Aminophosphonate modified conductive polymer material and use thereof for thorium enrichment

The efficient adsorption and separation of thorium ions are achieved through aminophosphonate modified conductive polymer materials in capacitance deionization technology, solving the problem of insufficient adsorption capacity and selectivity in the traditional method, and achieving efficient enrichment and separation of thorium. And support the recycling of the device.

CN118874428AActive Publication Date: 2024-11-01GANJIANG INNOVATION ACAD CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410908619.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

During the enrichment and separation of thorium, traditional solvent extraction and adsorption methods have problems such as insufficient extraction agent, long extraction equilibrium time, high solvent requirements, and insufficient adsorption capacity and selectivity in the process of thorium, which limits its application expansion.

Method used

Design and prepared an aminophosphonate modified conductive polymer material, which efficient adsorption and separation of thorium ions through capacitive deionization technology, and combines conductive polymer matrix with aminophosphonate compounds to achieve the thorium ions. Selective adsorption.

Benefits of technology

It achieves high adsorption capacity and selectivity, effectively enrich and separate thorium ions, suitable for efficient enrichment and separation of low concentrations of thorium, and the loaded capacitive deionization device can be recycled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874428A_ABST
    Figure CN118874428A_ABST
Patent Text Reader

Abstract

The invention relates to an aminophosphonate modified conductive polymer material and application thereof to thorium enrichment. The aminophosphonate modified conductive polymer material comprises: a conductive polymer matrix; the compound is doped and combined with the conductive polymer matrix, wherein R1 is selected from C1-C12 alkylene; r < 2 > and R < 3 > are respectively and independently selected from hydrogen, C1-C8 alkyl groups, C3-C10 cycloalkyl groups and C6-C10 aryl groups; and R4 and R5 are respectively and independently selected from alkyl groups with 1 to 16 carbon atoms and aryl groups with 6 to 10 carbon atoms. The amino phosphonate modified conductive polymer material has high adsorption capacity on thorium ions in a capacitive deionization technology, and can be applied to selective adsorption of thorium in a thorium and rare earth-containing mixed feed liquid. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thorium enrichment, and particularly relates to an aminophosphonate modified conductive polymer material and use thereof in enriching thorium. Background Art

[0002] Thorium, as a rare earth mineral associated element, can be transferred through the soil layer to the water layer, atmosphere and biological layer. Radioactive nuclides in the soil and water enter the body of organisms after being absorbed by animals and plants, and then continue to accumulate in the human body through the food chain, eventually causing great damage to the human body. In the nuclear industry, potential nuclear fuel can be used 232 Th makes nuclear fuel 233 U: Thermal neutron impact 232 Th is formed first 233 Th, which then decays to form 233 U. 233 U and natural 235 U can also release a large amount of nuclear fission energy. 232 If Th can be used as a substitute for uranium, it will greatly increase my country's nuclear fuel reserves. Therefore, it is of great practical significance to remove radioactive thorium from rare earths and enrich trace thorium.

[0003] Solvent extraction is a method of separating a mixture by using the difference in solubility of different components in a solvent. Solvent extraction is an important method for enriching and separating thorium, but there are still problems such as the imperfect demulsification technology of the extractant in the extraction process, the long extraction equilibrium time, and the high requirements of the extractant for the solvent extract, which limits the application of the extraction method in other directions. In comparison, the adsorption method has become a method for separating and purifying thorium that is being studied more at this stage due to its high efficiency, low cost, and practicality.

[0004] CN104766643A discloses a method for removing thorium ions from rare earth smelting wastewater using urea-formaldehyde resin. The initial concentration of thorium ions is 200 mg / L, the solution volume is 100 mL, 10 g of urea-formaldehyde (UF) resin is added, and the adsorption temperature is 25°C. After 6 hours of adsorption, the adsorption capacity of UF resin for thorium ions is 13.78 mg / g.

[0005] CN116550307A discloses a method for preparing a micro-membrane adsorption material for rapid and efficient adsorption of radioactive nuclide thorium ions. Studies have shown that the saturated adsorption capacity of ZIF-67@PA micro-membrane adsorption material for Th(IV) within 50 minutes is 703.59 mg / g, and after being reused 7 times, it still has an ultra-high adsorption capacity.

[0006] CN109174060A discloses a phosphonic acid group-containing chelating resin, which is prepared by solvent thermal polymerization of di(methacryloyloxyethyl) hydrogen phosphate. Under the premise of a raw material liquid volume of 25 mL and a concentration of 100 ppm, the adsorption capacity of thorium is 85.2 mg / g.

[0007] CN103589866A discloses a method for separating and recovering thorium and uranium using a silicon-based anion exchange resin. In a nitric acid system, an anion exchange resin is added to perform ion exchange adsorption, and after the ion exchange is completed, the thorium adsorbed on the anion exchange resin is eluted with an eluent, thereby achieving separation and recovery of thorium and uranium.

