Supported PtNi double-site adiponitrile hydrogenation catalyst as well as preparation method and application thereof

The introduction of Pt and Ni on the tungsten oxide nanorod support by the supported PtNi two-site catalysts solves the problem of low efficiency and high cost of catalyzing adipiconet hydrogenation under mild conditions, and achieves high selectivity and The efficient formation of primary amines has important industrial application value.

CN118874491AActive Publication Date: 2024-11-01RES & DEV INST OF NORTHWESTERN POLYTECHNICAL UNIV IN SHENZHEN

Patent Information

Application Number
CN202410923018.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-01
Estimated Expiration
2044-07-10

AI Technical Summary

Technical Problem

The existing adipiconet hydrogenation catalysts have problems such as crushing, spontaneous combustion, requiring a large amount of ammonia and alkali solution to suppress side reactions, complex preparation process and high cost, and it is difficult to efficiently catalyze the hydrogenation of adipiconet to form primary amines under mild conditions.

Method used

Using a supported PtNi bisite catalyst, Pt and Ni bimetallic active sites were introduced on the tungsten oxide nanorod support, and prepared by traditional impregnation method to achieve spatial separation of single atomic form of Pt and particle form of Ni, breaking the linear mark The degree limit is to reduce the load of precious metals and simplify the preparation process.

Benefits of technology

The catalytic activity of adipicnitrile hydrogenation and the selectivity of target products are improved, and the efficient catalytic hydrogenation of adipicnier is achieved under mild conditions to form primary amines, reducing the use of ammonia and alkali solutions, with low cost and industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874491A_ABST
    Figure CN118874491A_ABST
Patent Text Reader

Abstract

The invention discloses a supported PtNi double-site adiponitrile hydrogenation catalyst as well as a preparation method and application thereof, and belongs to the technical field of thermocatalysis. The preparation method comprises the following steps: (1) dispersing ammonium tungsten oxide pentahydrate in water, adding an acidic solution, condensing, refluxing, heating, reacting, centrifugally filtering, drying and precipitating to prepare a tungsten oxide nanorod carrier; (2) dispersing the tungsten oxide nanorod carrier in a solvent, adding a platinum salt solution, stirring, evaporating the solvent, and calcining a solid to prepare a catalyst precursor; and (3) dispersing the catalyst precursor in a solvent, adding a nickel salt solution, stirring, evaporating the solvent, and calcining the solid to obtain the catalyst. The bimetallic active site catalyst is constructed by introducing Pt and Ni on the reducible WO3 carrier, can catalyze the reaction of preparing primary amine through adiponitrile hydrogenation under mild conditions, has the characteristics of low noble metal loading capacity, high activity and high selectivity, and has important industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermal catalysis, and in particular to a supported PtNi dual-site adiponitrile hydrogenation catalyst and a preparation method and application thereof. Background Art

[0002] The hydrogenation of nitrile compounds to produce the corresponding primary amines is one of the topics actively studied in the field of bulk chemicals and fine chemicals. Primary amines are important chemical raw materials and fine chemical intermediates, and can be widely used in the synthesis of plastics, detergents, textile auxiliaries, flotation agents, antistatic agents and preservatives. However, in the process of hydrogenation of nitrile to produce primary amines, hydrogenation and condensation of unsaturated -C≡N bonds can occur simultaneously. Therefore, the formation of primary amines is often accompanied by by-products such as secondary amines and tertiary amines. Therefore, the key step to improve the selectivity of primary amines is to inhibit the formation of the above-mentioned by-products. Therefore, it is of great significance to construct a suitable catalytic system to achieve high selectivity of nitrile to prepare primary amines under mild conditions.

[0003] The hydrogenation of adiponitrile (ADN) to prepare primary amines is the most effective and reasonable reaction pathway. Since ADN is highly unsaturated and includes two -C≡N functional groups, the hydrogenation reaction includes semi-hydrogenation (6-aminocapronitrile, ACN) and full hydrogenation (1,6-hexanediamine, HDA) products. In addition, imine, as a highly active intermediate, condenses within the molecule to form a by-product cyclohexylamine (ACH). Among them, ACN and HMDA are important chemical intermediates. The former is used to prepare ε-caprolactam (CPL). CPL is a very important organic chemical intermediate and is also the main raw material for synthesizing nylon-6 fibers, nylon-6 engineering plastics and films. The latter is used to prepare nylon-66. For example Figure 1 As shown, ADN hydrogenation is a complex process with different reaction pathways. First, ADN is semi-hydrogenated to form highly active imines, which can be further hydrogenated to primary amines of ACN and HDA. CAN continues to hydrogenate the intermediate imines, which can also react with primary amines, by nucleophilic addition of primary amines to the α-carbon of aldehyde amines to form 1-(alkylamine)-1-amine (intermolecular condensation) and azepan-2-amine (intermolecular condensation), and then further deamination to form N-substituted imines (tertiary amines). Then hydrogenation is performed to form 1-azepane (ACH), the main byproduct of secondary amines.

