AI Technical Summary
The electrochemical performance of traditional sodium-ion secondary batteries is difficult to meet the needs of high energy density and long cycle life, especially due to the instability of the negative electrode plate interface, which leads to limited cycle performance.
By introducing carbon-based materials with a specific particle size range into the negative electrode sheet of the secondary battery, and adjusting its volume proportion to increase the contact area and close packing between the negative electrode active particles, improve the adhesion of the negative electrode sheet, thereby improving Cycling performance of secondary batteries.
It effectively improves the cycle performance and first-efficiency performance of secondary batteries, prolongs the service life of the battery, while maintaining excellent energy density.
Smart Images

Figure CN118872091A_ABST
Abstract
Description
Secondary battery and electrical device containing same Technical Field
[0001] The present application relates to the field of batteries, and in particular to a secondary battery and an electrical device containing the same. Background Art
[0002] Secondary batteries are increasingly widely used due to their clean and renewable characteristics. They have the advantages of high energy density, low self-discharge, and excellent cycle performance.
[0003] As demand increases, people have higher and higher requirements for the electrochemical performance of secondary batteries. Especially as the supply of lithium resources becomes increasingly tight, sodium-ion secondary batteries with richer sodium resources and lower costs have come into people's attention. However, the electrochemical performance of traditional sodium-ion batteries is difficult to meet people's needs and needs further improvement.
[0004] Summary of the Invention
[0005] In view of the above problems, the present application provides a secondary battery and an electrical device containing the same, aiming to improve the cycle performance of the secondary battery.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present application provides a secondary battery, including a negative electrode plate, the negative electrode plate including a negative electrode collector and a negative electrode film layer provided on at least one surface of the negative electrode collector, the negative electrode film layer including a negative electrode active material, and the negative electrode active material including a carbon-based material; in the negative electrode active material, the volume proportion of the first carbon-based material with a particle size less than or equal to 2 μm is greater than or equal to 15%.
[0007] In the above-mentioned secondary battery, the negative electrode active material of the negative electrode film layer in the negative electrode plate is controlled to contain a first carbon-based material with a specific particle size range, and its volume proportion in the negative electrode active material is regulated to increase the contact area between the negative electrode active particles, so that the negative electrode active particles are closely stacked, thereby improving the adhesion of the negative electrode plate, and further improving the cycle performance of the secondary battery.
[0008] In any embodiment of the present application, the volume proportion of the first carbon-based material in the negative electrode active material is 20% to 70%, and optionally 30% to 60%. The volume proportion of the first carbon-based material having a particle size of 2 μm or less is further adjusted to better blend it with other negative electrode active materials, thereby further improving the cycle performance of the secondary battery.
[0009] In any embodiment of the present application, the first carbon-based material satisfies at least one of the following conditions (1) to (7):
[0010] (1) the volume distribution particle size Dv10 of the first carbon-based material is 0.2 μm to 0.5 μm;
[0011] (2) the volume distribution particle size Dv50 of the first carbon-based material is 0.5 μm to 2 μm;
[0012] (3) the volume distribution particle size Dv90 of the first carbon-based material is ≤ 2 μm;
[0013] (4) The specific surface area SSA of the first carbon-based material is 5 m 2 / g~20m 2 / g;
[0014] (5) In the Raman spectrum test of the first carbon-based material, I D / I G 0.95~1.35;
[0015] (6) The powder compaction density of the first carbon-based material under a force of 50,000 N is 0.8 g / cm 3 ~1.1g / cm 3 ;
[0016] (7) The tap density of the first carbon-based material is 0.3 g / cm 3 ~0.8g / cm 3 .
[0017] In any embodiment of the present application, in the negative electrode active material, the volume proportion of the second carbon-based material with a particle size greater than 2 μm and less than or equal to 25 μm is 20% to 80%; optionally 50% to 60%.
[0018] In any embodiment of the present application, the second carbon-based material satisfies at least one of the following conditions (I) to (VIII):
[0019] (I) the volume particle size distribution of the second carbon-based material is unimodal;
[0020] (II) the volume distribution particle size Dv10 of the second carbon-based material is 2 μm to 4 μm;
[0021] (III) the volume distribution particle size Dv50 of the second carbon-based material is 4 μm to 8 μm;
[0022] (IV) the volume distribution particle size Dv90 of the second carbon-based material is 8 μm to 20 μm;
[0023] (V) the volume distribution particle size Dv99 of the second carbon-based material is 20 μm to 25 μm;
[0024] (VI) The specific surface area SSA of the second carbon-based material is 1 m 2 / g~10m 2 / g;
[0025] (VII) The powder compaction density of the second carbon-based material under a force of 50,000 N is 0.92 g / cm 3 ~1.2g / cm 3 ;
[0026] (VIII) The tap density of the second carbon-based material is 0.6 g / cm 3 ~0.94g / cm 3 .
[0027] In any embodiment of the present application, in the negative electrode active material, the volume proportion of the third carbon-based material having a particle size greater than 40 μm and less than or equal to 100 μm is less than or equal to 10%; optionally less than or equal to 5%.
[0028] In any embodiment of the present application, the third carbon-based material satisfies at least one of the following conditions (1) to (4):
[0029] (1) The specific surface area SSA of the third carbon-based material is 1 m 2 / g~10m 2 / g;
[0030] (2) In the Raman spectrum test of the third carbon-based material, I D / I G 0.95~1.35;
[0031] (3) The powder compaction density of the third carbon-based material under a force of 50,000 N is 0.7 g / cm 3 ~1g / cm 3 ;
[0032] (4) The tap density of the third carbon-based material is 0.5 g / cm 3 ~0.8g / cm 3 .
[0033] In any embodiment of the present application, the volume distribution particle size Dv50 of the negative electrode active material is less than or equal to 8 μm; optionally, the volume distribution particle size Dv50 of the negative electrode active material is 2 μm to 6 μm.
[0034] Further regulating the volume distribution particle size Dv50 of the negative electrode active material to have a specific range can further improve the initial efficiency of the secondary battery.
[0035] In any embodiment of the present application, the volume distribution particle size of the negative electrode active material satisfies: 4 μm≤Dv90≤20 μm; optionally, 5 μm≤Dv90≤16 μm.
[0036] In any embodiment of the present application, the volume distribution particle size Dv10 of the negative electrode active material satisfies: 0.2 μm≤Dv10≤2 μm; optionally, 0.5 μm≤Dv10≤1.8 μm.
