Modified biochar composite material for improving saline-alkali soil and preparation method of modified biochar composite material
By carbonizing and impregnating crop straw, modified biochar composite materials with high adsorption performance were prepared, which solved the problem of poor adsorption performance of existing biochar in saline-alkali land improvement, and significantly improved the adsorption capacity and soil improvement effect.
Patent Information
- Application Number
- CN202410922855.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
In the improvement of existing biochar, there are problems of poor selection adsorption performance and small specific surface area in saline-alkali land, which affects the adsorption efficiency and ability.
After pretreating crop straw and carbonizing in a pyrolysis furnace, biochar is placed in a mixture of CaCl2 and hexamethylenetetramine, and pyrolytic activation is performed for high-temperature pyrolysis and combined with pickling treatment, the preparation is prepared Modified biochar composite materials with a large specific surface area and strong adsorption capacity are produced.
It significantly improves the adsorption capacity and specific surface area of biochar, enhances the adsorption capacity of metal ions, reduces the pH of saline-alkali soil, improves the physical and chemical properties of the soil, improves the crop germination rate, and realizes the recycling and utilization of plant straw.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of soil improvement, and in particular to a modified biochar composite material for improving saline-alkali land and a preparation method thereof. Background Art
[0002] Biochar, also known as biomass charcoal, is a solid substance formed by thermal cracking of biomass raw materials such as crop straw, livestock and poultry manure, waste wood chips and sludge under oxygen-deficient or oxygen-limited conditions. Biochar prepared from different biomass materials has different names, such as straw charcoal, charcoal and bamboo charcoal. Its composition includes C, H, N, O, ash, carbohydrates, minerals and inorganic carbonates, and the carbon content accounts for 70-80% of the total. According to the classification of biomass components, it can be roughly divided into cellulose-based biochar, hemicellulose-based biochar and lignin-based biochar. Biochar is alkaline, has a high specific surface area, and a highly aromatic structure. Its surface honeycomb structure and strong chemical electrolytic activity can enrich a large number of functional groups such as carboxyl, quinone and phenolic hydroxyl groups. It is a good adsorbent and has strong adsorption for organic matter and heavy metals. Biochar can be used as a carbon fixer, soil conditioner, hygroscopic agent, i.e., heavy metal adsorption stabilizer, etc., and is greatly affected by raw materials and pyrolysis temperature. As an emerging material, biochar has the characteristics of wide sources, low cost and excellent properties. The structure of biochar is stable and it can exist in the soil for thousands of years. It is an ideal soil remediation material.
[0003] For example, Chinese patent CN114891512A discloses a saline-alkali land improved calcium chloride-loaded biochar composite material and its preparation method, which includes the following steps: 1) Collecting plant raw materials, washing with deionized water and then completely drying, then oxygen-limited cracking at 450°C for 1h, cooling and crushing the biochar with a pulverizer to obtain raw biochar; mixing the raw biochar with a calcium chloride solution with a concentration of 0.5 mol / L at a solid-liquid ratio of 1:15 (g:mL); then fully stirring under a constant temperature oscillator, filtering out and washing with ultrapure water until the pH of the washing liquid is stable in conductivity; 3) After completely drying at a certain temperature, oxygen-limited cracking at 200°C for 1h, the resulting product is marked as a biochar-loaded calcium chloride-modified biochar composite material. The invention can effectively reduce the pH in saline-alkali soil, improve the physical and chemical properties of the soil, increase the germination rate of plants, has low cost, and will not cause secondary pollution, which is conducive to the development and utilization of saline-alkali land, maintaining the stability of existing cultivated land, and protecting the ecological environment.
[0004] For example, Chinese patent CN113145076A discloses a method for preparing modified biochar and modified biochar, which includes the following steps: pre-treating crop straw; immersing the pre-treated crop straw powder in an iron oxide suspension, heating, stirring, shaking, and drying; pyrolyzing the above substances to obtain the modified biochar. The modified biochar obtained by the invention has a large specific surface area and has a good adsorption capacity for anions.
[0005] However, the existing biochar still has the defects of poor selective adsorption performance and small specific surface area, which affects the adsorption efficiency and capacity of biochar for specific technical elements. Therefore, it is necessary to develop a modified biochar composite material with strong selective adsorption performance, large specific surface area and large adsorption capacity for saline-alkali land improvement and its preparation method. Summary of the invention
[0006] Based on the deficiencies in the prior art, the present invention aims to provide a modified biochar composite material for improving saline-alkali land with strong selective adsorption performance, large specific surface area and large adsorption capacity, and a preparation method thereof.