[0004] The ADN hydrogenation catalysts reported so far include Raney-type catalysts, Ziegler-type catalysts, amorphous alloy catalysts, non-supported and supported nickel-based catalysts, and precious metal catalysts such as Ru or Rh. ADN hydrogenation on Raney-type catalysts has problems such as breakage, spontaneous combustion, and the need for a large amount of ammonia and alkaline solutions to inhibit side reactions. Ru complex homogeneous catalysts and Rh supported catalysts have high conversion rates and selectivities of ADN to ACN and HDA during liquid-phase hydrogenation, but these catalysts have the disadvantages of complex preparation processes, high costs, and the need for a large amount of ammonia and alkaline solutions to inhibit the formation of by-products. A catalyst with low precious metal loading, high activity, high selectivity, stable structure, easy recycling, and the ability to catalyze the hydrogenation of adiponitrile to prepare primary amines under relatively mild conditions is in urgent need of development. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a supported PtNi dual-site adiponitrile hydrogenation catalyst and its preparation method and application, so as to solve the problems of existing adiponitrile hydrogenation catalysts such as breakage, spontaneous combustion, the need for a large amount of ammonia and alkaline solution to inhibit side reactions, complex preparation process, high cost, etc.

[0006] The technical solution of the present invention to solve the above technical problems is as follows:

[0007] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0008] (1) Preparation of tungsten oxide nanorod carrier: disperse ammonium tungsten oxide pentahydrate in water, add acidic solution, condense and reflux, heat to react, centrifuge and filter, and dry the precipitate to obtain;

[0009] (2) Preparation of catalyst precursor: dispersing the tungsten oxide nanorod carrier obtained in step (1) in a solvent, adding a platinum salt solution, stirring, evaporating the solvent, and calcining the solid to obtain;

[0010] (3) Preparation of supported PtNi dual-site adiponitrile hydrogenation catalyst: The catalyst precursor obtained in step (2) is dispersed in a solvent, a nickel salt solution is added, stirred, the solvent is evaporated, and the solid is calcined to obtain the catalyst.

[0011] The beneficial effects of the present invention are as follows: the present invention adopts a traditional impregnation method to introduce Pt and Ni bimetallic active sites on a tungsten oxide nanorod carrier, wherein the Pt loading is very low and exists in the form of a single atom, and Ni exists in the form of particles, thereby realizing the spatial separation of the bimetallic sites and breaking the contradiction of the linear scaling limitation of the traditional supported catalyst itself, thereby improving the catalytic activity of adiponitrile hydrogenation and the selectivity of the target product, the preparation method is simple, the noble metal loading is low, the cost is low, and a large amount of ammonia and alkaline solution are not required to inhibit side reactions, and the present invention has a high industrial value.

[0012] Furthermore, in step (1), the molar volume ratio of ammonium tungsten oxide pentahydrate, water and acidic solution is 1-5mmol:30-50mL:5-15mL; the acidic solution is a nitric acid solution with a concentration of 2-3mol / L.

[0013] Preferably, in step (1), the molar volume ratio of ammonium tungsten oxide pentahydrate, water and acidic solution is 2.5mmol:40mL:10mL; the acidic solution is a nitric acid solution with a concentration of 2.5mol / L.

[0014] Furthermore, in step (1), the condensation reflux temperature is 80-90°C, and the time is 30-90 min; the heating reaction temperature is 120-200°C, and the time is 10-15 h; the drying temperature is 40-80°C, and the time is 5-12 h.

[0015] Preferably, in step (1), the temperature of condensation reflux is 85°C and the time is 60 min; the temperature of heating reaction is 160°C and the time is 12 h; the temperature of drying is 60°C and the time is 8 h.

[0016] The beneficial effect of adopting the above further technical scheme is: the present invention uses ammonium tungsten oxide pentahydrate as a raw material to prepare a tungsten oxide nanorod carrier, and the surface of the carrier is rich in oxygen defects, which not only provides sufficient active sites for the subsequent Pt and Ni bimetallic loading, but also can be used as a reducible carrier to provide the possibility for the occurrence of hydrogen overflow.

