doublet, t means triplet, q means quartet, quin means quintet, sex means sextet, m means multiplet, and br means broad.

[0124] [Gas Chromatography Analysis] For the measurement, a GC-2014 gas chromatograph manufactured by Shimadzu Corporation was used. As the column, a capillary column DB-1 (length 30 m or 15 m, inner diameter 0.25 mm, film thickness 0.25 μm) manufactured by Agilent Technologies Inc. (currently: Keysight Technologies, Inc.) was used. Nitrogen (1 ml / min) was used as the carrier gas. The temperature of the sample vaporization chamber was set at 300 °C, and the temperature of the detector (FID) part was set at 300 °C. The sample was dissolved in an appropriate solvent such as acetone and prepared into a 1 wt% solution, and 1 μl of the obtained solution was injected into the sample vaporization chamber. As the recorder, a GCSolution system manufactured by Shimadzu Corporation or the like was used.

[0125] <HPLC Analysis> For the measurement, a Prominence (LC-20AD; SPD-20A) manufactured by Shimadzu Corporation was used. As the column, a YMC-Pack ODS-A (length 150 mm, inner diameter 4.6 mm, particle size 5 μm) manufactured by WMC Co., Ltd. was used. The eluent was prepared by appropriately mixing methanol / water or acetonitrile / water. As the detector, a UV detector, an RI detector, a CORONA detector, etc. were appropriately used. When a UV detector was used, the detection wavelength was set at 210 - 254 nm. The sample was dissolved in methanol or acetonitrile and prepared into a 0.1 wt% solution, and 1 μL of this solution was introduced into the sample chamber. As the recorder, a C-R7Aplus manufactured by Shimadzu Corporation was used.

[0126] <Ultraviolet-Visible Spectrophotometric Analysis> For the measurement, a PharmaSpec UV-1700 manufactured by Shimadzu Corporation was used. The detection wavelength was set from 190 nm to 700 nm. The sample was dissolved in acetonitrile and prepared into a 0.01 mmol / L solution, placed in a quartz cell (optical path length 1 cm), and measured.

[0127] <Measurement Sample> When measuring the transition temperature (clear point, melting point, polymerization initiation temperature, etc.) and, when the compound exhibits a liquid crystal phase, the phase structure, the compound itself was used as the sample.

[0128] (1) Transition temperature (℃) For the measurements, a high-sensitivity differential scanning calorimeter, X-DSC7000, manufactured by Hitachi High-Tech Science Co., Ltd. (formerly SII Nanotechnology Co., Ltd.) was used. The temperature of the sample was raised and lowered at a rate of 3 to 5°C / min, and the onset of the endothermic or exothermic peak associated with the phase change of the sample was extrapolated to determine the transition temperature. The melting point and polymerization initiation temperature of the compound were also measured using this device. When a compound exhibits a liquid crystal phase, the temperature at which the solid transitions to a liquid crystal phase such as a smectic phase or nematic phase is sometimes abbreviated as the "lower limit temperature of the liquid crystal phase." The temperature at which a compound transitions from a crystal to a liquid is sometimes abbreviated as the "clearing point."

[0129] Crystals were represented as C. When the types of crystals could be distinguished, they were represented as C1, C2, etc. When liquid crystal phases were present, smectic phases were represented as S and nematic phases as N. When smectic phases could be distinguished into smectic A, smectic B, smectic C, or smectic F, they were represented as SA, SB, SC, or SF, respectively. Liquids (isotropic phase) were represented as I. Transition temperatures were represented as, for example, "C 50.0 N 100.0 I." This indicates that the transition temperature from crystal to nematic phase is 50.0°C, and the transition temperature from nematic phase to liquid is 100.0°C.

[0130] (2) Phase structure When a compound exhibited a liquid crystal phase, the sample was placed on a hot plate (Mettler Toledo FP-52 hot stage) of a melting point measuring device equipped with a polarizing microscope. The sample was heated at a rate of 3°C / min, and the phase state and its change were observed under a polarizing microscope to identify the type of phase.