[0007] The present invention controls the activating agent, the pyrolysis temperature and the pyrolysis rate so that the obtained biochar has a strong adsorption ability, a large adsorption capacity and a large specific surface area, and can be applied to the improvement of saline-alkali land.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] In one aspect, the present invention provides a method for preparing a modified biochar composite material for improving saline-alkali land, comprising the following steps:
[0010] (1) Pre-treating crop straw;
[0011] (2) placing the pretreated crop straw in a pyrolysis furnace for carbonization to obtain biochar;
[0012] (3) impregnating the biochar obtained in step (2) in a mixed solution of CaCl2 and hexamethylenetetramine to obtain impregnated biochar;
[0013] (4) drying the impregnated biochar obtained in step (3), placing it in a pyrolysis furnace for pyrolysis activation, and then cooling it to obtain modified biochar;
[0014] (5) The modified biochar obtained in step (4) is acid-washed and then washed with deionized water until it becomes neutral to obtain the modified biochar composite material.
[0015] The crop straw described in step (1) is selected from one or more of corn straw, wheat straw, rice straw and sorghum straw; preferably rice straw.
[0016] The pretreatment described in step (1) is to clean the crop straw and then dry it.
[0017] Step (2) and step (3) need to be carried out under the protection of an inert gas, wherein the inert gas is nitrogen.
[0018] The heating rate of the carbonization treatment in step (2) is 3-6°C / min, preferably 4-5°C / min, and more preferably 4°C / min; the temperature is raised to 320-380°C, preferably 370°C; the insulation time is 1-2h, preferably 1.5h.
[0019] The present invention controls the heating rate, carbonization temperature and insulation time during the initial carbonization process, so that the crop straw is heated more evenly, and the pyrolysis and carbonization reaction can occur better and more evenly, thereby forming a stable carbon skeleton and obtaining better quality biochar.
[0020] The mass ratio of the biochar to the mixed liquid in step (3) is 1-2.5:1; preferably 1.5:1; the mass ratio of CaCl2 to hexamethylenetetramine is 1-3:1; preferably 1.5-2.5:1; more preferably 2.5:1.
[0021] The biochar was impregnated with a mixture of CaCl2 and hexamethylenetetramine. The addition of CaCl2 can load Ca on the biochar composite material. 2+ At the same time, it can increase the carbonate minerals on the surface of biochar and provide more cationic adsorption sites; while hexamethylenetetramine can dope biochar with nitrogen atoms, which can enhance the interaction between the carbon structure and the active center.
[0022] The immersion time in step (3) is 12-24 hours, preferably 18 hours, and the immersion temperature is 25-35°C, preferably 30°C.
[0023] During the impregnation process, the biochar is brought into contact with the activator by controlling the impregnation temperature and time, which helps the activator to diffuse better and more evenly into the interior of the biochar, thereby greatly improving the performance of the biochar.
[0024] The drying in step (4) is carried out at a temperature of 100-120° C., preferably 110° C., and for a time of 15-20 hours, preferably 18 hours.
[0025] The heating rate of the pyrolysis in step (4) is 5-12°C / min, preferably 8-10°C / min, and more preferably 10°C / min. The temperature is raised to 800-950°C, preferably 900°C. The holding time is 3-5h, preferably 4h.
[0026] In step (4), high temperature pyrolysis activation is used to make the obtained activated carbon composite material have a developed pore structure, a large specific surface area, and a suitable pore size structure ratio, so that the biochar has better adsorption ability and adsorption capacity.
[0027] The cooling rate in step (4) is 3-8°C / min, preferably 6°C / min.
[0028] In step (4), a uniform cooling method is adopted to avoid excessive local cooling speed, which may cause the collapse or destruction of the biochar pores, thereby ensuring the uniformity and integrity of the biochar pores.
[0029] In step (5), the modified biochar activated carbon is acid-washed, and the acid is hydrochloric acid with a concentration of 1-2 mol / L, preferably 1.5 mol / L.
[0030] In this step, the modified biochar is acid-washed and water-washed to remove impurities and unreacted active agents on the biochar and make the pore structure more complete.