[0017] Furthermore, in step (2), the mass volume ratio of the oxide nanorod carrier, the solvent and the platinum salt solution is 200-400 mg: 10-50 mL: 4-8 μL; the solvent is ethanol; and the platinum salt solution is an aqueous solution of platinum nitrate with a concentration of 3-7 mg / mL.

[0018] Preferably, in step (2), the mass volume ratio of the oxide nanorod carrier, the solvent and the platinum salt solution is 300 mg:30 mL:6 μL; the solvent is ethanol; and the platinum salt solution is an aqueous solution of platinum nitrate with a concentration of 5 mg / mL.

[0019] Furthermore, in step (2), the stirring time is 30-90 min, and the rotation speed is 300-500 rpm; the calcination conditions are: in a mixture of hydrogen and rare gas, the temperature is increased to 300-700° C. at a rate of 3-7° C. / min, and kept warm for 1-3 h, wherein the volume fraction of hydrogen in the mixed gas is 1-10%.

[0020] The beneficial effect of adopting the above further technical solution is: the present invention loads Pt on the tungsten oxide nanorod carrier by the traditional impregnation method, so that Pt exists in the form of a single atom, and acts as an adsorption and activation site for hydrogen to catalyze the hydrogenation reaction of adiponitrile.

[0021] Furthermore, in step (3), the mass volume ratio of the catalyst precursor, the solvent and the nickel salt solution is 200-400 mg: 10-50 mL: 1-10 mL; the solvent is ethanol; and the nickel salt solution is a nickel nitrate aqueous solution with a concentration of 3-7 mg / mL.

[0022] Furthermore, in step (3), the stirring time is 30-90 min, and the rotation speed is 300-500 rpm; the calcination conditions are: in a mixture of hydrogen and rare gas, the temperature is increased to 300-700° C. at a rate of 3-7° C. / min, and kept warm for 1-3 h, wherein the volume fraction of hydrogen in the mixed gas is 1-10%.

[0023] The beneficial effect of adopting the above further technical scheme is as follows: the present invention loads Ni on the tungsten oxide nanorod carrier by the traditional impregnation method, so that Ni exists in the form of particles, realizes the spatial separation of the bimetallic sites, breaks the contradiction of the linear scaling limitation of the traditional supported catalyst itself, and acts as an activation site of the -C≡N bond to catalyze the hydrogenation reaction of adiponitrile.

[0024] A supported PtNi dual-site adiponitrile hydrogenation catalyst is prepared by adopting the preparation method.

[0025] The supported PtNi dual-site adiponitrile hydrogenation catalyst is used in catalyzing the adiponitrile hydrogenation reaction to prepare primary amines.

[0026] A method for preparing primary amines by catalyzing the hydrogenation reaction of adiponitrile, comprising mixing the above-mentioned supported PtNi dual-site adiponitrile hydrogenation catalyst, a reaction solvent, an alkaline solution and adiponitrile, and reacting at 80-120° C. under a hydrogen pressure of 1-3 MPa to prepare primary amines;

[0027] The masses of the catalyst and adiponitrile are 10-30 mg and 50-150 mg respectively.

[0028] Furthermore, the mass / volume ratio of the catalyst, reaction solvent and alkaline solution is 10-30 mg: 1-3 mL: 10-100 μL; the reaction solvent is ethanol; the alkaline solution is any one of sodium hydroxide solution, potassium hydroxide solution, sodium carbonate solution and sodium bicarbonate solution, and the concentration is 3-7 mol / L.

[0029] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing primary amines by catalyzing the hydrogenation reaction of adiponitrile with a supported PtNi dual-site adiponitrile hydrogenation catalyst. The preparation method uses hydrogen as a hydrogen ion source, which is in line with the green, pollution-free and environmentally friendly development concept. The catalytic reaction conditions are mild, the yield of primary amines is high, the selectivity is high, the utilization rate of the catalyst is high, the stability is good, and the method has important industrial application value.

[0030] The present invention has the following beneficial effects:

[0031] (1) The present invention provides a method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst, which can be obtained by a traditional impregnation method, is simple and efficient, and ensures that the noble metal ions are completely loaded on the tungsten oxide carrier, wherein the loading amount of Pt is very low and exists in the form of a single atom, and Ni exists in the form of particles, thereby achieving spatial separation of the dual metal sites, breaking the contradiction of the linear scaling limitation of the traditional supported catalyst itself, thereby improving the catalytic activity of adiponitrile hydrogenation and the selectivity of the target product.