[0037] In any embodiment of the present application, the specific surface area SSA of the negative electrode active material is less than or equal to 20 m 2 / g; SSA≤10m can be selected 2 / g.
[0038] In any embodiment of the present application, in the Raman spectroscopy test of the negative electrode active material, I D / I G It is 0.87~1.35; it can be selected as 0.91~1.25.
[0039] In any embodiment of the present application, in the X-ray diffraction test of the negative electrode active material, there is a (002) crystal plane peak in the range of 22° to 24°, and the interlayer spacing of the (002) crystal plane of the negative electrode active material is ≥0.37nm, which can be optionally 0.37nm to 0.42nm.
[0040] In any embodiment of the present application, the powder compaction density of the negative electrode active material under a force of 50000N is 0.90g / cm 3 ~1.5g / cm 3 ; Optional 0.95g / cm 3 ~1.3g / cm 3 .
[0041] In any embodiment of the present application, the tap density of the negative electrode active material is 0.50 g / cm 3 ~0.97g / cm 3 ; Optional 0.6g / cm 3 ~0.94g / cm 3 .
[0042] In any embodiment of the present application, the carbon-based material includes a plurality of nanopore structures. Optionally, the carbon-based material includes a plurality of pore structures with a pore diameter of less than 10 nm.
[0043] In any embodiment of the present application, the carbon-based material includes a hard carbon material.
[0044] In any embodiment of the present application, the secondary battery is a sodium ion secondary battery.
[0045] In a second aspect of the present application, an electrical device is provided, comprising the secondary battery according to the first aspect of the present application.
[0046] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0048] FIG1 is a schematic diagram of one embodiment of a secondary battery.
[0049] FIG2 is an exploded view of FIG1 .
[0050] FIG. 3 is a schematic diagram of a battery pack according to an embodiment.
[0051] FIG. 4 is an exploded view of FIG. 3 .
[0052] FIG. 5 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present invention.
[0053] FIG6 is an electron microscope image of the hard carbon particles before mixing in Example 1.
[0054] FIG. 7 is an electron microscope image of the mixed hard carbon particles in Example 1.
[0055] Description of reference numerals:
[0056] 1. Battery pack; 2. Upper box; 3. Lower box; 4. Secondary battery; 41. Shell; 42. Electrode assembly; 43. Cover; 5. Electrical device. DETAILED DESCRIPTION
[0057] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.
[0058] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.
[0059] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.
[0060] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0061] In the description of the embodiments of this application, the term "and / or" is simply a description of the association relationship between associated objects, indicating that three relationships can exist. For example, A and / or B can represent the following three situations: A exists alone, A and B exist simultaneously, and B exists alone. In addition, the character " / " in this document generally indicates that the associated objects are in an "or" relationship.
[0062] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0063] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or position relationship, are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.
[0064] In the description of the embodiments of the present application, unless otherwise expressly specified or limited, technical terms such as "installed," "connected," "connected," and "fixed" should be understood in a broad sense. For example, they can refer to fixed connections, detachable connections, or integration; mechanical connections or electrical connections; direct connections or indirect connections through an intermediate medium; internal connections between two components or interactions between two components. Those skilled in the art can understand the specific meanings of the above terms in the embodiments of the present application based on specific circumstances.
[0065] Secondary batteries primarily rely on the movement of active ions between the positive and negative electrodes to generate electrical energy. During charging, the active ions are deintercalated from the positive electrode and embedded into the negative electrode through the electrolyte, while the reverse occurs during discharge. However, during the charge and discharge process of secondary batteries, the intercalation and deintercalation of active ions (such as sodium ions) causes the expansion and contraction of the negative electrode sheet, damaging the structure of the negative electrode material. Furthermore, during the cyclic charge and discharge process, the co-intercalation of electrolyte solvents, the reduction of organic solvents, and the generation of gas under high currents all cause the negative electrode active material to peel off, leading to increased interfacial instability, resulting in loss of negative electrode active material and damage to the solid electrolyte interface (SEI) film, thereby reducing the cycle life of the battery.
[0066] In summary, the instability of the negative electrode interface limits the improvement of the secondary battery's cycling performance. Traditionally, improvements to the binder have been made to enhance the interface stability of the negative electrode. However, these binders typically require the use of macromolecular resins, which expand after long-term contact with the electrolyte, ultimately deteriorating the secondary battery's cycling performance.
[0067] Based on this, the researchers of this application took a different approach and creatively proposed regulating the particle size of the negative electrode active material to enhance the synergistic interaction between the negative electrode active material particles, thereby improving the adhesion of the negative electrode sheet and, in turn, the cycle performance of the secondary battery. After extensive experimental research, the researchers of this application arrived at the technical solution of this application.
[0068] In one embodiment of the present application, a secondary battery is provided, comprising a negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, the negative electrode film layer comprising a negative electrode active material, the negative electrode active material comprising a carbon-based material; in the negative electrode active material, the volume proportion of a first carbon-based material having a particle size less than or equal to 2 μm is greater than or equal to 15%.
[0069] In the above-mentioned secondary battery, the negative electrode active material of the negative electrode film layer in the negative electrode plate is controlled to contain a first carbon-based material with a specific particle size range, and its volume proportion in the negative electrode active material is simultaneously regulated, thereby increasing the contact area between the negative electrode active particles and making the negative electrode active particles closely stacked, thereby improving the adhesion of the negative electrode plate, and thus effectively improving the cycle performance of the secondary battery.
[0070] In any embodiment of the present application, in the negative electrode active material, the volume proportion of the first carbon-based material is 20% to 70%, and can be optionally 30% to 60%.
[0071] The volume proportion of the first carbon-based material with a particle size of less than or equal to 2 μm is further regulated to enable better compounding with other negative electrode active materials, thereby further improving the cycle performance of the secondary battery.
[0072] %, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%, 81%, 82%, 83%, 84%, 85%, 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%, 97%, 98%, 99%, 100%, 101%, 102%, 103%, 104%, 105%, 106%, 107%, 108%, 109%, 110%, 111%, 112%, 113%, 114%, 115%, 116%, 117%, 118%, 119%, 120%, 121%, 122%, 123%, 124%, 125%, 126%, 127%, 128%, 129%, 200 or a range consisting of any two values, for example, 20% to 50%, 20% to 60%, 20% to 65%, 20% to 70%, 25% to 50%, 25% to 60%, 25% to 65%, 25% to 70%, 30% to 40%, 30% to 50%, 30% to 60%, 30% to 65%, 35% to 55%, 35% to 60%, 35% to 65%, 35% to 70%, 40% to 60%, 40% to 65%, 40% to 70%, 45% to 60%, 45% to 65%, 45% to 70%, 50% to 60%, 50% to 65%, 50% to 70%, 60% to 70%, 65% to 70%.