[0008] However, traditional adsorption methods are difficult to meet the high adsorption capacity and high selectivity of target metal ions, and have high requirements on experimental conditions, material stability, adsorption equilibrium time, cycle practicality and acidity of the feed solution, which further limits its expanded application. Summary of the invention

[0009] In view of the shortcomings of the above-mentioned solvent extraction method and adsorption method, the present invention designs and prepares an aminophosphonate modified conductive polymer material, and applies it to the capacitive deionization technology to further enrich and separate thorium ions. Experimental verification shows that the material has a high adsorption capacity for thorium ions in the capacitive deionization technology, and can be used to selectively adsorb thorium in a mixed liquid containing thorium and rare earth, thereby completing the present invention.

[0010] In one aspect, the present invention provides an aminophosphonate-modified conductive polymer material comprising:

[0011] (1) Conductive polymer matrix;

[0012] (2) Compounds of formula I doped with conductive polymer matrix:

[0013]

[0014] in,

[0015] R1 is selected from C1~C 12 Alkylene;

[0016] R2 and R3 are each independently selected from hydrogen, C1-C8 alkyl, C3-C 10 Cycloalkyl, and C6~C 10 Aryl;

[0017] R4 and R5 are each independently selected from C1 to C 16 Alkyl and C6~C 10 Aryl.

[0018] In some embodiments, the conductive polymer matrix is ​​selected from polyaniline and polypyrrole.

[0019] In some embodiments, the compound of formula I may be doped and combined with the conductive polymer matrix through the interaction of positive and negative charges. In this case, the compound of formula I may exist in the material as the following structure:

[0020]

[0021] Wherein, "*" indicates that the compound of formula I is doped and combined with the conductive polymer.

[0022] In addition to the positive and negative charge effects, the compound of formula I may also be doped and combined with the conductive polymer matrix in various ways, such as through van der Waals forces, hydrogen bonds, etc. Therefore, the present invention does not specifically limit the doping and combining method of the compound of formula I with the conductive polymer matrix.

[0023] In some embodiments, R1 is selected from C1 to C 10 Alkylene, for example C1-C8 alkylene or C1-C6 alkylene.

[0024] In some embodiments, R2 and R3 are the same or different. In some embodiments, R2 and R3 are each independently selected from hydrogen, C1-C6 alkyl, C5-C8 cycloalkyl and C6-C8 aryl.

[0025] In some embodiments, R4 and R5 are the same or different. In some embodiments, R4 and R5 are each independently selected from C2 to C 14 Alkyl and C6-C8 aryl, more preferably C3-C 12 Alkyl and C6~C8 aryl.

[0026] The terms C1 to C2 used in the present invention are 16 Alkyl refers to a straight or branched chain alkyl group containing 1 to 16 carbon atoms, such as a straight or branched chain alkyl group having 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 or 16 carbon atoms, including but not limited to methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, isobutyl, n-pentyl, neopentyl, isopentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, etc. 12 Alkyl, C1~C 10 Alkyl, C1-C8 alkyl, C1-C6 alkyl, C2-C 14 Alkyl and C3~C 12 The meaning of alkyl is similar.

[0027] The terms C1 to C2 used in the present invention are 16Alkylene refers to the above C1~C 16 The alkyl group loses another hydrogen atom to form a divalent group.

[0028] The terms C3 to C4 used in the present invention 10 Cycloalkyl refers to a saturated cyclic alkyl group containing 3 to 10 carbon atoms including the carbon atoms of the substituent, and the saturated cyclic alkyl group may be a monocyclic or bicyclic group, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, etc., and the substituent may be one or more substituents selected from C1 to C4 alkyl. The meaning of C5 to C8 cycloalkyl, etc. is similar.

[0029] The terms C6 to C 10 Aryl refers to an aromatic group containing 6 to 10 carbon atoms including the carbon number of the substituent, such as phenyl and phenyl substituted with one or more substituents selected from C1 to C4 alkyl, such as tolyl, dimethylphenyl, trimethylphenyl, ethylphenyl, etc. The meaning of C6 to C8 aromatic groups, etc., is similar.

[0030] In some embodiments, the compound of formula I is one or more selected from the following compounds.

[0031]

[0032] Another aspect of the present invention provides a method for preparing an aminophosphonate-modified conductive polymer material, the method comprising: subjecting a conductive polymer monomer and the compound of formula I to a conductive polymer polymerization reaction to obtain an aminophosphonate-modified conductive polymer material.

[0033] The compound of formula I can be synthesized by referring to known or similar methods in the prior art (CN201410765062.1; CN201611012369.X, etc.), or synthesized similarly to the methods disclosed in the examples.

[0034] For example, as shown in Reaction Scheme 1, the compound of Formula I can be obtained by reacting Compound II, Compound III and Compound IV via Kabachnik-Fields reaction, but the present invention is not limited thereto.

[0035]

[0036] In some embodiments, the above reaction can be carried out with or without a catalyst and with or without a solvent. The solvent can be, for example, benzene, acetonitrile, tetrahydrofuran, dichloromethane, chloroform, etc. The catalyst can be Lewis acid such as SnCl2, NiSO4, anhydrous AlCl3, p-toluenesulfonic acid, SnCl4, ZnCl2, MgBr2, BF3·Et2O, etc. The reaction time is 5-24h and the reaction temperature is 25-90°C, but the present invention is not limited thereto.