[0032] (2) In the supported PtNi dual-site adiponitrile hydrogenation catalyst prepared by the present invention, Pt and Ni serve as the adsorption site and activation site of hydrogen and the activation site of -C≡N bond, respectively, and the WO3 carrier rich in oxygen defects on the surface serves as a reducible carrier, which provides the possibility for the occurrence of hydrogen overflow. H2 molecules are activated at the Pt site to generate activated hydrogen atoms (*H), adiponitrile molecules are adsorbed on the surface of Ni particles through -C≡N bonds, and *H overflows from the WO3 surface to the surface of Ni particles, thereby achieving hydrogenation of adiponitrile to generate primary amines (hexamethylenediamine and 6-aminocapronitrile).

[0033] (3) The present invention provides a method for preparing primary amines by hydrogenating adiponitrile using a supported PtNi dual-site adiponitrile hydrogenation catalyst. The method uses hydrogen as a hydrogen ion source, conforms to the green, pollution-free, and environmentally friendly development concept, and is widely used in industry. The catalytic reaction conditions are mild, the yield of primary amines is high, the selectivity is high, the utilization rate of the catalyst is high, the stability is good, and it has important industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is the reaction pathway diagram of adiponitrile hydrogenation;

[0035] Figure 2 The experimental results of the catalytic hydrogenation reaction of adiponitrile to produce primary amines in the test example, wherein a is a schematic diagram of the dual-site hydrogenation reaction, b is the conversion rate of different catalysts, c is the selectivity of different catalysts to the product, d is the relationship between the Ni loading and the reaction rate, e is the H2-TPR diagram of different catalysts, and f is the TOF value of different catalysts;

[0036] Figure 3 The experimental results of the reaction mechanism study of catalytic hydrogenation of adiponitrile to produce primary amines in the test example, where a is the W of the catalyst obtained at different calcination temperatures. 5+ X-ray photoelectron spectroscopy, b is the H2-TPR diagram of the catalysts prepared at different calcination temperatures, c is the conversion rate and selectivity of the catalysts prepared at different calcination temperatures in catalyzing the hydrogenation reaction of adiponitrile to produce primary amines; d is the relationship between the hydrogen overflow rate and the reaction rate of the catalysts prepared at different calcination temperatures;

[0037] Figure 4 The selectivity of primary amines in the test case and the Ni content on the surface of Pt-Ni / WO3 catalyst at different reduction temperatures 0 The relationship experimental results, where a is the Ni element X-ray photoelectron spectrum of the catalysts prepared at different calcination temperatures, b is the d band center test result, and c is the Ni on the catalyst surface. 0 The relationship between quantity and selectivity, d is the relationship between binding energy and selectivity, and e is the relationship between binding energy and reaction rate. DETAILED DESCRIPTION

[0038] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0039] Embodiment 1:

[0040] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0041] (1) Preparation of tungsten oxide nanorod (NR-WO3) carrier

[0042] First, 2.5mmol (3.06g) (NH4) 10 W 12 O4·5H2O was placed in a round-bottom flask, 40mL of deionized water was added and stirred; then 10mL of 2.5mol / L dilute nitric acid solution was slowly added dropwise to the above suspension, condensed and refluxed at 85°C for 1h; then the precipitate after the reaction was poured into a stainless steel hydrothermal autoclave with a polytetrafluoroethylene liner and heated at 160°C for 12h, cooled to room temperature, centrifuged and filtered to obtain a precipitate, and the precipitate was washed 3 times with deionized water; finally, it was dried at 60°C overnight to obtain a light yellow tungsten oxide powder (oxide nanorod carrier).

[0043] (2) Preparation of Pt1 / NR-WO3 catalyst precursor

[0044] At room temperature, 300 mg of the NR-WO3 powder obtained in step (1) was uniformly dispersed in 30 mL of ethanol by ultrasound and stirring; 6 μL of a 5 mg / mL platinum nitrate aqueous solution was then added dropwise to the dispersion, stirred at 400 rpm for 1 h, and then heated to completely evaporate the ethanol to obtain a solid powder. Finally, the solid powder was heated to 350°C at a rate of 5°C / min in a mixture of hydrogen and argon (the volume fraction of hydrogen in the mixture is 5%), and calcined for 2 h to obtain a Pt1 / NR-WO3 catalyst precursor, where the mass fraction of the Pt metal loading was 0.01%.

[0045] (3) Preparation of Pt1-Ni / NR-WO3 catalyst:

[0046] At room temperature, 300 mg of the Pt1 / NR-WO3 catalyst precursor obtained in step (2) is uniformly dispersed in 30 mL of ethanol by ultrasound and stirring; 3 mL of a 5 mg / mL nickel nitrate aqueous solution is then added dropwise to the dispersion, stirred for 1 hour, and then heated to completely evaporate the ethanol to obtain a solid powder; finally, the solid powder is heated to 350° C. at a rate of 5° C. / min in a mixture of hydrogen and argon (the volume fraction of hydrogen in the mixture is 5%), and calcined for 2 hours to obtain a Pt1-Ni / NR-WO3 catalyst in which the loading mass fraction of metal Ni is 5%, named Pt-Ni / WO3-350.