[0131] [Synthesis Example 1] Compound (S01: Compound (1), R 1a and R 1b are both formulas (PG-5), R b is hydrogen (multiple symbols are the same), q=0, A 1 and A 2 Both are 1,4-cyclohexylene, Z1 Ha-CH 2 O-, Z 2 is a single bond, Z 4 HA-OCH 2 -, m1=0) TIFF2024167588000020.tif15454,4'-Bicyclohexyldiol (S01-a) is commercially available, for example, from Fujifilm Wako Pure Chemical Industries, Ltd. This raw material was purified using a general method such as recrystallization filtration, and the trans isomer was isolated and used.

[0132] TIFF2024167588000021.tif20111Under a nitrogen atmosphere, 4,4'-dicyclohexanol (S01-a) (5.00 g, 25.3 mmol) was added to a solution of sodium hydride (55 wt%) (2.42 g, 55.56 mmol) in N,N-dimethylformamide (60 mL) at 10 ° C. After stirring this solution at 40 ° C for 30 minutes, epibromohydrin (10.4 g, 75.8 mmol) was added and the mixture was heated and stirred at 40 ° C for 3 days. The reaction mixture was slowly added to pure water and extracted with toluene (200 mL), the organic layer was washed three times with pure water, and the obtained organic layer was concentrated under reduced pressure. The obtained residue was purified by silica gel column chromatography (solvent: toluene / ethyl acetate = 4 / 1 (volume ratio)) to obtain compound (S01) (5.10 g, 16.5 mmol). The transition point of this compound (S01) was C 38.3 I (℃), and the polymerization initiation temperature was 137.1℃.

[0133] In addition, compound (S01) 1 The H-NMR signals were as follows: δ (ppm; CDCl 3 ):3.71-3.68(dd,2H), 3.46-3.42(dd,2H), 3.24-3.17(tt,2H), 3.14-3.10(m,2H), 2.79-2.78(dd,2 H), 2.60-2.59(dd,2H), 2.08-2.01(m,4H), 1.77-1.71(m,4H), 1.23-1.12(m,4H), 1.05-0.92(m,6H).

[0134] [Synthesis Example 2] Compound (S02: Compound (1), R 1a and R 1b are both formulas (PG-5), R b is hydrogen (multiple symbols are the same), q=0, A 1 and A 2 Both are 1,4-cyclohexylene, Z 1 Ha-(CH 2 ) 4 O-, Z 2 is a single bond, Z 4 is -O(CH 2 ) 4 -, m1=0) TIFF2024167588000022.tif1559 TIFF2024167588000023.tif411364,4'-Bicyclohexyldiol (S01-a) is commercially available, for example, from Fujifilm Wako Pure Chemical Industries, Ltd. This raw material was purified using a general method such as recrystallization filtration, and the trans isomer was isolated and used. 1-Bromo-6-hexene is commercially available, for example, from Fujifilm Wako Pure Chemical Industries, Ltd.

[0135] (Step 1) Synthesis of 2-(4-bromobutyl)oxirane Under a nitrogen atmosphere, metachloroperbenzoic acid (mCPBA) (70 wt%) (45.2 g, 184 mmol) was added little by little to a dichloromethane (200 mL) solution of 1-bromo-6-hexene (25.0 g, 153 mmol) at 25°C, and the mixture was stirred at room temperature for 3 hours. The reaction mixture was poured into pure water, extracted with dichloromethane (200 ml), and the organic layer was washed once with a saturated aqueous solution of sodium thiosulfate and twice with pure water, and the organic layer was concentrated under reduced pressure at 55°C and 0.01 MPa. The resulting residue was purified by silica gel column chromatography (solvent: dichloromethane) to obtain colorless liquid 2-(4-bromobutyl)oxirane (24.6 g, 138 mmol).

[0136] (Step 2) Synthesis of compound (S02) Compound (S02) (8.00 g, 20.35 mmol) was obtained by the same procedure as in [Synthesis Example 1], except that 2-(4-bromobutyl)oxirane (7.26 g, 40.6 mmol) obtained in the previous step was used instead of epibromohydrin. Compound (S02) was obtained by the same procedure as in [Synthesis Example 1], and was crystallized at -5°C when cooled. The polymerization initiation temperature was 200.0°C. In addition, compound (S02) 1 The H-NMR signals were as follows: δ (ppm; CDCl 3 ):3.40-3.37(dd,4H), 3.36-3.35(dd,2H), 3.07-3.02(tt,2H), 2.87-2.83(m,2H), 2.69-2.67(m,2H), 2.41-2 .39(dd,2H), 1.99-1.95(m,4H), 1.69-1.66(m,4H), 1.55-1.41(m,12H), 1.13-1.05(m,4H), 1.00-0.87(m,6H).