[0073] In any embodiment of the present application, the volume distribution particle size Dv10 of the first carbon-based material is 0.2 μm to 0.5 μm.
[0074] In any embodiment of the present application, the volume distribution particle size Dv50 of the first carbon-based material is 0.5 μm to 2 μm.
[0075] In any embodiment of the present application, the volume distribution particle size Dv90 of the first carbon-based material is ≤ 2 μm.
[0076] In any embodiment of the present application, the specific surface area SSA of the first carbon-based material is 5m 2 / g~20m 2 / g.
[0077] In any embodiment of the present application, in the Raman spectrum test of the first carbon-based material, I D / I G It is 0.95~1.35.
[0078] In any embodiment of the present application, the powder compaction density of the first carbon-based material under a force of 50,000 N is 0.8 g / cm 3 ~1.1g / cm 3 .
[0079] In any embodiment of the present application, the tap density of the first carbon-based material is 0.3 g / cm 3 ~0.8g / cm 3 .
[0080] In any embodiment of the present application, in the X-ray diffraction test of the first carbon-based material, there is a (002) crystal plane peak in the range of 22° to 24°, and the interlayer spacing of the (002) crystal plane of the negative electrode active material is 0.37nm to 0.42nm.
[0081] In any embodiment of the present application, in the negative electrode active material, the volume proportion of the second carbon-based material with a particle size greater than 2 μm and less than or equal to 25 μm is 20% to 80%; optionally 50% to 60%.
[0082] In the above “20% to 80%”, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 36%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, 76%, 77%, 78%, 79%, 80%; or a range consisting of any two values, for example, 20% to 60%, 20% to 65%, 20% to 70%, 20% to 75%, 20% to 80%, 25% to 60%, 25% to 65%, 25% to 70%, 25% to 75%, 25% to 80%, 30% to 60%, 30% to 65 %, 35%-70%, 35%-75%, 35%-80%, 35%-60%, 35%-65%, 35%-70%, 35%-75%, 35%-80%, 40%-60%, 40%-65%, 40%-70%, 40%-75%, 40%-80%, 45%-60%, 45%-65%, 45%-70%, 45% ~75%, 45%~80%, 50%~60%, 50%~65%, 50%~70%, 50%~75%, 50%~80%, 55%~65%, 55%~75%, 55%~80%, 60%~70%, 60%~75%, 60%~80%, 65%~70%, 65%~75%, 65%~80%, 70%~80%.
[0083] In any embodiment of the present application, the volume particle size distribution of the second carbon-based material is unimodal.
[0084] In any embodiment of the present application, the volume distribution particle size Dv10 of the second carbon-based material is 2 μm to 4 μm.
[0085] In any embodiment of the present application, the volume distribution particle size Dv50 of the second carbon-based material is 4 μm to 8 μm.
[0086] In any embodiment of the present application, the volume distribution particle size Dv90 of the second carbon-based material is 8 μm to 20 μm.
[0087] In any embodiment of the present application, the volume distribution particle size Dv99 of the second carbon-based material is 20 μm to 25 μm.
[0088] In any embodiment of the present application, the specific surface area SSA of the second carbon-based material is 1 m 2 / g~10m 2 / g.
[0089] In any embodiment of the present application, the powder compaction density of the second carbon-based material under a force of 50,000 N is 0.92 g / cm 3 ~1.2g / cm 3 .
[0090] In any embodiment of the present application, the tap density of the second carbon-based material is 0.6 g / cm 3 ~0.94g / cm 3 .
[0091] In any embodiment of the present application, in the X-ray diffraction test of the second carbon-based material, there is a (002) crystal plane peak in the range of 22° to 24°, and the interlayer spacing of the (002) crystal plane of the negative electrode active material is 0.37nm to 0.42nm.
[0092] In any embodiment of the present application, in the negative electrode active material, the volume proportion of the third carbon-based material having a particle size greater than 40 μm is 0.
[0093] The particle composition in the negative electrode active material is regulated so that the volume proportion of carbon-based materials with a particle size greater than 40 μm is 0, that is, there is no carbon-based material with a particle size greater than 40 μm, so as to avoid the negative impact of larger particle sizes on the compounding effect.
[0094] Furthermore, if a third carbon-based material with a particle size greater than 40 μm exists in the negative electrode active material, the volume proportion of the third carbon-based material with a larger particle size can be further adjusted so that it can be better compounded with the carbon-based material with a smaller particle size to reduce the impact on the battery cycle performance.
[0095] In some embodiments, in the negative electrode active material, the volume proportion of the third carbon-based material having a particle size greater than 40 μm is less than or equal to 10%; optionally, less than or equal to 5%.
[0096] In the negative electrode active material, the volume proportion of the third carbon-based material with a particle size greater than 40 μm can be selected as any number among 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, or a range consisting of any two numbers; for example For example, it can be 0.1% to 5%, 0.1% to 4.5%, 0.1% to 4%, 0.1% to 3.5%, 0.1% to 3%, 0.1% to 2.5%, 0.1% to 2%, 0.1% to 1.5%, 0.1% to 1%, 0.1% to 0.5%, 1% to 5%, 1% to 4.5%, 1% to 4%, 1% to 3.5%, 2% to 4%, 3% to 5%.
[0097] Optionally, the particle size of the third carbon-based material having a particle size greater than 40 μm is greater than 40 μm and less than or equal to 100 μm.
[0098] In any embodiment of the present application, the specific surface area SSA of the third carbon-based material is 1 m 2 / g~10m 2 / g.
[0099] In any embodiment of the present application, in the Raman spectrum test of the third carbon-based material, I D / I G It is 0.95~1.35.
[0100] In any embodiment of the present application, the powder compaction density of the third carbon-based material under a force of 50,000 N is 0.7 g / cm 3 ~1g / cm 3 .
[0101] In any embodiment of the present application, the tap density of the third carbon-based material is 0.5 g / cm 3 ~0.8g / cm 3 .