[0047] Embodiment 2:

[0048] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0049] The preparation method is the same as that of Example 1, except that the amount of nickel nitrate aqueous solution added in step (3) is changed to 1.2 mL, and the loading mass fraction of the obtained catalyst metal Ni is 2%.

[0050] Embodiment 3:

[0051] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0052] The preparation method is the same as that of Example 1, except that the amount of nickel nitrate aqueous solution added in step (3) is changed to 1.8 mL, and the loading mass fraction of the obtained catalyst metal Ni is 3%.

[0053] Embodiment 4:

[0054] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0055] The preparation method is the same as that of Example 1, except that the amount of nickel nitrate aqueous solution added in step (3) is changed to 2.4 mL, and the loading mass fraction of the obtained catalyst metal Ni is 4%.

[0056] Embodiment 5:

[0057] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0058] The preparation method is the same as that of Example 1, except that the calcination temperature of step (2) and step (3) is changed to 450°C. The prepared catalyst is named Pt-Ni / WO3-450.

[0059] Embodiment 6:

[0060] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0061] The preparation method is the same as that of Example 1, except that the calcination temperature of step (2) and step (3) is changed to 550°C. The prepared catalyst is named Pt-Ni / WO3-550.

[0062] Embodiment 7:

[0063] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0064] The preparation method is the same as that of Example 1, except that the calcination temperatures of step (2) and step (3) are both modified to 600°C. The prepared catalyst is named Pt-Ni / WO3-600.

[0065] Embodiment 8:

[0066] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0067] The preparation method is the same as that of Example 1, except that the calcination temperature of step (2) and step (3) is changed to 650°C. The prepared catalyst is named Pt-Ni / WO3-650.

[0068] Comparative Example 1:

[0069] A method for preparing a supported Pt single-site adiponitrile hydrogenation catalyst comprises the following steps:

[0070] (1) Preparation of tungsten oxide nanorod (NR-WO3) carrier

[0071] First, 2.5mmol (3.06g) (NH4) 10 W 12O4·5H2O was placed in a round-bottom flask, 40mL of deionized water was added and stirred; then 10mL of 2.5mol / L dilute nitric acid solution was slowly added dropwise to the above suspension, condensed and refluxed at 85°C for 1h; then the precipitate after the reaction was poured into a stainless steel hydrothermal autoclave with a polytetrafluoroethylene liner and heated at 160°C for 12h, cooled to room temperature, centrifuged and filtered to obtain a precipitate, and the precipitate was washed 3 times with deionized water; finally, it was dried at 60°C overnight to obtain a light yellow tungsten oxide powder (oxide nanorod carrier).

[0072] (2) Preparation of supported Pt single-site adiponitrile hydrogenation catalyst Pt / WO3

[0073] At room temperature, 300 mg of the NR-WO3 powder obtained in step (1) was uniformly dispersed in 30 mL of ethanol by ultrasound and stirring; 6 μL of a 5 mg / mL platinum nitrate aqueous solution was then added dropwise to the dispersion, stirred at 400 rpm for 1 h, and then heated to completely evaporate the ethanol to obtain a solid powder. Finally, the solid powder was heated to 350° C. at a rate of 5° C. / min in a mixture of hydrogen and argon (the volume fraction of hydrogen in the mixture is 5%), and calcined for 2 h to obtain a supported Pt single-site adiponitrile hydrogenation catalyst Pt / WO3, named Pt / WO3, where the mass fraction of the Pt metal loading was 0.01%.

[0074] Comparative Example 2:

[0075] A method for preparing a supported Ni single-site adiponitrile hydrogenation catalyst comprises the following steps:

[0076] (1) Preparation of tungsten oxide nanorod (NR-WO3) carrier

[0077] First, 2.5mmol (3.06g) (NH4) 10 W 12 O4·5H2O was placed in a round-bottom flask, 40mL of deionized water was added and stirred; then 10mL of 2.5mol / L dilute nitric acid solution was slowly added dropwise to the above suspension, condensed and refluxed at 85°C for 1h; then the precipitate after the reaction was poured into a stainless steel hydrothermal autoclave with a polytetrafluoroethylene liner and heated at 160°C for 12h, cooled to room temperature, centrifuged and filtered to obtain a precipitate, and the precipitate was washed 3 times with deionized water; finally, it was dried at 60°C overnight to obtain a light yellow tungsten oxide powder (oxide nanorod carrier).