[0137] [Synthesis Example 3] Compound (S03: Compound (1-3), R 1a and R 1b are both formulas (PG-5), R b is hydrogen (multiple symbols are the same), q=0, Z 1 Ha-(CH 2 ) b O-, Z 2 is a single bond, Z 4 is -O(CH 2 ) b -, b=4, n=2, and X at positions 3 and 5 are both methyl) TIFF2024167588000024.tif2072 TIFF2024167588000025.tif41145

[0138] Synthesis of compound (S03-b) Under a nitrogen atmosphere, 6-bromo-1-hexene (17.1 g, 105 mmol) was added to a solution of 3,3',5,5'-tetramethyl-1,1'-biphenyl-4,4'-diol (S03-a) (10.0 g, 41.3 mmol), potassium carbonate (15.0 g, 109 mmol), and tetrabutylammonium bromide (TBAB) (4.0 g, 12.4 mmol) in N,N'-dimethylformamide (DMF) (200 mL) at room temperature, and the mixture was stirred at 60 ° C for 6 hours. The reaction mixture was added to pure water and extracted three times with toluene (200 mL). The combined organic layer was washed three times with pure water and once with brine, and then the organic layer was concentrated under reduced pressure at 40 ° C. The obtained residue was purified by silica gel column chromatography (solvent: heptane / ethyl acetate=9 / 1 (volume ratio)) to obtain compound (S03-b) (14.7 g, 36.0 mmol).

[0139] (Step 2) Synthesis of compound (S03) Under a nitrogen atmosphere, metachloroperbenzoic acid (mCPBA) (65wt%) (37.3g, 140.7mmol) was added little by little to a dichloromethane (200mL) solution of compound (S03-b) (13.0g, 32.0mmol) under ice cooling, and the mixture was stirred overnight while returning to room temperature. The reaction solution was added to a saturated aqueous sodium thiosulfate solution, and the aqueous layer was extracted twice with dichloromethane (200ml). The combined organic layer was washed once with a saturated aqueous sodium thiosulfate solution, once with pure water, and once with brine, and then the organic layer was concentrated under reduced pressure at 40°C. The resulting residue was purified by silica gel column chromatography (solvent: toluene / ethyl acetate = 9 / 1 (volume ratio)), and recrystallized from toluene / ethanol = 1 / 4 (volume ratio) to obtain compound (S03) (6.81g, 32.0mmol). The transition point of this compound (S03) was C 99.2 I (°C). The polymerization initiation temperature was 165°C. In addition, compound (S03) 1 The H-NMR signals were as follows: δ (ppm; CDCl 3):7.18(s,4H), 3.81-3.79(t,4H), 2.99-2.96(m,2H), 2.80-2.78(dd,2H), From 2.5 2-2.51(dd,2H), 2.32(s,12H), 1.92-1.86(m,4H), 1.76-1.60(m,8H).