[0037] In one embodiment, the conductive polymer is polyaniline, and the conductive polymer monomer is aniline. Aniline polymerization reaction can be carried out in the presence of the compound of formula I to obtain aminophosphonate-modified polyaniline material.

[0038] The polymerization reaction of polyaniline can be seen in the following reaction formula 2.

[0039]

[0040] The aminophosphonate modified polyaniline material may have a structure as shown in the following formula V, wherein the compound of formula I is doped with polyaniline through positive and negative charge interactions, but is not limited thereto.

[0041]

[0042] The polymerization reaction of polyaniline can adopt a conventional polymerization method of polyaniline, as long as it does not affect the structure and performance of the compound of formula I. For example, aniline and an acidic aqueous solution can be mixed, an initiator is added, and the reaction is stirred at low temperature for a period of time, but the present invention is not limited thereto. In some embodiments, the acidic aqueous solution includes but is not limited to acidic liquids such as HCl, dodecylsulfonic acid, dodecylbenzenesulfonic acid, and naphthalenesulfonic acid, wherein HCl + The concentration can be 0.5-5.5 mol / L; the initiator includes but is not limited to (NH4)2S2O8, K2Cr2O7, KIO3, FeCl4, H2O2 and other oxidants; the reaction temperature of the polymerization reaction can be 0-5°C, and the reaction time can be 5-24h; but the present invention is not limited thereto.

[0043] In some embodiments, the conductive polymer is polypyrrole, and the conductive polymer monomer is pyrrole. The polymerization reaction of pyrrole can be carried out in the presence of the compound of formula I to obtain an aminophosphonate-modified polypyrrole material.

[0044] The structure of polypyrrole is shown in Formula VI below.

[0045]

[0046] The aminophosphonate-modified polypyrrole material may have a structure as shown in the following formula VII, wherein the compound of formula I is doped with polypyrrole through positive and negative charge interactions, but is not limited thereto.

[0047]

[0048] Experiments have confirmed that the aminophosphonate-modified conductive polymer material of the present invention can selectively adsorb thorium, and in particular, can selectively adsorb thorium in a mixed solution of rare earth and thorium after being prepared into an electrode.

[0049] Therefore, another aspect of the present invention provides the use of the aminophosphonate-modified conductive polymer material of the present invention as a negative electrode material in the preparation of a device for adsorbing thorium, which may be, for example, a negative electrode plate or a capacitive deionization device.

[0050] Another aspect of the present invention provides a negative electrode plate, comprising: a current collector; and a negative electrode material layer on the current collector, wherein the negative electrode material layer comprises the aminophosphonate-modified conductive polymer material according to the present invention as a negative electrode material.

[0051] In addition to comprising the aminophosphonate modified conductive polymer material according to the present invention as the negative electrode material, the composition of the negative electrode material layer may include the components required in the conventional negative electrode material layer. For example, the negative electrode material layer may also include the conductive agent and binder required for preparing the electrode material layer, but is not limited thereto. The conductive agent includes but is not limited to conductive carbon black, conductive graphite, and conductive slurry, etc. The binder includes but is not limited to polyvinylidene fluoride (PVDF), polyacrylic acid (PAA), polyacrylonitrile (PAN), etc.

[0052] There is no particular restriction on the composition of the negative electrode material layer of the negative electrode plate, as long as the prepared negative electrode material layer is uniform and does not crack. For example, in the negative electrode material layer, the mass ratio of the aminophosphonate-modified conductive polymer material, conductive carbon black and binder according to the present invention can generally be maintained at 8:1:1, but is not limited thereto.

[0053] The thickness of the negative electrode material layer may be 0.01-0.1 cm, but is not limited thereto.

[0054] In order to prepare the negative electrode material layer, the components of the negative electrode material layer can be mixed with a dispersant to prepare a slurry. The dispersant includes but is not limited to solvents such as N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAC), and N,N-dimethylformamide (DMF). The proportion of the dispersant can be added according to actual conditions.

[0055] Any suitable coating device may be used to coat the slurry on the current collector, including but not limited to a high-precision adjustable coater, a wire rod coater, an automatic coater, and the like.

[0056] The current collector may be any suitable current collector, for example, a titanium plate, a copper plate, etc., but is not limited thereto.

[0057] Another aspect of the present invention provides a capacitive deionization device, namely a CDI module, which comprises a negative electrode plate according to the present invention.

[0058] Except for including the negative electrode plate according to the present invention, the CDI module may have the structure of a conventional CDI module without any particular limitation, for example, consisting of two corresponding organic glass plates, a positive electrode and a negative electrode, and a silicone gasket.

[0059] Another aspect of the present invention provides a method for adsorbing thorium, the method comprising: in a powered state, passing a thorium-containing liquid into the capacitor deionization device of the present invention, and adsorbing thorium ions into the negative electrode material layer under the action of the electric field.