[0031] On the other hand, the present invention also provides a modified biochar composite material prepared by the above method.
[0032] In another aspect, the present invention also provides the use of the modified biochar composite material prepared by the above method in the preparation of a soil conditioner.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) In the initial carbonization process, the present invention controls the heating rate, carbonization temperature and insulation time to make the crop straw heated more evenly, so that the pyrolysis and carbonization reaction can occur better and more evenly, thereby forming a stable carbon skeleton and obtaining better quality biochar.
[0035] (2) The present invention uses a mixed solution of CaCl2 and hexamethylenetetramine to impregnate the biochar. The addition of CaCl2 can load Ca on the biochar composite material. 2+ At the same time, it can increase the carbonate minerals on the surface of biochar and provide more cationic adsorption sites; while hexamethylenetetramine can dope biochar with nitrogen atoms, which can enhance the interaction between the carbon structure and the active center.
[0036] (3) The present invention adopts high temperature pyrolysis activation in the preparation process so that the obtained activated carbon composite material has a developed pore structure, a large specific surface area, and a suitable pore size structure ratio, so that the biochar has better adsorption ability and adsorption capacity.
[0037] (4) The biochar composite material prepared by the present invention can better reduce the pH of saline-alkali soil, improve the physical and chemical properties of soil, have a stronger adsorption capacity for metal ions in the soil, reduce soil conductivity, increase crop germination rate, promote plant growth, and at the same time achieve the effect of recycling plant straw and plant waste. DETAILED DESCRIPTION
[0038] Below, in conjunction with specific implementation modes, the present invention is further described:
[0039] In the present invention, unless otherwise specified, the equipment and raw materials used can be purchased from the market or are commonly used in the art. The methods in the following embodiments, unless otherwise specified, are all conventional methods in the art.
[0040] Example 1 A modified biochar composite material for improving saline-alkali land
[0041] Prepared by the following method:
[0042] (1) Clean the corn stalks and dry them for later use;
[0043] (2) placing the pretreated crop straw in a pyrolysis furnace for carbonization treatment under nitrogen protection, heating the temperature to 320°C at a rate of 3°C / min, and keeping the temperature for 3 hours to obtain biochar;
[0044] (3) placing the biochar obtained in step (2) in a mixed solution of CaCl2 and hexamethylenetetramine (mass ratio of 1:1) at 35°C for 12 hours to obtain impregnated biochar; the mass ratio of biochar to the mixed solution is 1:1;
[0045] (4) drying the impregnated biochar obtained in step (3) at 100° C. for 20 hours, placing it in a pyrolysis furnace for pyrolysis activation under nitrogen protection, heating it to 800° C. at a rate of 5° C. / min, keeping it at that temperature for 5 hours, and then cooling it at a rate of 3° C. / min to obtain modified biochar;
[0046] (5) The modified biochar obtained in step (4) is acid-washed with 1 mol / L hydrochloric acid, and then washed with deionized water until it becomes neutral, thereby obtaining the modified biochar composite material.
[0047] Example 2 A modified biochar composite material for improving saline-alkali land
[0048] Prepared by the following method:
[0049] (1) Clean the wheat straw and dry it for later use;
[0050] (2) placing the pretreated crop straw in a pyrolysis furnace for carbonization treatment under nitrogen protection, heating the temperature to 380°C at a rate of 6°C / min, and keeping the temperature for 1 hour to obtain biochar;
[0051] (3) placing the biochar obtained in step (2) in a mixed solution of CaCl2 and hexamethylenetetramine (mass ratio of 3:1) at 25°C for 24 hours to obtain impregnated biochar; the mass ratio of biochar to the mixed solution is 2.5:1;
[0052] (4) drying the impregnated biochar obtained in step (3) at 120° C. for 20 hours, placing it in a pyrolysis furnace for pyrolysis activation under nitrogen protection, heating it to 950° C. at a rate of 12° C. / min, keeping it at that temperature for 3 hours, and then cooling it at a rate of 8° C. / min to obtain modified biochar;
[0053] (5) The modified biochar obtained in step (4) is acid-washed with 2 mol / L hydrochloric acid, and then washed with deionized water until it becomes neutral, thereby obtaining the modified biochar composite material.