[0140] [Physical property evaluation of adhesive properties (peel strength), dielectric properties (dielectric constant and dielectric tangent) and heat dissipation properties (thermal diffusivity)] [Example 1] <Preparation of samples for measuring adhesive properties and evaluation of adhesive properties> 0.31 g of a polymerizable compound (S01) as compound (1), which is a bifunctional or higher polymerizable liquid crystal compound, and polyphenylene ether oligomer (both terminal hydroxyl groups) manufactured by SABIC LLC, product name: Noryl, as a curing component (curing agent). TM 1.60 g of SA90-100 resin (mPPE) was weighed out and placed in a 20 mL screw tube bottle, and 3.0 g of toluene and 1.0 g of N-methylpyrrolidone were further added and dissolved at 80° C. This solution was left overnight in a laboratory with the temperature set at 25° C., and 2-ethyl-4-methylimidazole (trade name, manufactured by Tokyo Chemical Industry Co., Ltd.) was added as a curing component (curing accelerator) using a medicine spoon so that the amount was 2 wt % of the resin component, and mixed to obtain a solution that is an adhesive for low dielectric electronic substrates of the present invention. The adhesive solution for low dielectric electronic substrates of the present invention to which a curing catalyst had been added was applied to a finely roughened surface of a metal foil for high frequency substrates (manufactured by Furukawa Electric Co., Ltd., product name: FV-WS (thickness 18 μm)) cut into a 7 cm square, using a spin coater (rotation at 1000 rpm for 20 seconds) so that the thickness after drying would be approximately 5 μm, and the solvent was dried for 30 minutes on a hot plate set at 100° C. The copper foil with the adhesive component coating layer after drying was cut into 1 cm widths with a design cutter knife, cut into 5 cm squares, and placed on the center of a liquid crystal polymer film (manufactured by Chiyoda Integre Co., Ltd., product name, Pericure (registered trademark) LCP, 50 μm thick) which is a low dielectric film that was degreased and washed with acetone as a low dielectric electronic substrate as shown in FIG. 1, sandwiched between two 200 μm thick PTFE sheets manufactured by AS ONE Co., Ltd., and cured at 200 ° C. for 30 minutes at a pressure of 10 MPa using a small manual heating press manufactured by Imoto Manufacturing Co., Ltd. During the temperature rise, degassing was performed by releasing the pressure once every time the temperature increased by 20 ° C. from 100 ° C. In this way, a test piece of a laminate in which a low dielectric electronic substrate and a metal foil were bonded together by an adhesive layer, which is a cured product of the adhesive, was obtained using the adhesive of the present invention. The entire back surface of the completed test piece was covered with double-sided tape (Nichiban Co., Ltd., product name: Nicetack), and a 2 mm thick aluminum plate was bent as shown in Figure 2 and fixed to a homemade jig. The test piece was then attached to an autograph AGC-X (1 kN type) made by Shimadzu Corporation, and the 2 cm long copper foil with adhesive layer, which was a 2 cm part protruding from a 5 cm square low dielectric film, was pulled straight up at a speed of 50 mm / min to measure the adhesive properties (peel strength). In addition, the peel strength in the vertical direction was measured, but if the measurement length becomes too long, an angle will be created unless the stage on which the substrate is attached is moved, so the part with the smallest peel torque between 1 and 21 mm after the start of measurement was taken as the measurement value. The measurement results are specified as shown in Table 1.

[0141] [Table 1] Adhesive properties (peel strength) evaluation criteria table TIFF2024167588000026.tif31140

[0142] <Preparation of samples for dielectric property evaluation and evaluation of dielectric properties> The same adhesive solution as that used for the adhesive property evaluation was applied using a bar coater so that the dry film thickness was about 40 μm and the applied area was 8 cm square or more, and then dried for 30 minutes on a hot plate set at 100 °C. If the film thickness was insufficient, the application and drying were repeated several times. After drying, the sample was fixed to the bottom of a container through which nitrogen could flow using commercially available polyimide adhesive tape to prevent the sample from curling, and placed in a hot air oven with nitrogen flowing, and cured at 200 °C for 30 minutes. The hardened sample was stored in an electronic desiccator because it would absorb moisture if left in the air.

[0143] <Method of evaluating dielectric properties> The shift and attenuation of the resonant frequency of the dielectric property measurement sample were measured using a cavity resonator (TE mode 10 GHz) manufactured by AET, INC. connected to a vector network analyzer (MS46522B-043 manufactured by Anritsu Corporation), and the dielectric properties of the relative permittivity and dielectric tangent (tan δ) were calculated using the company's software. Since the film thickness has a large effect on the measurement accuracy, the total thickness of the prepared sample was measured at five points using a digimatic micrometer manufactured by Mitutoyo Corporation, and the average value was used for calculation. In order to reduce the effect of the moisture content in the sample during measurement, the sample was left in an electronic desiccator the night before, and on the day of measurement, the sample was left to stand for more than 60 minutes in a laboratory with a temperature of 20°C and a relative humidity of 48% RH, and then the measurement was started. Since the film thickness is large, the sample may curl due to cure shrinkage, but it was pressed flat so that it could be inserted into the resonator for measurement. Also, cracks may appear during this process, but if there are no gaps, this has almost no effect on the resonance method, so we continued with the measurement as is. Since these measured values ​​are the results for two layers, the polyimide film and the cured film, at the same time as making the sample, we also prepared only the polyimide film by heat treating it at 200°C for one hour, and used the measured values ​​of this polyimide film as the dielectric properties of the first layer to calculate the dielectric constant and dielectric tangent of just the cured film using the company's two-layer film calculation spreadsheet.