[0060] When the thorium-containing liquid flows through the capacitive deionization device of the present invention, the positively charged thorium ions move toward the negative electrode plate and are adsorbed into the negative electrode material layer under the action of the electric field, thereby achieving the purpose of removing the thorium ions in the liquid.

[0061] In some embodiments, the method for adsorbing thorium according to the present invention further comprises: desorbing the thorium adsorbed into the negative electrode material layer with a desorbent in an off-circuit state.

[0062] The thorium in the slurry is adsorbed in the negative electrode material layer by the dual effects of pseudocapacitance and double-layer capacitance. Generally, when the electric field is not energized, that is, when the circuit is open, the thorium adsorbed on the negative electrode material will fall off under the action of the desorbent in the absence of the electric field force, and a desorption solution containing thorium is obtained. The desorbent can be nitric acid, sulfuric acid, hydrochloric acid or a mixed solution of any ratio of the above acids, and the acidity can be 0-1 mol / L, measured by the concentration of H ions.

[0063] The capacitive deionization device after desorption can be recycled and can be used again to enrich and separate thorium from thorium-containing feed liquid.

[0064] The thorium-containing liquid may contain thorium and mineral acid and other non-thorium elements. The thorium concentration may be 1 to 1000 mg / L, preferably 100 to 1000 mg / L. In addition, in addition to thorium, the liquid may also contain other elements such as rare earth, alkali metal, alkaline earth metal, transition metal and non-metallic elements. There is no clear restriction on the preparation of the thorium-containing liquid, as long as the thorium-containing liquid is prepared.

[0065] Preferably, the pH value of the thorium-containing feed liquid can be 0-4, preferably 1-3, for example 1, 1.5, 2, 2.5, 3, etc., but not limited thereto. Within the above pH range, it is beneficial to the adsorption performance of the negative electrode material of the present invention, and can maintain a relatively high adsorption capacity and adsorption efficiency. If the pH value exceeds the above range, the adsorption capacity and adsorption efficiency of the negative electrode material of the present invention will be reduced. Therefore, in the process of capacitor deionization, it is preferably within the above pH range to improve the adsorption performance of thorium. The thorium-containing feed liquid system includes but is not limited to nitric acid, sulfuric acid or hydrochloric acid solution.

[0066] Unless otherwise specified, the numerical ranges listed in the present invention include the endpoints and all point values ​​therein that are increased or decreased by the smallest unit of the endpoints and all sub-ranges composed of these point values.

[0067] Beneficial Effects

[0068] The aminophosphonate modified conductive polymer material of the present invention has a simple preparation method, a large adsorption capacity for thorium, good selectivity, and is suitable for efficient enrichment and separation of low-concentration thorium. After the thorium-loaded capacitor deionizer is disconnected and the desorbent is acid-washed, the desorption process can be completed, and the material can be used repeatedly in a cycle. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 The DTG curves of the polyaniline (PANI) synthesized in the present invention and the aminophosphonate-modified polyaniline PANI-PN1 synthesized in Preparation Example 1 are shown.

[0070] Figure 2 The XPS full spectrum and P 2p and N1s peak spectra of the polyaniline (PANI) synthesized in the examples of the present invention and the aminophosphonate-modified polyaniline PANI-PN1 synthesized in Preparation Example 1 are shown.

[0071] Figure 3 The SEM images and EDS energy spectrum distribution diagrams of the polyaniline (PANI) synthesized in the examples of the present invention and the aminophosphonate-modified polyaniline PANI-PN1 synthesized in Preparation Example 1 are shown. DETAILED DESCRIPTION

[0072] In order to further illustrate the solution of the present invention, specific implementation cases of the present invention are provided to help those skilled in the art understand and implement the present invention, but the present invention is not limited to these embodiments.

[0073] Example

[0074] Reagents and instruments

[0075] Stannous chloride (SnCl2) was purchased from Shanghai Titan Technology Co., Ltd., product number 01114991.

[0076] Polyvinylidene fluoride (PVDF) was purchased from Shanghai Titan Technology Co., Ltd., product number 014116501.

[0077] N-Methyl-2-pyrrolidone (NMP) was purchased from Shanghai Titan Technology Co., Ltd., product number 01376439.

[0078] Conductive carbon black (Ketjen Black carbon) was purchased from Shanghai Titan Technology Co., Ltd., product number 04482773.

[0079] Activated carbon was purchased from Shanghai Titan Technology Co., Ltd., product number 013831607.

[0080] Reagent materials such as organic amines, aldehydes, ketones, and dialkyl phosphites were purchased from Aladdin Reagent Company and were all analytically pure reagents. Thorium-containing liquid was prepared by the laboratory. Other reagents (such as acids, organic reagents, etc.) were all commercially available analytically pure reagents.

[0081] The concentration of thorium ions in the feed solution was determined using an inductively coupled plasma optical emission spectrometer (ICP-OES, model: PQ9000, manufacturer: Jena) and an inductively coupled plasma mass spectrometer (ICP-MS, model: Agilent 9800, manufacturer: Agilent).