[0054] Example 3 A modified biochar composite material for improving saline-alkali land
[0055] Prepared by the following method:
[0056] (1) cleaning the rice straw and drying it for later use;
[0057] (2) placing the pretreated crop straw in a pyrolysis furnace for carbonization treatment under nitrogen protection, heating the temperature to 370°C at a rate of 4°C / min, and keeping the temperature for 2 hours to obtain biochar;
[0058] (3) placing the biochar obtained in step (2) in a mixed solution of CaCl2 and hexamethylenetetramine (mass ratio of 2.5:1) at 30°C for 18 hours to obtain impregnated biochar; the mass ratio of biochar to the mixed solution is 1.5:1;
[0059] (4) drying the impregnated biochar obtained in step (3) at 110° C. for 18 hours, placing it in a pyrolysis furnace for pyrolysis activation under nitrogen protection, heating at a rate of 10° C. / min to 900° C., keeping the temperature for 4 hours, and then cooling at a rate of 6° C. / min to obtain modified biochar;
[0060] (5) The modified biochar obtained in step (4) is acid-washed with 1.5 mol / L hydrochloric acid, and then washed with deionized water until it becomes neutral, thereby obtaining the modified biochar composite material.
[0061] Comparative Example 1
[0062] The difference from Example 3 is that the impregnation solution only contains CaCl2, and the other steps and operations are the same as those in Example 3.
[0063] Comparative Example 2
[0064] The difference from Example 3 is that CaCl2 is replaced by ZnCl2, and the other steps and operations are the same as those in Example 3.
[0065] Comparative Example 3
[0066] The difference from Example 3 is that the mass ratio of CaCl2 to hexamethylenetetramine is 1:2, and the other steps and operations are the same as those in Example 3.
[0067] Comparative Example 4
[0068] The difference from Example 3 is that the heating rate of pyrolysis in step (4) is 10°C / min, the temperature is 550°C, and the other steps and operations are the same as those in Example 3.
[0069] Comparative Example 5
[0070] The difference from Example 3 is that in step (4), the pyrolysis is carried out by first heating the temperature to 500°C at a rate of 5°C / min and keeping the temperature for 1 hour, then heating the temperature to 800°C at a rate of 10°C / min and keeping the temperature for 2 hours. The other steps and operations are the same as those in Example 3.
[0071] Performance data
[0072] 1. Detection of metal ion adsorption by biochar composite materials
[0073] Take the biochar composite materials prepared in Examples 1-3 and Comparative Example 15, weigh 0.05 g of the biochar composite material sample in a 50 mL centrifuge tube, add 30 mL of 100 mg / L Cu 2+ Cr 3+ and Pb 2+ The solution was shaken at 25°C and 150 r / min for 3 h, centrifuged at 3500 r / min for 5 min, the supernatant was filtered, and the Cu 2+ Cr 3+ and Pb 2+ The adsorption amount was calculated and the results are shown in Table 1 below.
[0074] Table 1
[0075] <![CDATA[Cu 2+ Adsorption capacity (mg / g)]]> <![CDATA[Cr 3+ Adsorption capacity (mg / g)]]> <![CDATA[Pb 2+ Adsorption capacity (mg / g)]]> Example 1 45.86 48.26 65.82 Example 2 46.21 47.32 66.40 Example 3 48.96 50.43 68.71 Comparative Example 1 40.28 42.51 56.14 Comparative Example 2 42.53 44.16 60.45 Comparative Example 3 42.82 43.95 61.83 Comparative Example 4 38.45 40.72 54.14 Comparative Example 5 40.16 41.64 53.85
[0076] According to the test data in Table 1 above, the biochar composite material prepared by the present invention has a better adsorption effect on Cu 2+ Cr 3+ and Pb 2+ All of them have good adsorption properties and high adsorption efficiency. In Examples 1-3, changing the type of impregnation solution components will affect the adsorption effect of the biochar composite material; in Examples 4-5, changing the temperature or heating method during the pyrolysis process will affect the formation of biochar, and then affect the adsorption effect of the biochar composite material.
[0077] 2. Test on soil improvement performance
[0078] 50 g of the biochar composite materials prepared in Examples 1-3 and Comparative Examples 1-5 were respectively added to 1000 g of saline-alkali soil, and a 90-day greenhouse soil culture test was carried out. Samples were taken on the 90th day to measure the soil pH and conductivity. The test results are shown in Table 2 below.