[0144] <Evaluation method for heat dissipation (thermal diffusivity)> The two-layer film for which the dielectric properties had been measured was folded to obtain a small piece of the cured material that had been peeled off from the polyimide film. The heat dissipation (thermal diffusivity) in the thickness direction of this small piece of cured material was measured using a thermal diffusivity measuring device, IPHASE Mobile Model 1, manufactured by IPHASE Corporation (this device can accurately measure thermal diffusivity on any surface that is 2 mm or more on a side, flat, and has parallel top and bottom surfaces).

[0145] [Example 2] A sample was prepared and evaluated in the same manner as in Example 1, except that 0.39 g of compound (S02), which is a polymerizable liquid crystal compound having two or more functionalities, was used as the polymerizable compound. The result is designated as Example 2.

[0146] [Example 3] A sample was prepared and evaluated in the same manner as in Example 1, except that 0.44 g of compound (S03), which is a polymerizable liquid crystal compound having two or more functionalities, was used as the polymerizable compound.

[0147] [Example 4] A sample was prepared and evaluated in the same manner as in Example 1, except that the curing component (curing accelerator) in Example 1 was changed to a phosphorus-based curing accelerator (manufactured by Hokko Chemical Industry Co., Ltd., product name: TBPLA) and added to the resin component to make it 3 wt%, silica powder (manufactured by Denka Co., Ltd., product name: Denka fused silica (DF) ultrafine particle spherical type SFP-130MC) was added as an inorganic filler to the resin component at 20 wt%, and a silane coupling agent (manufactured by JNC Co., Ltd., product name: Sila Ace S510) was added at 1 wt% relative to the solid content. The result is Example 4.

[0148] [Example 5] A sample was prepared and evaluated in the same manner as in Example 1, except that the curing component (curing accelerator) in Example 1 was changed to a phosphorus-based curing accelerator (trade name: TBPLA, manufactured by Hokko Chemical Industry Co., Ltd.) and added to the resin component so as to account for 3 wt % of the resin component, and boron nitride powder (trade name: Boron Nitride Powder (BN) PTX25, manufactured by Momentive Energy Supply Co., Ltd.), which is a nitride filler, was added as an inorganic filler to the resin component at 20 wt %. The result is Example 5.

[0149] [Example 6] A sample was prepared and evaluated in the same manner as in Example 1, except that the curing component (curing agent) in Example 1 was changed to 0.45 g of an active ester curing agent (manufactured by DIC Corporation under the trade name of HPC-8000H-65T) and the curing component (curing accelerator) was changed to a phosnium-based curing accelerator (manufactured by Hokko Chemical Industry Co., Ltd. under the trade name of TBP-3S) which was added to make up 3 wt % of the resin component. The results are shown as Example 6.

[0150] [Example 7] A sample was prepared and evaluated in the same manner as in Example 1, except that the curing component (curing accelerator) in Example 3 was changed to a phosphorus-based curing accelerator (manufactured by Hokko Chemical Industry Co., Ltd., product name: TBPLA) and added to the resin component at 3 wt %. The result is Example 6.

[0151] [Comparative Example 1] The polymerizable compound was changed to 0.74 g of commercially available bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation, product name: JER (registered trademark) 828), and the curing component (curing agent) was changed to polyphenylene ether oligomer (both terminal hydroxyl groups), product name: Noryl, manufactured by SABIC Co., Ltd. TM A sample was prepared and evaluated in the same manner as in Example 1, except that 3.20 g of SA90-100 resin (mPPE) was used. The results are shown as Comparative Example 1.

[0152] [Comparative Example 2] A sample was prepared by adding 20 wt % of silica powder as an inorganic filler, which was the same as in Example 4, to the same adhesive solution as in Comparative Example 1, and was evaluated. The result is referred to as Comparative Example 2.