[0082] Preparation of aminophosphonate compounds

[0083] The aminophosphonate compound PN1 was synthesized via the Kabachnik–Fields reaction.

[0084]

[0085] Bis(2-ethylhexyl)phosphite (18.38mL, 60mmol) was placed in a three-necked flask, and then benzaldehyde (6.12mL, 60mmol) and aniline (5.47mL, 60mmol) were added in sequence, and the mixture was stirred and mixed evenly on a heating magnetic stirrer. Then 0.19g of SnCl2 was added, and the mixture was heated to 100±3°C, and the reaction was stirred for 24h at this temperature, and the reaction degree of the experiment was determined by thin layer chromatography (TLC) spot plate. After determining that the reaction was complete, the product was dissolved in 100mL ethyl acetate solution, and then 50mL NaCl saturated aqueous solution was added in three batches in sequence, and the ethyl acetate solution of the product was washed. The organic layer was collected, and anhydrous sodium sulfate solid was added to the organic layer to remove excess water in the organic phase, and then the ethyl acetate in the organic phase was vacuum-dried to obtain the aminophosphonate compound PN1.

[0086] Except for changing the reaction raw materials as shown in Table 1, an aminophosphonate compound was synthesized in the same manner as above.

[0087] Table 1 Aminophosphonate compounds

[0088]

[0089]

[0090] Comparative Preparation Example 1 Preparation of polyaniline (PANI)

[0091] The dilute hydrochloric acid solution was obtained by diluting 11.73 mL of concentrated hydrochloric acid to 70 mL.

[0092] 5.96 mL of aniline and the above-mentioned dilute hydrochloric acid solution are mixed and stirred evenly in an ice bath at 0-5°C, and then 70 mL of 0.44 mol / L ammonium persulfate aqueous solution is slowly added dropwise. After the addition is completed, the reaction is continued at this temperature for 24 hours. After the reaction is completed, the reaction is allowed to stand, and the reactants are separated into layers to obtain a supernatant and a precipitate. The precipitate is washed three times with ethanol and pure water in sequence to obtain polyaniline.

[0093] Comparative Preparation Example 2 Preparation of polypyrrole (PPY)

[0094] 6 mL (86.67 mmol) of pyrrole and 70 mL of 2 mol / L dilute hydrochloric acid were mixed and stirred for 30 min, and then 100 mL of 0.86 mol / L FeCl3 aqueous solution was slowly added dropwise, and the mixture was stirred in an ice bath at 0-5°C for 6 h. The suspension was filtered, and the obtained solid was repeatedly washed with deionized water until the washing liquid was neutral. The solid product was then vacuum dried at 50°C for 24 h, and a powdered polypyrrole product with finer particles was obtained after grinding.

[0095] Preparation Example 1: Preparation of aminophosphonate-modified polyaniline PANI-PN1

[0096] First, 5.96 mL of aniline and 3.12 mL of aminophosphonate PN1 were mixed, and the molar ratio of aniline to aminophosphonate was 1:0.1. Then, the mixed solution was dripped dropwise into 31.8 mL of 2 mol / L dilute hydrochloric acid at a low temperature of 0-5°C. At the same time, 70 mL of 0.44 mol / L ammonium persulfate was also added dropwise into the dilute hydrochloric acid. After the addition was completed, the reaction was carried out at a temperature of 0-5°C for 5 hours. The product was filtered and washed with water three times to obtain aminophosphonate-modified polyaniline PANI-PN1.

[0097] Thermogravimetric analysis of the polyaniline (PANI) prepared in the comparative preparation example 1 and the aminophosphonate-modified polyaniline PANI-PN1 prepared in the preparation example 1 was performed on a synchronous thermal analyzer (STA449F3) in the temperature range of 40 to 800°C and at a heating rate of 5°C / min. The results are shown in Figure 1, the left figure is the DTG curve of PANI, and the right figure is the DTG curve of PANI-PN1.

[0098] It can be seen from the DTG curve of PANI that there are two weight loss peaks in the figure, corresponding to the two stages of the weight loss process of polyaniline. The weight loss peak at 101.34°C corresponds to the volatilization of residual solvents (water, ethanol) in the material; the weight loss at 514.96°C corresponds to the oxidative decomposition of polyaniline (the oxidative decomposition of organic matter is generally between 350 and 600°C).

[0099] Correspondingly, the DTG curve of PANI-PN1 has a weight loss peak at 105.25℃ and 508.80℃, which are almost consistent with the weight loss peak of PANI. The weight loss peak at 256℃ corresponds to the decomposition process of the aminophosphonate functional groups doped in PANI, and also represents the dedoping process of aminophosphonate in PANI, which indicates that aminophosphonate is successfully doped on polyaniline with a percentage of 17.42%.

[0100] XPS spectra of the polyaniline and aminophosphonate-modified polyaniline PANI-PN1 prepared above were analyzed on an X-ray photoelectron spectrometer (AXIS SUPRA+). The results are shown in Figure 2 , where (a) is the XPS full spectrum of PANI-PN1 and PANI, (b) is the N1s peak spectrum of PANI-PN1 and PANI, and (c) is the P 2p peak spectrum of PANI-PN1 and PANI.