[0079] Table 2
[0080] pH Conductivity (μS / cm) Blank Sample 10.5 1254.82 Example 1 9.4 526.41 Example 2 9.3 489.35 Example 3 9.0 368.72 Comparative Example 1 9.7 824.63 Comparative Example 2 9.5 887.15 Comparative Example 3 9.5 896.42 Comparative Example 4 9.4 927.64 Comparative Example 5 9.5 938.71
[0081] According to the test data in Table 2 above, the biochar composite materials prepared in Examples 1-3 of the present invention are more capable of reducing the pH of saline-alkali soil and improving the physical and chemical properties of soil. Since the prepared biochar composite materials have stronger adsorption capacity for metal ions, as shown in Table 1, the soil conductivity can be better reduced.
[0082] 3. Germination rate test
[0083] 1000g of saline-alkali soil was taken and naturally matured for 40 days. 50g of biochar composite material was added to the saline-alkali soil, and sunflower seeds were sown for 60 days to measure the germination rate. The test results are shown in Table 3 below.
[0084] Table 3
[0085] Germination rate% Blank Sample 51.4 Example 1 95.8 Example 2 98.2 Example 3 100 Comparative Example 1 80.4 Comparative Example 2 85.7 Comparative Example 3 88.2 Comparative Example 4 75.4 Comparative Example 5 76.3
[0086] According to the test results in Table 3, it can be seen that the biochar composite materials prepared in Examples 1-3 of the present invention are better able to reduce the pH of saline-alkali soil and improve the physical and chemical properties of soil, thereby being more conducive to plant growth. The germination rate of plants in the soil improved by the biochar composite materials is significantly improved.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for preparing a modified biochar composite material for improving saline-alkali land, characterized in that: The steps include: (1) Pre-treating crop straw; (2) placing the pretreated crop straw in a pyrolysis furnace for carbonization to obtain biochar; (3) impregnating the biochar obtained in step (2) in a mixed solution of CaCl2 and hexamethylenetetramine to obtain impregnated biochar; (4) drying the impregnated biochar obtained in step (3), placing it in a pyrolysis furnace for pyrolysis activation, and then cooling it to obtain modified biochar; (5) The modified biochar obtained in step (4) is acid-washed and then washed with deionized water until it becomes neutral to obtain the modified biochar composite material.
2. The preparation method according to claim 1, characterized in that: The heating rate of the carbonization treatment in step (2) is 3-6°C / min; the temperature is raised to 320-380°C; and the insulation time is 1-3h.
3. The preparation method according to claim 2, characterized in that: The heating rate of the carbonization treatment in step (2) is 4°C / min; the temperature is raised to 370°C; and the insulation time is 2h.
4. The preparation method according to claim 1, characterized in that: The mass ratio of the biochar to the mixed liquid in step (3) is 1-2.5:
1.
5. The preparation method according to claim 4, characterized in that: The mass ratio of the biochar to the mixed liquid in step (3) is 1.5:
1.
6. The preparation method according to claim 1, characterized in that: The mass ratio of CaCl2 to hexamethylenetetramine described in step (3) is 1-3:
1.
7. The preparation method according to claim 1, characterized in that: The mass ratio of CaCl2 to hexamethylenetetramine described in step (3) is 2.5:
1.
8. The preparation method according to claim 1, characterized in that: The heating rate of the pyrolysis in step (4) is 5-12°C / min, preferably 8-10°C / min, and more preferably 10°C / min. The temperature is raised to 800-950°C, preferably 900°C. The holding time is 3-5h, preferably 4h.
9. A modified biochar composite material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of a modified biochar composite material prepared by the preparation method according to any one of claims 1 to 8 in preparing a soil conditioner.
Citation Information
Patent Citations
Calcium chloride-loaded modified charcoal composite material for improving saline-alkali soil and preparation method thereof
CN114891512A
Broussonetia papyrifera charcoal and preparation method thereof, and broussonetia papyrifera charcoal-based soil heavy metal mineralizer and application thereof
CN116673031A
Cited By
Cow dung biochar composite material for saline-alkali soil improvement, preparation method and application
CN120305933A
Preparation method of modified charcoal-based material and application of modified charcoal-based material in saline-alkali soil improvement
CN120423526A
Soil environment remediation type charcoal-based organic fertilizer and preparation method thereof