[0102] In any embodiment of the present application, in the X-ray diffraction test of the third carbon-based material, there is a (002) crystal plane peak in the range of 22° to 24°, and the interlayer spacing of the (002) crystal plane of the negative electrode active material is 0.37nm to 0.42nm.
[0103] In any embodiment of the present application, the volume distribution particle size Dv50 of the negative electrode active material is less than or equal to 8 μm.
[0104] Optionally, the volume distribution particle size Dv50 of the negative electrode active material is 1 μm to 8 μm.
[0105] Optionally, the volume distribution particle size Dv50 of the negative electrode active material is 1 μm to 6 μm.
[0106] Optionally, the volume distribution particle size Dv50 of the negative electrode active material is 2 μm to 6 μm.
[0107] Further regulating the volume distribution particle size Dv50 of the negative electrode active material to have a specific range can further improve the initial efficiency of the secondary battery.
[0108] In any embodiment of the present application, the volume distribution particle size of the negative electrode active material satisfies: 4 μm≤Dv90≤20 μm; optionally, 5 μm≤Dv90≤16 μm.
[0109] In any embodiment of the present application, the volume distribution particle size Dv10 of the negative electrode active material satisfies: 0.2 μm≤Dv10≤2 μm; optionally, 0.5 μm≤Dv10≤1.8 μm.
[0110] In this application, the above-mentioned Dv10, Dv50, or Dv90 represents the particle size corresponding to the 10%, 50%, or 90% cumulative volume distribution percentage of the material, respectively. These can be measured using instruments and methods known in the art. For example, they can be conveniently measured using a laser particle size analyzer, referring to GB / T 19077-2016 Particle Size Distribution Laser Diffraction Method. The testing instrument can be a Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK.
[0111] In any embodiment of the present application, the specific surface area SSA of the negative electrode active material is less than 20m 2 / g; SSA≤10m can be selected 2 / g.
[0112] The specific surface area of the negative electrode active material is determined according to GB / T 19587-2004, which stipulates the determination of the specific surface area of solid substances by the BET method for gas adsorption.
[0113] In any embodiment of the present application, in the Raman spectrum test of the negative electrode active material, I D / I G It is 0.87~1.35; it can be selected as 0.91~1.25.
[0114] Above I D / I G It refers to the ratio of the peak intensities of D peak and G peak in the Raman spectrum of the material; D The Raman spectrum of carbon materials is 1350±50cm -1 The D peak intensity at I G The Raman spectrum of carbon materials is 1580±50cm -1 The G peak intensity at .
[0115] In any embodiment of the present application, the carbon-based material includes a hard carbon material.
[0116] Carbon materials are classified by their difficulty in graphitizing into graphite, soft carbon, and hard carbon. Hard carbon refers to carbon that is difficult to completely graphitize above 2800°C, as its disordered structure is difficult to eliminate at high temperatures. Furthermore, the precursors for preparing hard carbon materials are not limited to mineral raw materials and can include all compounds containing C, H, and O elements, with the exception of mineral raw materials that are particularly easy to graphitize.
[0117] In any embodiment of the present application, there is a (002) crystal plane peak in the range of 22° to 24°, and the interlayer spacing of the (002) crystal plane of the negative electrode active material is ≥0.37nm, and can be optionally 0.37nm to 0.42nm.
[0118] Specifically, in the X-ray diffraction test of the negative electrode active material, the (002) crystal plane interlayer spacing is calculated using the Bragg formula.
[0119] In any embodiment of the present application, the powder compaction density of the negative electrode active material under a force of 50000N is 0.90g / cm 3 ~1.5g / cm 3 ; Optional 0.95g / cm 3 ~1.3g / cm 3 .
[0120] Further control the powder compaction density of the negative electrode active material, improve the bonding force of the negative electrode sheet, and maintain excellent first efficiency while improving the cycle performance of the secondary battery.
[0121] In any embodiment of the present application, the tap density of the negative electrode active material is 0.50 g / cm 3 ~0.97g / cm 3 ; Optional 0.6g / cm 3 ~0.94g / cm 3 .
[0122] In any embodiment of the present application, the carbon-based material includes a plurality of nanopore structures. Optionally, the carbon-based material includes a plurality of pore structures with a pore diameter of less than 10 nm.
[0123] In any embodiment of the present application, based on the total weight of the negative electrode film layer, the mass proportion of the negative electrode active material is 85 wt % to 95 wt %.
[0124] In any embodiment of the present application, the negative electrode film layer further includes a negative electrode conductor and a negative electrode binder.
[0125] In any embodiment of the present application, the negative electrode conductive agent may be a conductive material commonly used in the art, including but not limited to at least one of graphite, carbon nanotubes, nanofibers, carbon black, and graphene. Specifically, the negative electrode conductive agent may be selected from at least one of SP, KS-6, acetylene black, branched Ketjen black ECP, SFG-6, vapor-grown carbon fiber VGCF, carbon nanotubes CNTs, graphene, and composite conductive agents thereof.
[0126] Based on the total weight of the negative electrode film layer, the weight ratio of the negative electrode conductive agent in the negative electrode film layer is 0 to 20 wt %.
[0127] The negative electrode binder can be a binder commonly used in the art, and can be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0128] Based on the total weight of the negative electrode film layer, the weight ratio of the negative electrode binder in the negative electrode active layer is 0 to 30 wt %.
[0129] In any embodiment of the present application, the negative electrode film layer may further optionally include other additives, such as a thickener, such as sodium carboxymethyl cellulose (CMC-Na), etc. Based on the total weight of the negative electrode active layer, the weight ratio of the other additives in the negative electrode active layer is 0 to 15 wt%.
[0130] In any embodiment of the present application, the current collector in the negative electrode plate may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0131] The secondary battery can be prepared by a commonly used preparation method in the art. The preparation method is described here by way of example, but is not limited to the following preparation method.
[0132] The method for preparing the secondary battery includes preparing a negative electrode plate by adopting the following steps S10 to S30.
[0133] S10, preparing the above-mentioned negative electrode active material.
[0134] S20, preparing the negative electrode active material into a negative electrode slurry.
[0135] S30, coating the negative electrode slurry on at least one surface of the negative electrode current collector to form a negative electrode film layer.
[0136] In any embodiment of the present application, the raw materials used to prepare the negative electrode active material include a first carbon-based material, a second carbon-based material and a third carbon-based material, the particle size of the first carbon-based material is ≤2μm, the particle size of the second carbon-based material is greater than 2μm and less than or equal to 25μm, and the particle size of the third carbon-based material is greater than 40μm.