[0078] (2) Preparation of supported Ni single-site adiponitrile hydrogenation catalyst Ni / WO3:

[0079] At room temperature, 300 mg of the NR-WO3 powder obtained in step (1) is uniformly dispersed in 30 mL of ethanol by ultrasonication and stirring; 3 mL of a 5 mg / mL nickel nitrate aqueous solution is then added dropwise to the dispersion, stirred for 1 hour, and then heated to completely evaporate the ethanol to obtain a solid powder; finally, the solid powder is heated to 350° C. at a rate of 5° C. / min in a mixed gas of hydrogen and argon (the volume fraction of hydrogen in the mixed gas is 5%), and calcined for 2 hours to obtain a supported Ni single-site adiponitrile hydrogenation catalyst Ni / WO3, named Ni / WO3, in which the loading mass fraction of metal Ni is 5%.

[0080] Comparative Example 3:

[0081] A method for preparing a supported Ni single-site adiponitrile hydrogenation catalyst comprises the following steps:

[0082] The preparation method is the same as that of Comparative Example 2, except that the amount of nickel nitrate aqueous solution added in step (2) is changed to 1.2 mL, and the loading mass fraction of metal Ni in the prepared catalyst is 2%.

[0083] Comparative Example 4:

[0084] A method for preparing a supported Ni single-site adiponitrile hydrogenation catalyst comprises the following steps:

[0085] The preparation method is the same as that of Comparative Example 2, except that the amount of nickel nitrate aqueous solution added in step (2) is changed to 1.8 mL, and the loading mass fraction of metal Ni in the prepared catalyst is 3%.

[0086] Comparative Example 5:

[0087] A method for preparing a supported Ni single-site adiponitrile hydrogenation catalyst comprises the following steps:

[0088] The preparation method is the same as that of Comparative Example 2, except that the amount of nickel nitrate aqueous solution added in step (2) is changed to 2.4 mL, and the loading mass fraction of metal Ni in the prepared catalyst is 4%.

[0089] Comparative Example 6:

[0090] A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst comprises the following steps:

[0091] (1) Preparation of tungsten oxide nanorod (NR-WO3) carrier

[0092] First, 2.5mmol (3.06g) (NH4) 10 W 12O4·5H2O was placed in a round-bottom flask, 40mL of deionized water was added and stirred; then 10mL of 2.5mol / L dilute nitric acid solution was slowly added dropwise to the above suspension, condensed and refluxed at 85°C for 1h; then the precipitate after the reaction was poured into a stainless steel hydrothermal autoclave with a polytetrafluoroethylene liner and heated at 160°C for 12h, cooled to room temperature, centrifuged and filtered to obtain a precipitate, and the precipitate was washed 3 times with deionized water; finally, it was dried at 60°C overnight to obtain a light yellow tungsten oxide powder (oxide nanorod carrier).

[0093] (2) Preparation of Pt1 / NR-WO3 catalyst precursor

[0094] At room temperature, 300 mg of the NR-WO3 powder obtained in step (1) was uniformly dispersed in 30 mL of ethanol by ultrasound and stirring; then 6 μL of a 5 mg / mL platinum nitrate aqueous solution was added dropwise to the dispersion, stirred at 400 rpm for 1 h, and then heated to completely evaporate the ethanol to obtain a solid powder Pt1 / NR-WO3 catalyst precursor.

[0095] (3) Preparation of Pt1-Ni / NR-WO3 catalyst:

[0096] At room temperature, 300 mg of the Pt1 / NR-WO3 catalyst precursor obtained in step (2) was uniformly dispersed in 30 mL of ethanol by ultrasonication and stirring; then 3 mL of a 5 mg / mL nickel nitrate aqueous solution was added dropwise to the dispersion, and after stirring for 1 hour, the ethanol was completely evaporated by heating to obtain a solid powder Pt1-Ni / NR-WO3 catalyst, named PtNi / WO3.

[0097] Test example:

[0098] 1. Experiment on catalytic hydrogenation of adiponitrile to produce primary amines

[0099] (1) Experimental methods

[0100] 20 mg of the catalyst was dispersed in a glass reaction bottle containing 2 mL of ethanol, and then transferred to a 500 mL autoclave, 50 μL of a 5 mol / L sodium hydroxide solution and 1 mmol of adiponitrile were added, and the mixture was washed with 1 MPa hydrogen for three times and then reacted in a 2 MPa hydrogen atmosphere at a reaction temperature of 100° C. After the reaction, the primary amine content in the liquid phase was quantitatively analyzed by gas chromatography, and subsequent analysis was performed.