[0101] Comparison of the XPS spectra of PANI-PN1 and PANI ( Figure 2 From a), it can be seen that the N1s peak of PANI is at 398.48 eV, while the N1s and P 2p peaks of PANI-PN1 appear at 400 eV and 134 eV, respectively.

[0102] Comparison of high-resolution N1s peak spectra of PANI-PN1 and PANI ( Figure 2 As can be seen from b), the N1s of PANI can be divided into three peaks, located at 398.48 eV (from -NH-, content 80.71%), 396.98 eV (from -N=, content 5.39%) and 399.98 eV (from -NH + =, content 13.90%); while the N1s of the PANI-PN1 composite material can also be divided into three peaks, located at 399.88eV (from -NH-, content 66.33%), 399.48eV (from -N=, content 24.50%) and 401.68eV (from -NH +=, content 20.44%), it can be seen that after the polyaniline was modified with aminophosphonate, the area and position of the N1s peak of PANI-PN1 changed compared with those before modification (PANI), indicating the successful synthesis of aminophosphonate-modified polyaniline.

[0103] Comparison of the high-resolution P 2p peak spectra of PANI-PN1 and PANI ( Figure 2 c) It can be seen that PANI has no P2p peak, while PANI-PN1 has a P 2p peak. The P 2p peak of PANI-PN1 can be divided into three peaks, located at 133.98 eV, 133.28 eV and 134.98 eV, corresponding to PO, P=O and PC, respectively.

[0104] The above characterization results indicate that aminophosphonate functional groups were successfully doped onto polyaniline.

[0105] The PANI and PANI-PN1 prepared above were examined by SEM on a high-resolution field emission transmission electron microscope (JEM-F200). Figure 3 , where a) is the SEM photo of polyaniline (PANI), b is the SEM photo of PANI-PN1, and c to f are the EDS surface scanning distribution diagrams of C, P, O, and N elements, respectively, indicating that the aminophosphonate was successfully doped on the surface of PANI.

[0106] Comparison of SEM images of PANI and PANI-PN1 ( Figure 3 ) It can be seen that more short rod-like structures appeared on the surface of PANI-PN1. This structural feature is beneficial to increasing the contact area between PANI-PN1 and metal ions, which is more conducive to the adsorption of metal ions.

[0107] Preparation Example 2-4: Preparation of aminophosphonate-modified polyaniline PANI-PN2 to PANI-PN4

[0108] Except for changing the reaction raw materials as shown in Table 2, aminophosphonate-modified polyanilines PANI-PN2 to PANI-PN4 were synthesized in the same manner as in Preparation Example 1.

[0109] Preparation Example 5: Preparation of aminophosphonate-modified polypyrrole PPY-PN5

[0110] First, 6 mL of pyrrole and 3.8 mL of aminophosphonate PN5 were mixed, and the molar ratio of pyrrole to aminophosphonate PN5 was 1:0.1. Then, the mixed solution was dripped dropwise into 31.8 mL of 2 mol / L dilute hydrochloric acid at a low temperature of 0-5°C. At the same time, 100 mL of 0.86 mol / L FeCl3 was also added dropwise into the dilute hydrochloric acid. After the addition was completed, the reaction was carried out at a temperature of 0-5°C for 5 hours. The product was filtered, washed with water until neutral, and dried to obtain aminophosphonate-modified polypyrrole PPY-PN5.

[0111] Preparation Example 6-8: Preparation of aminophosphonate-modified polypyrroles PPY-PN6 to PPY-PN8

[0112] Aminophosphonate-modified conductive polypyrroles PPY-PN6 to PPY-PN8 were synthesized in the same manner as in Preparation Example 5, except that the reaction raw materials were changed as shown in Table 2.

[0113] Table 2

[0114]

[0115]

[0116] Example

[0117] Preparation of negative electrode plate:

[0118] Take 0.24g of binder polyvinylidene fluoride (PVDF) and dissolve it in 12mL dispersant N-methyl-2-pyrrolidone (NMP). Then take 0.32g of negative electrode material, 0.04g of conductive carbon black, and 2mL of mixed solution of PVDF and NMP, that is, mix them evenly in the ratio of negative electrode material: conductive carbon black: PVDF = 8:1:1, and then use an adjustable wet film preparation device (KTQ-Ⅱ) to evenly coat it on a titanium plate (effective area 5×5cm), with a coating thickness of 1mm, and then place the electrode plate in a vacuum drying oven to dry for 8 hours.

[0119] Preparation of positive electrode plate:

[0120] Except for changing the electrode material from negative electrode material to positive electrode material activated carbon, the other preparation methods are the same as those of the negative electrode plate.

[0121] Electrosorption experiment:

[0122] An asymmetric electrode system was assembled using two corresponding organic glass plates, the negative and positive electrode plates and a silicone gasket to serve as a capacitive deionization (CDI) device.