[0137] It can be understood that the first carbon-based material, the second carbon-based material and the third carbon-based material are configured according to the particle size volume ratio of the negative electrode active material.
[0138] The selection and parameter control of the first carbon-based material, the second carbon-based material and the third carbon-based material are the same as above and will not be repeated here.
[0139] In any embodiment of the present application, the specific steps of preparing the negative electrode active material include the following steps:
[0140] The first carbon-based material, the second carbon-based material and the third carbon-based material are mixed to obtain a negative electrode active material.
[0141] Optionally, in the above mixing step, the mixing time is 0.5h to 10h.
[0142] Control the mixing time to ensure that the materials are mixed evenly without destroying the structure of the original material particles.
[0143] Specifically, the mixing step is carried out in a mixer.
[0144] In any embodiment of the present application, the solid content of the negative electrode slurry is 30wt% to 70wt%, and the viscosity at room temperature is adjusted to 2000mPa·s to 10000mPa·s; the obtained negative electrode slurry is coated on the negative electrode current collector, and after a drying process, cold pressing such as rolling to obtain a negative electrode sheet. The negative electrode powder coating unit area density is 75mg / m 2 ~220 mg / m 2 , the compaction density of the negative electrode is 1.2g / m 3 ~2.0g / m 3 .
[0145] In any embodiment of the present application, the secondary battery further includes a positive electrode sheet, an electrolyte and a separator.
[0146] Optionally, the secondary battery may be a sodium ion battery, a lithium ion battery, or a potassium ion battery.
[0147] In a specific example, the secondary battery is a sodium ion battery.
[0148] The following examples are given for the positive electrode sheet and the electrolyte separator, but are not limited to the following scope.
[0149] [Positive electrode]
[0150] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer provided on at least one surface of the positive electrode current collector, and the components of the positive electrode film layer include a positive electrode active material.
[0151] As an example, the current collector in the positive electrode sheet has two surfaces opposite to each other in its thickness direction, and the positive electrode active material layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.
[0152] In any embodiment of the present application, the current collector in the positive electrode plate may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0153] The positive electrode active material may be a commonly used positive electrode active material in the present application, such as a lithium ion positive electrode active material or a sodium ion positive electrode active material.
[0154] Further, as an example, the lithium ion active material may include at least one of the following materials: lithium-containing phosphates of olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium manganese phosphate (such as LiMnPO4), and lithium manganese iron phosphate.
[0155] In any embodiment of the present application, the molecular formula of the lithium ion active material is: LiFe x Mn (1-x) PO4, x is any number from 0 to 1.
[0156] It can be understood that when x is 0, LiFe x Mn (1-x) PO4 is LiMnPO4 lithium manganese phosphate, and when x is 1, LiFePO4 is LiFePO4 lithium iron phosphate (LFP).
[0157] As an example, the sodium ion active material may include at least one of the following materials: a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as sodium ion battery positive electrode active materials may also be used.
[0158] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Sodium transition metal oxide is, for example, Na x MO2, wherein M includes at least one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0159] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. Transition metals include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y includes at least one of P, S, and Si; n represents (YO4) n- valence.
[0160] Polyanionic compounds can also be sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y includes at least one of P, S, and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0161] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y includes at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, including at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0162] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).
[0163] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' each independently include at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0164] Based on the total weight of the positive electrode film layer, the weight ratio of the positive electrode active material in the positive electrode film layer is 80 wt % to 100 wt %.
[0165] In any embodiment of the present application, the components of the positive electrode film layer further include a positive electrode conductor and a positive electrode binder.
[0166] The positive electrode conductive agent may be any commonly used conductive agent in the art, including but not limited to at least one of graphite, carbon nanotubes, nanofibers, carbon black, and graphene. Specifically, the positive electrode conductive agent may be selected from at least one of SP, KS-6, acetylene black, branched Ketjen black ECP, SFG-6, vapor-grown carbon fiber (VGCF), carbon nanotubes (CNTs), graphene, and composite conductive agents thereof.
[0167] Based on the total weight of the positive electrode film layer, the weight ratio of the positive electrode conductive agent in the positive electrode active layer is 0 to 20 wt %.
[0168] In any embodiment of the present application, the binder of the above-mentioned positive electrode binder can be polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, hydrogenated nitrile rubber, styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS) and at least one of fluorine-containing acrylate resin.
[0169] Based on the total weight of the positive electrode film layer, the weight ratio of the positive electrode binder in the positive electrode active layer is 0 to 30 wt %.
[0170] In any embodiment of the present application, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained. The positive electrode slurry has a solid content of 40wt% to 80wt%, and the viscosity at room temperature is adjusted to 5000mPa·s to 25000mPa·s. The positive electrode slurry is coated on the surface of the positive electrode collector, dried and then cold-pressed by a cold rolling mill to form a positive electrode sheet; the positive electrode powder coating unit area density is 150 to 350mg / m 2 The compaction density of the positive electrode is 3.0-3.6 g / cm 3 , can be selected as 3.3~3.5g / cm 3 The calculation formula for compacted density is:
[0171] Compaction density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).
[0172] [Electrolyte]
[0173] The electrolyte includes electrolyte salt and solvent
[0174] In some embodiments, the electrolyte salt may be selected from electrolyte salts commonly used in the art, including lithium ion electrolyte salts and sodium ion electrolyte salts.
[0175] As an example, the lithium ion electrolyte salt is selected from: lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LIDFOB), lithium dioxalatoborate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LIDFOP), Li(FSO2)2N, LiCF3SO3 and lithium tetrafluorooxalatophosphate (LiTFOP). One or more of the following.
[0176] As an example, the sodium ion electrolyte salt is selected from one or more of: sodium hexafluorophosphate (NaPF6), NaClO4, NaAIClh, NaFeClh, NaBF4, NaBClh, NaNO3, NaPOFA, NaSCN, NaCN, NaAsF6, NaCF3CO2, NaSbF6, NaC6HsCO2, Na(CH3)C6H4SO3, NaHSO4, and NaB(C6Hs)4.
[0177] In any embodiment of the present application, the solvent may be selected from one or more of fluoroethylene carbonate (FEC), ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), ethyl methyl sulfone (EMS) and diethyl sulfone (ESE).