[0101] The catalysts obtained by mixing Examples 1-4, Comparative Examples 1-5, and Comparative Example 1 and Comparative Example 2 in a mass ratio of 1:1 were used as experimental catalyst samples for experiments.

[0102] (2) Experimental results

[0103] The experimental results are as follows Figure 2 shown.

[0104] in, Figure 2 Figure a in the middle is a schematic diagram of the dual-site hydrogenation reaction of the supported PtNi dual-site adiponitrile hydrogenation catalyst prepared by the present invention. Figure 2 Figures b and c show the catalytic hydrogenation performance of different catalysts under 100°C and 2MPa hydrogen conditions. According to the experimental results, the catalyst sample Pt-Ni / WO3-350 prepared in Example 1 of the present invention has very excellent catalytic activity and the highest primary amine selectivity (>95%). Figure 2 Figure d in the middle shows catalysts with different Ni metal loadings (i.e., catalysts prepared in Examples 1-4 and Comparative Examples 1-4). According to the experimental data in the figure, as the Ni loading increases from 2% to 5%, the rate ratios of Pt-Ni / WO3 and Ni / WO3 catalysts increase by 5.6 times and 3.5 times, respectively, which fully demonstrates that the overflow hydrogen provided by Pt enhances the reaction activity of Ni. Figure 2 Figure e shows that through H2-TPR testing, both Pt / WO3 and Ni / WO3 samples have obvious characteristic peaks, among which Ni 2+ Restore to Ni 0 The temperature is 384℃. When metal Pt and Ni form a dual site, the reduction temperature of Ni in Pt-Ni / WO3 (290℃) is lower than that of Ni / WO3, which confirms the hydrogen overflow phenomenon between Pt and Ni bimetallic. Specifically, H2 is activated and dissociated on the single atom Pt to form activated hydrogen species *H, which then overflows on the surface of the WO3 support to promote Ni 2+ Reduction to Ni 0 In addition, according to Figure 2 As shown in Figure f, under the same catalytic conditions, the Pt-Ni / WO3-350 catalyst prepared in Example 1 of the present invention not only has a much higher hydrogenation reaction rate than the catalyst prepared in the comparative example, but also has a primary amine selectivity of more than 95%, and a TOF value of up to 519.1h -1 , which is 5.5 times that of NiWO3 obtained in Example 2.

[0105] 2. Study on the reaction mechanism of catalytic hydrogenation of adiponitrile to primary amines

[0106] The catalysts prepared in Example 1 and Examples 5-8 were used for the experiment. The number of oxygen defects on the catalyst surface was characterized by X-ray photoelectron spectroscopy and H2-TPR spectra. 5+ The number of oxygen defects was used instead of the oxygen defect concentration, and an experiment was carried out to catalyze the hydrogenation of adiponitrile to produce primary amines to detect its conversion rate (Conv.) and selectivity (Sel.).

[0107] The experimental results are as follows Figure 3 As shown, Figure 3As shown in Figures a and b, with the increase of calcination temperature during the preparation process, the amount of Ov on the catalyst surface gradually increases, and according to the H2-TPR spectrum, the characteristic distribution between 50-200°C can be attributed to the hydrogen overflow between Pt and Ni metal on the surface of the Pt-Ni / WO3 catalyst, among which the hydrogen overflow temperature of the Pt-Ni / WO3-550 sample is as low as 65°C. Figure 3 Figures c and d show that under the same experimental conditions, the Pt-Ni / WO3-550 catalyst exhibits the highest activity and the lowest reduction temperature, indicating that the hydrogen overflow rate is greater than that of other catalysts. When the calcination temperature is further increased to 600℃ and 650℃, the reaction rate drops sharply. It is speculated that the reason is that the OH formed by the overflow of *H on the WO3 surface is limited.

[0108] 3. Primary amine selectivity and Ni on the surface of Pt-Ni / WO3 catalyst at different calcination temperatures 0 Relationship

[0109] The catalysts prepared in Example 1 and Examples 5-8 were used for experiments. X-ray photoelectron spectroscopy was used to analyze the primary amine selectivity and the Ni content on the surface of the Pt-Ni / WO3 catalyst at different calcination temperatures. 0 relationship.

[0110] The experimental results are as follows Figure 4 As shown. Figure 4 It can be seen that with the increase of calcination temperature, the Ni 0 The number gradually increases, and by testing the d-band center, the catalyst's desorption ability for the product gradually increases, which well explains the reason for the improvement of primary amine selectivity.