[0123] During the electrosorption process, the feed liquid was pumped into the CDI device at a flow rate of 10 mL / min through a peristaltic pump and returned to the feed container. At the same time, a constant voltage of 2.4 V was applied to the CDI device, and the concentration changes of ions in the feed liquid were observed by the conductivity meter until the reading of the conductivity meter did not change and the electrosorption reached equilibrium.

[0124] Inductively coupled plasma atomic emission spectrometry (ICP-OES) was used to determine the metal ions (Th 4+ ,La 3+ , Gd 3+ He Lu 3+ ) concentration.

[0125] Adsorption capacity (Q, mg g) of the negative electrode material layer (including negative electrode material, conductive carbon black and PVDF) -1 ), removal rate (%), desorption capacity (Q′, mg g -1 ), desorption rate (%), distribution coefficient K d and the selectivity coefficient β Th / RE The calculation formula is as follows:

[0126]

[0127]

[0128] In the formula,

[0129] Q is the adsorption capacity of the negative electrode material layer (mg / g);

[0130] C0 and C t represent the metal ion concentrations in the feed solution at the initial time t0 and time t (mg / L), respectively;

[0131] V represents the volume of the feed solution (L);

[0132] m represents the mass of the negative electrode material layer (g);

[0133] Q′ represents the desorption capacity (mg / g);

[0134] C t ′ represents the metal ion concentration in the desorption solution after desorption time t (mg / L);

[0135] C0′ represents the metal ion concentration in the desorption solution when the desorption time is 0 (mg / L);

[0136] V′ represents the volume of the desorption liquid (L);

[0137] K d is the partition coefficient of the metal ion;

[0138] and represent the distribution coefficients of thorium ions and rare earth ions, respectively.

[0139] Desorption experiment:

[0140] In the off-circuit state, desorption was performed using 0.5 M H2SO4 solution by off-circuit (0 V potential) for 12 hours, and the concentrations of thorium ions and rare earth ions in the desorbed solution were measured.

[0141] Examples 1-8 and Comparative Examples 1-2

[0142] The aminophosphonate-modified conductive polymers prepared in Preparation Examples 1-8, the polyaniline synthesized in Comparative Preparation Example 1, and the polypyrrole synthesized in Comparative Preparation Example 2 were used as negative electrode materials to prepare negative electrode plates, and assembled into a capacitive deionization device as above.

[0143] First, an electrosorption experiment was conducted to calculate the adsorption capacity, and then a desorption experiment was conducted using 5 mL of a 0.1 ml / L dilute sulfuric acid solution to determine the thorium ion concentration in the desorbed solution and calculate the enrichment multiple.

[0144] Experimental conditions:

[0145] Th(SO4)2 solution: The initial thorium ion concentration C0 is shown in Table 3 below, the volume is 1L, the pH is 3,

[0146] Adsorption time t = 1200min,

[0147] The applied voltage is U=2.4V.

[0148] When using different aminophosphonates to modify the conductive polymer or polyaniline, the adsorption capacity and enrichment multiples of the negative electrode material layer are shown in Table 3.

[0149] Table 3

[0150]

[0151]

[0152] From the results in Table 3, it can be concluded that the aminophosphonate-modified conductive polymer of the present invention has a high adsorption capacity for thorium and a high enrichment multiple. In particular, by comparing the results of the material of the present invention with those of Comparative Examples 1-2, it can be concluded that the enrichment performance of the aminophosphonate-modified conductive polymer of the present invention is significantly higher than that of the unmodified conductive polymer material.

[0153] Examples 9-16 and Comparative Examples 3-4

[0154] Aminophosphonate-modified conductive polymers prepared in Preparation Examples 1-8, polyaniline synthesized in Comparative Preparation Example 1, and polypyrrole synthesized in Comparative Preparation Example 2 were used as negative electrode materials to prepare negative electrode plates and assembled into a capacitive deionization device. A mixed solution of rare earth and thorium was used to carry out an electrosorption experiment and calculate its separation coefficient.

[0155] Experimental conditions:

[0156] Mixed solution of rare earth and thorium: the initial concentration C0 of La, Gd, Lu, and Th is all 100 mg / L, the volume is V = 100 mL, and the pH is 3;

[0157] Electrosorption time: 120min.

[0158] The separation coefficients of thorium and rare earth ions under different negative electrode material conditions are shown in Table 4.

[0159] Table 4

[0160] Example Anode Materials <![CDATA[β Th / La ]]> <![CDATA[β Th / Gd ]]> <![CDATA[β Th / Lu ]]> Example 9 PANI-PN1 136.32 17.10 73.45 Example 10 PANI-PN2 84.97 5.59 36.62 Embodiment 11 PANI-PN3 11.84 42.30 4.58 Example 12 PANI-PN4 21.01 136.98 5.11 Embodiment 13 PPY-PN5 115.67 6.24 72.83 Embodiment 14 PPY-PN6 60.23 40.25 21.33 Embodiment 15 PPY-PN7 11.85 42.30 5.58 Example 16 PPY-PN8 23.38 37.58 6.20 Comparative Example 3 PANI 2.87 0.97 1.35 Comparative Example 4 PPY 3.94 11.70 8.63

[0161] The results in Table 4 show that compared with polyaniline (PANI), the aminophosphonate modified conductive polymer synthesized in the present invention has a higher selectivity for thorium within a certain electrical adsorption time, and can be used to efficiently separate thorium from a thorium-containing rare earth solution.