[0178] In any embodiment of the present application, the concentration of the electrolyte salt is generally 0.5 mol / L to 15 mol / L.
[0179] In any embodiment of the present application, the electrolyte may further optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives capable of improving certain battery properties, such as additives that improve battery overcharge performance, and additives that improve battery high or low temperature performance.
[0180] [Isolation film]
[0181] The separator is provided between the positive electrode sheet and the negative electrode sheet.
[0182] The present application has no particular limitation on the type of isolation membrane, and any known isolation membrane with a porous structure having good chemical stability and mechanical stability can be selected.
[0183] In some embodiments, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0184] The secondary battery further comprises a shell for packaging the positive electrode sheet, the negative electrode sheet, the separator and the electrolyte.
[0185] In some embodiments, the housing may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the housing may be a soft package, such as a bag-type soft package. The soft package may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0186] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a secondary battery 4 having a square structure as an example.
[0187] In some embodiments, referring to FIG2 , the housing may include a shell 41 and a cover 43. Shell 41 may include a bottom plate and side plates connected to the bottom plate, with the bottom plate and side plates enclosing a receiving cavity. Shell 41 may have an opening communicating with the receiving cavity, and cover 43 may be positioned over the opening to seal the receiving cavity.
[0188] The positive electrode sheet, the negative electrode sheet, and the separator can be wound or laminated to form an electrode assembly 42. The electrode assembly 42 is enclosed in a housing. The electrolyte is infiltrated into the electrode assembly 42. The battery 4 can contain one or more electrode assemblies 42, which can be adjusted based on demand.
[0189] The present application also provides an electrical device, which includes the above-mentioned secondary battery.
[0190] Furthermore, in the above-mentioned electrical device, the secondary battery may exist in the form of a battery cell, or may be further assembled into a battery pack.
[0191] Figures 3 and 4 illustrate an example battery pack 1. Battery pack 1 includes a battery case and one or more secondary batteries 4 disposed within the battery case. The battery case comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for the secondary batteries 4.
[0192] The plurality of secondary batteries 4 can be arranged in the battery box in any manner.
[0193] The secondary battery or the battery pack assembled therefrom can be used as a power source for an electrical device or as an energy storage unit for an electrical device.
[0194] The above-mentioned electrical devices may be, but are not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0195] Figure 5 shows an example of an electric device 5. The electric device 5 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device 5's requirements for high power and high energy density of the secondary battery, a battery pack can be used.
[0196] As another example, the power-consuming device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery as a power source.
[0197] The present invention will be described below with reference to specific embodiments, but the present invention is not limited to the following embodiments. It should be understood that the appended claims summarize the scope of the present invention. Under the guidance of the concept of the present invention, those skilled in the art should realize that certain changes made to the various embodiments of the present invention will be covered by the spirit and scope of the claims of the present invention.
[0198] The following are specific examples.
[0199] Specific embodiments
[0200] Example 1
[0201] (1) Mixing of negative electrode active particles:
[0202] Hard carbon particles are provided, including first hard carbon particles, second hard carbon particles and third hard carbon particles, wherein the particle sizes are T1, T2 and T3 respectively.
[0203] The Mastersizer 2000E laser particle size analyzer was used to obtain the particle size-volume cumulative distribution curves of the first, second, and third hard carbon particles, respectively, in accordance with the GB / T19077-2016 standard. The compacted density and tapped density of the powders were also measured. The specific parameters are shown in Table 1.
[0204] The hard carbon particles were mixed in a mixer according to a preset volume ratio for 4 hours to obtain mixed hard carbon particles.
[0205] The morphologies of the hard carbon particles before and after mixing were observed respectively. The electron microscope images of the hard carbon particles before mixing are shown in FIG6 , where (a) in FIG6 is an electron microscope image of the first hard carbon particles before mixing, and (b) in FIG6 is an electron microscope image of the second hard carbon particles before mixing. The electron microscope image of the hard carbon particles after mixing is shown in FIG7 .
[0206] The mixed hard carbon particles were subjected to XRD and Raman tests. The XRD results showed that the d002 peak position was 22°~24°; the Raman results showed that the peak position was 1350±50cm -1 The D peak at 1580±50cm -1 The peak intensity ratio of the G peak at I D / I G XRD and Raman both show that the hard carbon particles after mixing still have the characteristic peaks of hard carbon, and the mixing process does not destroy the structure of hard carbon.
[0207] The particle size of the mixed hard carbon particles was measured using a Mastersizer 2000E laser particle size analyzer in accordance with the standard GB / T19077-2016 to obtain its particle size-volume cumulative distribution curve. The relevant parameter results are shown in Table 4. Taking the total volume peak area of the mixed hard carbon particles as the benchmark, the volume peak area proportions of carbon-based material hard carbon particles with a particle size of less than or equal to 2 μm, hard carbon particles with a particle size greater than 2 μm and less than or equal to 25 μm, and hard carbon particles with a particle size greater than 40 μm are recorded as D1, D2, and D3, respectively. By adjusting the ratio of carbon particles at each level, the values of D1, D2, and D3 meet the relationship in Table 4.
[0208] The compacted density and tapped density of the mixed hard carbon particles were tested. The specific results are shown in Table 3.
[0209] The above-mentioned powder compaction density test is carried out under a pressure of 50,000 N with reference to the standard GB / T 24533-2009, and the above-mentioned tap density is carried out with reference to the standard GB / T 5162-2006.
[0210] The specific surface area of the mixed hard carbon particles was tested according to the standard GB / T 19587-2004 for determining the specific surface area of solid matter by gas adsorption BET method. The specific results are shown in Table 2.
[0211] (2) Preparation of negative electrode sheet:
[0212] The mixed hard carbon particles, conductive agent carbon black, binder water-soluble unsaturated resin SR-1B (alkyd unsaturated polyester resin), and thickener sodium hydroxymethyl cellulose (CMC-Na) are mixed in a weight ratio of 95:1.74:2.3:0.96, and then dispersed in solvent deionized water to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. Among them, the unit area density of the negative electrode sheet is 50g / m 2 The compaction density of the negative electrode is 1.2g / m 3 .
[0213] The compaction density and areal density of the electrode are well known in the art. The areal density of the electrode refers to the weight of the active layer per unit area of the electrode. Unit areal density = weight of active layer / area of active layer. The weight of the active layer can be calculated by subtracting the weight of the current collector from the weight of the electrode.