[0153] [Comparative Example 3] A sample was prepared and evaluated in the same manner as in Example 6, except that the polymerizable compound (S01) in Example 6 was changed to 0.76 g of a commercially available bisphenol A type epoxy resin (manufactured by Mitsubishi Chemical Corporation under the trade name of JER (registered trademark) 828) and the curing component (curing agent) was changed to 0.89 g of an active ester curing agent (manufactured by DIC Corporation under the trade name of HPC-8000H-65T). The result is Comparative Example 3.

[0154] <Evaluation Results> [Table 2] Characteristics of adhesives with different polymerizable compounds TIFF2024167588000027.tif31142

[0155] [Table 3] Properties of adhesives containing inorganic fillers TIFF2024167588000028.tif26119

[0156] [Table 4] Characteristics table of adhesives with different hardeners as hardening components TIFF2024167588000029.tif26141

[0157] [Table 5] Characteristics table of adhesives with different curing accelerators as curing components TIFF2024167588000030.tif26141

[0158] From Table 2, it can be seen that by using the adhesive of the present invention using the bifunctional or higher polymerizable liquid crystal compound used in the present invention, it is possible to realize adhesion with excellent dielectric properties and adhesive properties. In addition, it can be seen that the thermal diffusivity is slightly high and the heat dissipation properties are good. It can be seen from Table 3 that by adding an inorganic filler to the adhesive of the present invention, it is possible to form an adhesive layer that has a low relative dielectric constant and dielectric tangent and is excellent in heat dissipation properties. Table 4 shows that when an active ester curing agent is used as the curing component, the dielectric constant and dielectric tangent are both higher than those of a PPE oligomer curing agent with hydroxyl groups. This is thought to reflect the technical difficulty of polymerizing an active ester curing agent with epoxy groups, and it is believed that this can be reduced by accumulating curing know-how. On the other hand, Table 5 shows that the dielectric properties (dielectric constant) and adhesive properties are also improved by changing the curing component (curing accelerator) from an imidazole-based to a phosphorus-based one. It is preferable to realize an adhesive that can bond more strongly and has excellent dielectric properties, but it is best to choose the optimum one based on the target insulation resistance and curing temperature.

[0159] Adhesives for electronic substrates are required to be heat resistant because they are soldered using a reflow oven, etc. For Example 1 and Comparative Example 1, the temperature at which the weight is reduced by 5% was measured using a TG / DTA thermal analyzer (Rigaku Corporation, 8121 / S-SL type TG / DTA).

[0160] [Table 6] TIFF2024167588000031.tif21138

[0161] From Table 6, it can be seen that the bifunctional or higher polymerizable liquid crystal compounds used in the present invention, even if they are alicyclic types such as compound (S-01), exhibit heat resistance that is comparable to that of biphenyl-type epoxy compounds that are widely used in semiconductor encapsulants, etc. Of course, it depends on the decomposition temperature of the curing agent, etc., but this shows that the adhesive of the present invention has heat resistance that allows it to be used without problems in semiconductor substrate applications. [Industrial Applicability]

[0162] As described above, the adhesive of the present invention is used to bond a low dielectric electronic substrate to a metal foil or a resist layer, and the laminate obtained from the adhesive can be used as various electronic components. Furthermore, various electronic components obtained by using the adhesive of the present invention are useful for use as various electronic devices of the present invention.

Claims

1. The adhesive contains a bifunctional or higher functional polymerizable liquid crystal compound and a curable component polymerizable with the polymerizable liquid crystal compound, and is used to bond a low dielectric electronic substrate to a metal foil or a resist layer.