[0162] Examples 17-24 and Comparative Examples 5-6 Cyclic Regeneration Experiments:

[0163] First, prepare 100 mL of Th(SO4)2 solution with a concentration of 100 mg / L and pH = 3.

[0164] The aminophosphonate-modified conductive polymers prepared in Preparation Examples 1-8, the polyaniline synthesized in Comparative Preparation Example 1, and the polypyrrole synthesized in Comparative Preparation Example 1 were used as negative electrode materials to prepare negative electrode plates and assembled into a capacitive deionization (CDI) device as above.

[0165] Then, at a voltage of 2.4V, cyclic electrosorption was performed in the CDI device for 24 hours. The electrosorption capacity of the negative electrode material can be obtained based on the initial concentration of the Th(SO4)2 solution and the concentration after 24 hours of electrosorption. Then, a desorption experiment was performed for 12 hours using a 0.5M H2SO4 solution with a circuit break (0V potential). Then, an electrosorption experiment was performed with the same feed solution as in the first electrosorption, and the electrosorption capacity at this time was calculated. And so on, the cycle was regenerated 5 times.

[0166] The specific experimental data are shown in Table 5 below:

[0167] Table 5

[0168]

[0169] It can be seen from Table 5 that, compared with PANI and PPY, the modified conductive polymer can still maintain good electrical adsorption performance after 5 cycles of regeneration.

Claims

1. An aminophosphonate-modified conductive polymer material comprising: (1) Conductive polymer matrix; (2) Compounds of formula I doped with conductive polymer matrix: in, R1 is selected from C1~C 12 Alkylene; R2 and R3 are each independently selected from hydrogen, C1-C8 alkyl, C3-C 10 Cycloalkyl, and C6~C 10 Aryl; R4 and R5 are each independently selected from C1 to C 16 Alkyl and C6~C 10 Aryl.

2. The aminophosphonate-modified conductive polymer material according to claim 1, wherein The conductive polymer matrix is ​​selected from polyaniline and polypyrrole.

3. The aminophosphonate-modified conductive polymer material according to claim 1, wherein R1 is selected from C1~C 10 Alkylene, such as C1-C8 alkylene or C1-C6 alkylene; and / or R2 and R3 are each independently selected from hydrogen, C1-C6 alkyl, C5-C8 cycloalkyl and C6-C8 aryl; and / or R4 and R5 are each independently selected from C2 to C 14 Alkyl and C6-C8 aryl, more preferably C3-C 12 Alkyl and C6~C8 aryl.

4. The aminophosphonate-modified conductive polymer material according to claim 1, wherein The compound of formula I is one or more selected from the following compounds:

5. Use of the aminophosphonate-modified conductive polymer material according to any one of claims 1 to 4 as a negative electrode material in the preparation of a device for adsorbing thorium, such as a negative electrode plate or a capacitive deionization device.

6. A negative electrode plate, comprising: current collector; and a negative electrode material layer on the current collector, wherein the negative electrode material layer comprises the aminophosphonate-modified conductive polymer material according to any one of claims 1 to 4 as a negative electrode material; In particular, the negative electrode material layer comprises: the aminophosphonate-modified conductive polymer material according to any one of claims 1 to 4 as a negative electrode material; a conductive agent; and a binder.

7. A capacitive deionization device comprising the negative electrode plate according to claim 5.

8. A method for adsorbing thorium, the method comprising, in a powered state, passing a thorium-containing liquid into the capacitive deionization device according to claim 7, and adsorbing thorium ions into a negative electrode material layer under the action of an electric field.

9. The method according to claim 8, wherein: The thorium concentration in the thorium-containing liquid is 1-1000 mg / L, preferably 100-1000 mg / L; the pH value is 0-4, preferably 1-3.

10. The method according to claim 8, wherein: The method further comprises: in an off-circuit state, desorbing thorium adsorbed into the negative electrode material layer using a desorbent; Particularly, the desorbent is nitric acid, sulfuric acid, hydrochloric acid or a mixed solution of the above acids in any ratio, and the acidity is 0-1 mol / L, measured in terms of H ion concentration.

Citation Information

Patent Citations

  • Purpose and method of amino-contained neutral phosphine extraction agent for extraction and separation of thorium

    CN105734289A

  • Membrane capacitive deionization desalination module, preparation method thereof and membrane capacitive deionization desalination device

    CN115536114A

  • Proton conducting polymer membrane comprising phoshphonic acid groups containing polyazoles and the use thereof in fuel cells

    CN1726071A

  • Phosphorous-containing polyaniline and manufacturing method thereof

    JP2017137457A

  • Electric capacitive deionization apparatus and method for treating fluid using same

    KR1020150011171A