[0214] The electrode's compacted density, described above, refers to the ratio of the electrode's surface density to the thickness of the active layer and is a reference indicator of the material's energy density. Test method: Determine the electrode's surface density using the above method. Use a vernier caliper to measure the electrode's total thickness, then subtract the current collector thickness to calculate the active layer thickness. Based on these two parameters, the electrode's compacted density can be calculated.
[0215] The adhesion and porosity of the prepared negative electrode sheet were tested. The porosity was tested according to the standard GB / T 19587-2004. The adhesion test steps are as follows:
[0216] At 25°C, use a blade to cut a sample of 30mm wide and 100-160mm long from the negative electrode, stick a special double-sided tape on the steel plate with a width of 20mm and a length of 90-150mm, stick the cut electrode sample on the double-sided tape with the test surface facing down, and then use a roller to roll it three times in the same direction, insert a paper tape with a width equal to the electrode and a length greater than the sample length by 80-200mm under the electrode, and fix it with wrinkle glue, turn on the power of the tensile machine, the indicator light will light up, adjust the limit block to the appropriate position, and put the steel plate un Fix one end of the electrode with the lower clamp, fold the paper tape upwards, and fix it with the upper clamp. Use the "up" and "down" buttons on the manual controller that comes with the tensile testing machine to adjust the position of the upper clamp. Turn on the dedicated computer connected to the tensile testing machine, double-click the desktop software icon, and perform the test. The stretching rate is 50m / min, the test distance is 50mm, and the software takes a data point every 10s. These data point values are the vertical coordinates, and the corresponding test distance is the horizontal coordinate. The vertical coordinate reading gradually stabilizes, and the vertical coordinate reading after reading the stability is the adhesion force.
[0217] Please see Table 3 for specific test results.
[0218] (3) Preparation of positive electrode sheet:
[0219] Preparation of sodium positive electrode sheets: Prussian white positive electrode active material, conductive agent carbon black, and polyvinylidene fluoride (PVDF) are dissolved in solvent N-methylpyrrolidone in a weight ratio of 95:5:5, and mixed evenly to prepare positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode collector copper foil at one time, and the sodium ion positive electrode sheets are obtained after drying, cold pressing, and cutting.
[0220] (4) Preparation of isolation membrane: Polypropylene film was used as the isolation membrane.
[0221] (5) Preparation of electrolyte:
[0222] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), the organic solvents ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3:7, NaPF6 salt was added and dissolved in the organic solvent, and stirred evenly to obtain an electrolyte with a NaPF6 salt concentration of 12.5wt%.
[0223] (6) The sodium ion positive electrode sheet and the negative electrode sheet are sequentially cut, shaped, assembled, shelled, injected with sodium ion battery electrolyte, and subjected to formation and aging processes to prepare a lithium ion battery.
[0224] (7) Cycle performance test of sodium ion battery:
[0225] The prepared sodium ion secondary battery was repeatedly charged and discharged at 25° C., and the capacitance retention rate (capacity) after n cycles of charge and discharge was calculated as follows:
[0226] At 25°C, the sodium ion battery prepared above was charged at a constant current of 1C to a charge cut-off voltage of 4.25V, then charged at a constant voltage to a current ≤0.05C, allowed to stand for 5 minutes, and then discharged at a constant current of 0.33C to a discharge cut-off voltage of 2.8V, allowed to stand for 5 minutes, and the capacity C0 at this time was recorded. This is one charge and discharge cycle.
[0227] The battery was subjected to a cyclic charge-discharge test for 500 cycles, and the discharge capacity at each cycle was recorded. The capacity at 500 cycles was recorded as C500, where C500 = (C500 / C0) × 100%. See Table 4 for the specific results.
[0228] (8) Initial performance test of sodium ion batteries:
[0229] At 25°C, discharge the corresponding battery at a constant current of 0.05C to 5mV, then discharge it at a constant voltage of 50μA to 5mV, let it rest for 1 hour, and then discharge it at 10μA to 5mV. The resulting capacity is recorded as the discharge capacity C0. Let it rest for another 1 hour, and then charge it at a cross current of 0.05C to 2V. The resulting capacity is recorded as the charge capacity C1. The initial coulombic efficiency P0 = C1 / C0*100%.
[0230] Please see Table 3 for specific results.
[0231] Examples 2 to 12
[0232] Examples 2 to 12 are substantially the same as Example 1, with the only difference being that the volume ratio of each hard carbon particle during the mixing of the negative electrode active particles in step (1) is controlled, so that some parameters of the mixed hard carbon particles in Examples 2 to 12 are different from those in Example 1. See Table 2 for details.
[0233] Examples 13 to 15
[0234] Examples 13 to 15 are substantially the same as Example 1, except that in step (1) of mixing the negative electrode active particles in Examples 13 to 15, the mixing times were 0.5 h, 2 h, and 8 h, respectively, resulting in some parameters of the mixed hard carbon particles in Examples 13 to 15 being different from those in Example 1. See Table 2 for details.
[0235] Comparative Example 1
[0236] Comparative Example 1 is basically the same as Example 1, except that the volume ratio of each hard carbon particle in the mixing of the negative electrode active particles in step (1) is adjusted so that some parameters of the mixed hard carbon particles in Comparative Example 1 are different from those in Example 1.
[0237] Please see Table 2 for details.
[0238] The parameters of the first hard carbon particles, the second hard carbon particles, and the third hard carbon particles used in each embodiment and comparative example are shown in Table 1.
[0239] Table 1
[0240]
[0241]
[0242] In the above table, “()” indicates that the value range in the brackets cannot take the endpoint values on both sides, “[]” indicates that the value range in the brackets can take the endpoint values on both sides, and “(]” or “[)” indicates that the value range in the brackets can take the endpoint value at the “[” end but cannot take the endpoint value at the “)” end.
[0243] The parameters of the mixed hard carbon particles of each embodiment and comparative example are shown in Table 2, and the negative electrode sheet parameters and performance test results of the sodium ion battery are shown in Table 3.
[0244] In Table 2, based on the total volume peak area of the mixed hard carbon particles, D1 represents: the volume peak area ratio of the first hard carbon particles having a particle size of less than or equal to 2 μm, D2 represents: the volume peak area ratio of the second hard carbon particles having a particle size greater than 2 μm and less than or equal to 25 μm, and D3 represents: the volume peak area ratio of the third hard carbon particles having a particle size greater than 40 μm.