[0111] In summary, the present invention constructs a bimetallic active site catalyst by introducing Pt and Ni on a reducible WO3 carrier, which can catalyze the hydrogenation of adiponitrile to primary amines under mild conditions. Specifically, single-atom Pt serves as an activation site for H2, and the overflow of *H on the WO3 surface allows the adiponitrile molecules adsorbed on the surface of Ni particles to complete the hydrogenation process, thereby achieving high activity of the Pt-Ni / WO3 catalyst and high selectivity for primary amines.

[0112] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a supported PtNi dual-site adiponitrile hydrogenation catalyst, characterized in that: The following steps are involved: (1) Preparation of tungsten oxide nanorod carrier: disperse ammonium tungsten oxide pentahydrate in water, add acidic solution, condense and reflux, heat to react, centrifuge and filter, and dry the precipitate to obtain; (2) Preparation of catalyst precursor: dispersing the tungsten oxide nanorod carrier obtained in step (1) in a solvent, adding a platinum salt solution, stirring, evaporating the solvent, and calcining the solid to obtain; (3) Preparation of supported PtNi dual-site adiponitrile hydrogenation catalyst: The catalyst precursor obtained in step (2) is dispersed in a solvent, a nickel salt solution is added, stirred, the solvent is evaporated, and the solid is calcined to obtain the catalyst.

2. The method for preparing the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 1, characterized in that: In the step (1), the molar volume ratio of ammonium tungstate pentahydrate, water and acidic solution is 1-5mmol:30-50mL:5-15mL; the acidic solution is nitric acid solution with a concentration of 2-3mol / L.

3. The method for preparing the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 1, characterized in that: In the step (1), the condensation reflux temperature is 80-90°C and the time is 30-90 min; the heating reaction temperature is 120-200°C and the time is 10-15 h; the drying temperature is 40-80°C and the time is 5-12 h.

4. The method for preparing the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 1, characterized in that: In the step (2), the mass volume ratio of the oxide nanorod carrier, the solvent and the platinum salt solution is 200-400 mg: 10-50 mL: 4-8 μL; the solvent is ethanol; the platinum salt solution is an aqueous solution of platinum nitrate, and the concentration is 3-7 mg / mL.

5. The method for preparing the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 1, characterized in that: The stirring time in step (2) is 30-90 min, and the rotation speed is 300-500 rpm; the calcination conditions are: in a mixture of hydrogen and rare gas, the temperature is raised to 300-700° C. at a rate of 3-7° C. / min, and kept warm for 1-3 h, wherein the volume fraction of hydrogen in the mixture is 1-10%.

6. The method for preparing the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 1, characterized in that: In the step (3), the mass volume ratio of the catalyst precursor, the solvent and the nickel salt solution is 200-400 mg: 10-50 mL: 1-10 mL; the solvent is ethanol; and the nickel salt solution is a nickel nitrate aqueous solution with a concentration of 3-7 mg / mL.

7. The method for preparing the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 1, characterized in that: The stirring time in step (3) is 30-90 min, and the rotation speed is 300-500 rpm; the calcination conditions are: in a mixture of hydrogen and rare gas, the temperature is raised to 300-700° C. at a rate of 3-7° C. / min, and kept warm for 1-3 h, wherein the volume fraction of hydrogen in the mixture is 1-10%.

8. A supported PtNi dual-site adiponitrile hydrogenation catalyst, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 8 in catalyzing the hydrogenation reaction of adiponitrile to prepare primary amines.

10. A method for preparing primary amines by catalytic hydrogenation of adiponitrile, characterized in that: The supported PtNi dual-site adiponitrile hydrogenation catalyst according to claim 8, a reaction solvent, an alkaline solution and adiponitrile are mixed, and reacted at 80-120° C. under a hydrogen pressure of 1-3 MPa to obtain a primary amine; The mass ratio of the catalyst to adiponitrile is 10-30 mg:50-150 mg.

Citation Information

Patent Citations

  • Nanotube / porous Ti / W / Ni oxide thin film catalytic electrode in-site loaded with platinum / palladium nanoparticles and preparation method therefor

    CN105261763A

  • Catalyst for preparing primary amine through nitrile hydrogenation and preparation method thereof

    CN117899856A

  • Supported catalyst Pt / PC-In2O3, preparation method and application of supported catalyst Pt / PC-In2O3 in hydrogen production by methanol water phase reforming

    CN117960169A

  • Supported CuPt bimetallic active site catalyst as well as preparation method and application thereof

    CN118217969A

  • Metal modified Pd / Ni catalysts

    US20030207761A1

Cited By

  • A catalyst for preparing hexanediamine by hydrogenating adiponitrile, a preparation method and application thereof

    CN122787027A