2. The adhesive according to claim 1 , wherein the bifunctional or higher functional polymerizable liquid crystal compound is a polymerizable liquid crystal compound represented by formula (1): R 1a -Z 1 -A 1 -Z 2 -A 2 -(Z 3 -A 3 ) m1 -Z 4 -R 1b (1) In formula (1), A 1 , A 2 , and A 3 are independently 1,4-cyclohexylene, 1,4-cyclohexenylene, 1,4-phenylene, bicyclo[2.2.2]octo-1,4-diyl, bicyclo[3.1.0]hex-3,6-diyl, or fluorene-2,7-diyl, and in these rings, at least one -CH 2 - may be replaced by -O-, at least one -CH= may be replaced by -N=, at least one hydrogen may be replaced by halogen or an alkyl having 1 to 12 carbon atoms in which at least one hydrogen may be replaced by halogen, and in this alkyl, at least one -CH 2 - may be replaced by -O-, -CO-, -COO-, -OCO-, or -C=C-; Z 1 , Z 2 , Z 3 , and Z 4 are independently a single bond or an alkylene having 1 to 20 carbon atoms, and in this alkylene, at least one -CH 2 - is -O-, -S-, -CO-, -COO-, -OCO-, -SO 2 may be replaced by -, -CH=CH-, -CF=CF-, -CH=N-, -N=CH-, or -N=N-, and at least one hydrogen may be replaced by a halogen; m1 is 0, 1, or 2; In the formula, Z 3 Or A 3 When there are multiple, they may be the same or different, R 1a and R 1b are independently a group selected from the polymerizable groups represented by formulas (PG-1) to (PG-5), In formulas (PG-1) to (PG-5), R b is hydrogen, halogen, -CF 3 or an alkyl group having 1 to 5 carbon atoms, q is 0 or 1, and there are multiple R b may be the same or different; A 1 and A 2 is 1,4-phenylene; Z 2 is a single bond, m1 is 0, and R 1a and R 1b In the case where the polymerizable group is represented by formula (PG-5), Z 1 and Z 4 is an alkylene having 3 to 20 carbon atoms, and in this alkylene, at least one -CH 2 - is -O-, -S-, -CO-, -COO-, -OCO-, -SO 2 may be replaced by -, -CH=CH-, -CF=CF-, -CH=N-, -N=CH-, or -N=N-, and at least one hydrogen may be replaced by a halogen.

3. A of the bifunctional or higher polymerizable liquid crystal compound 1 From the right end A 3 The mesogen portion up to is a biphenyl structure, and the biphenyl structure and R 1a and R 1b A linear Z having 3 or more carbon atoms is placed between the epoxy groups. 1 and Z 4 The adhesive of claim 2 .

4. The adhesive according to claim 2 , wherein a mesogen moiety of the di- or higher functional polymerizable liquid crystal compound has a bicyclohexyl structure.

5. 3. The adhesive according to claim 2, wherein the polymerizable group of the di- or higher functional polymerizable liquid crystal compound is the polymerizable group represented by formula (PG-5).

6. The adhesive of claim 1 , wherein the curing component comprises at least one selected from the group consisting of a curing agent, a polymerization initiator, a curing accelerator, and a crosslinking agent.

7. 7. The adhesive of claim 6, wherein the curing agent comprises at least one selected from the group consisting of a polyphenylene ether oligomer having at least two hydroxyl groups, an active ester curing agent, and an alkyl ether having at least two hydroxyl groups.

8. The adhesive according to claim 1 , further comprising 1 to 30 volume % of an inorganic filler.

9. 9. The adhesive of claim 8, wherein the inorganic filler is at least one selected from the group consisting of silicon oxide compounds of spherical silica, crushed silica, hollow silica, and fumed silica, carbon nanotubes, graphene, silicon carbide, and metal oxides of magnesium oxide and zinc oxide.

10. The adhesive described in claim 8, wherein the inorganic filler is a nitride filler, and the thermal conductivity of the cured product of the adhesive is 1 W / m·K or more.

11. The adhesive of claim 1 , wherein the adhesive is a solid adhesive.

12. 12. The adhesive of claim 1 or 11, wherein the low dielectric electronic substrate comprises at least one layer selected from the group consisting of liquid crystal polymer resin, modified polyimide resin, polyphenylene ether resin, polyphenylene sulfide resin, cycloolefin resin, and fluororesin.

13. An electronic device using the adhesive according to claim 1 or 11.

Citation Information

Patent Citations

  • Polymer, composition for low dielectric substrate, cured product, and electronic apparatus using the same

    JP2023035176A

  • Composition for forming low dielectric resin, low dielectric member, and electronic apparatus using the same

    JP2023047892A

  • A method for welding at least two layers

    JP2015515927A

  • Low dielectric adhesive composition

    JP2022133352A

  • Low dielectric adhesive composition

    JP2023032286A