[0245] Table 2
[0246]
[0247]
[0248] Table 3
[0249]
[0250]
[0251] It can be seen from the data in Table 3 that the negative electrode active material of the negative electrode film layer in the negative electrode sheet is controlled to contain a carbon-based material with a specific particle size range, and its volume proportion in the negative electrode active material is regulated, thereby increasing the contact area between the negative electrode active particles and making the negative electrode active particles closely stacked, thereby improving the adhesion of the negative electrode sheet, and further improving the first efficiency and cycle performance of the secondary battery.
[0252] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application, and they should all be included in the scope of the claims and specification of the present application. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A secondary battery comprising a negative electrode plate, the negative electrode plate comprising a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer comprising a negative electrode active material, and the negative electrode active material comprising a carbon-based material; In the negative electrode active material, the volume proportion of the first carbon-based material having a particle size of less than or equal to 2 μm is greater than or equal to 15%.
2. The secondary battery according to claim 1, wherein In the negative electrode active material, the volume proportion of the first carbon-based material is 20% to 70%, and can be optionally 30% to 60%.
3. The secondary battery according to claim 1 or 2, wherein The first carbon-based material satisfies at least one of the following conditions (1) to (7): (1) the volume distribution particle size Dv10 of the first carbon-based material is 0.2 μm to 0.5 μm; (2) the volume distribution particle size Dv50 of the first carbon-based material is 0.5 μm to 2 μm; (3) the volume distribution particle size Dv90 of the first carbon-based material is ≤ 2 μm; (4) The specific surface area SSA of the first carbon-based material is 5 m 2 / g~20m 2 / g; (5) In the Raman spectrum test of the first carbon-based material, I D / I G 0.95~1.35; (6) The powder compaction density of the first carbon-based material under a force of 50,000 N is 0.8 g / cm 3 ~1.1g / cm 3 ; (7) The tap density of the first carbon-based material is 0.3 g / cm 3 ~0.8g / cm 3 .
4. The secondary battery according to any one of claims 1 to 3, wherein In the negative electrode active material, the volume proportion of the second carbon-based material with a particle size greater than 2 μm and less than or equal to 25 μm is 20% to 80%, and can be optionally 50% to 60%.
5. The secondary battery according to claim 4, wherein The second carbon-based material satisfies at least one of the following conditions (I) to (VIII): (I) the volume particle size distribution of the second carbon-based material is unimodal; (II) the volume distribution particle size Dv10 of the second carbon-based material is 2 μm to 4 μm; (III) the volume distribution particle size Dv50 of the second carbon-based material is 4 μm to 8 μm; (IV) the volume distribution particle size Dv90 of the second carbon-based material is 8 μm to 20 μm; (V) the volume distribution particle size Dv99 of the second carbon-based material is 20 μm to 25 μm; (VI) The specific surface area SSA of the second carbon-based material is 1 m 2 / g~10m 2 / g; (VII) The powder compaction density of the second carbon-based material under a force of 50,000 N is 0.92 g / cm 3 ~1.2g / cm 3 ; (VIII) The tap density of the second carbon-based material is 0.6 g / cm 3 ~0.94g / cm 3 .
6. The secondary battery according to any one of claims 1 to 5, wherein In the negative electrode active material, the volume proportion of the third carbon-based material having a particle size greater than 40 μm and less than or equal to 100 μm is less than or equal to 10%; optionally, less than or equal to 5%.
7. The secondary battery according to claim 6, wherein The third carbon-based material satisfies at least one of the following conditions (1) to (4): (1) The specific surface area SSA of the third carbon-based material is 1 m 2 / g~10m 2 / g; (2) In the Raman spectrum test of the third carbon-based material, I D / I G 0.95~1.35; (3) The powder compaction density of the third carbon-based material under a force of 50,000 N is 0.7 g / cm 3 ~1g / cm 3 ; (4) The tap density of the third carbon-based material is 0.5 g / cm 3 ~0.8g / cm 3 .
8. The secondary battery according to any one of claims 1 to 7, wherein The volume distribution particle size Dv50 of the negative electrode active material is less than or equal to 8 μm; optionally, the volume distribution particle size Dv50 of the negative electrode active material is 2 μm to 6 μm.
9. The secondary battery according to any one of claims 1 to 8, wherein The volume distribution particle size of the negative electrode active material satisfies: 4 μm≤Dv90≤20 μm; optionally, 5 μm≤Dv90≤16 μm.
10. The secondary battery according to any one of claims 1 to 9, wherein The volume distribution particle size Dv10 of the negative electrode active material satisfies: 0.2 μm≤Dv10≤2 μm; optionally, 0.5 μm≤Dv10≤1.8 μm.
11. The secondary battery according to any one of claims 1 to 10, wherein The specific surface area SSA of the negative electrode active material is less than or equal to 20 m 2 / g; optionally, SSA≤10m 2 / g.
12. The secondary battery according to any one of claims 1 to 11, wherein In the Raman spectrum test of the negative electrode active material, I D / I G It is 0.87~1.35; it can be selected as 0.91~1.
25.
13. The secondary battery according to any one of claims 1 to 12, wherein In the X-ray diffraction test of the negative electrode active material, there is a (002) crystal plane peak in the range of 22° to 24°, and the interlayer spacing of the (002) crystal plane of the negative electrode active material is ≥0.37nm, and can be selected from 0.37nm to 0.42nm.
14. The secondary battery according to any one of claims 1 to 13, wherein The powder compaction density of the negative electrode active material under a force of 50,000 N is 0.90 g / cm 3 ~1.5g / cm 3 ; Optional 0.95g / cm 3 ~1.3g / cm 3 .
15. The secondary battery according to any one of claims 1 to 14, wherein The tap density of the negative electrode active material is 0.50 g / cm 3 ~0.97g / cm 3 ; Optional 0.6g / cm 3 ~0.94g / cm 3 .
16. The secondary battery according to any one of claims 1 to 15, wherein The carbon-based material includes a plurality of nanopore structures. Optionally, the carbon-based material includes a plurality of pore structures with a pore diameter of less than 10 nm.
17. The secondary battery according to any one of claims 1 to 16, wherein The carbon-based material includes a hard carbon material.
18. The secondary battery according to any one of claims 1 to 17, wherein The secondary battery is a sodium ion secondary battery.
19. An electric device comprising the secondary battery according to any one of claims 1 to 18.
Citation Information