Preparation method and application of 3D printing zero-valent iron doped ferrophosphorus composite material
The zero-valent iron-doped iron-phosphate composite material prepared by 3D printing technology uses phosphating reaction to form a highly reactive catalyst, which solves the problem of limited electron transfer rate in the catalyst reaction of traditional iron-based materials and achieves efficient degradation of water. Carbamazepine has economic benefits and environmental advantages.
Patent Information
- Application Number
- CN202410992149.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional iron-based materials have limited electron transfer rates and Fe2+/Fe3+ cycle conversion in catalyst reactions, making it difficult to effectively degrade organic pollutants in water, especially carbamazepine.
The zero-valent iron-doped phosphate-ferrous composite material is prepared by 3D printing technology. Through high-energy ball milling and laser rapid heating, the organic phosphorus source releases PH3 and phosphorus elements and undergoes phosphating reaction with Fe0, forming a catalyst with high reactivity and porous structure. Efficiently degrade carbamazepine in water.
It has achieved industrial application of efficient degradation of carbamazepine, with high reactive activity, low oxidation and corrosion and easy recycling economic benefits, and has significantly improved the degradation performance of traditional metal powder catalysts.
Smart Images

Figure CN118874502A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of organically polluted wastewater and 3D printing materials, and in particular to a preparation method and application of a 3D printing zero-valent iron-doped ferrophosphorus composite material. Background Art
[0002] In recent years, 3D printing technology has become an innovative method for manufacturing complex structures with excellent size and geometric controllability, and its application in the field of catalyst material preparation has received widespread attention. Compared with traditional catalyst preparation methods, 3D printing technology has obvious advantages, including simple operation and high degree of automation, material integrated molding, free structural design, more efficient complex integrated 3D structure, material saving, and certain compressive resistance of materials. These advantages enable 3D printing technology to realize the manufacture of multi-scale objects, which not only have the characteristics of nanomaterials and customized geometric shapes, but also improve the efficiency between design iterations in one step and increase the integration of components. Through these advantages, 3D printing technology can freely design the structure and form of catalysts, which can solve the problem that traditional metal powder catalysts are difficult to recycle in Fenton-like reactions, and improve the practicality and feasibility of metal catalysts in actual water purification.
[0003] Traditional iron-based materials, such as iron oxide and zero-valent iron, are mostly affected by the electron transfer rate and Fe 2+ / Fe 3+ The excellent electron transfer ability and regulation of Fe 2+ / Fe 3+ The rapid redox cycle of Fenton reaction or Fenton-like reaction is the key to its application. Iron phosphide is a typical iron-based material with rich Fe 2+ It also has a lower electron transfer resistance, making it easier to activate oxidants in the Fenton reaction to produce highly active free radicals to quickly degrade organic pollutants.
[0004] The 3D printed zero-valent iron-doped ferrophosphorus material provided in the present invention can effectively degrade pollutants such as carbamazepine in water. Summary of the invention
[0005] In order to solve the shortcomings of the prior art, the present invention provides a method for preparing a zero-valent iron-doped phosphorus-iron composite material using a 3D printing technology. The method comprises: mixing an appropriate amount of an organic phosphorus source with Fe by a pre-high-energy ball milling method. 0 / FeP metal powder is mixed. Because of the rapid heating of the laser during the 3D printing process, the organic phosphorus source will release PH3 and phosphorus at high temperature. Since phosphorus has electrophilicity and high electron donating ability, it can react with Fe 0The metal powder undergoes phosphating reaction to form phosphide. The high reducibility of PH3 will further slow down the oxidation during the preparation of iron-based materials. The final 3D printed zero-valent iron-doped phosphorus-iron composite material has excellent water treatment performance and can be used to efficiently degrade pollutants such as carbamazepine in water. Compared with traditional metal powders, it has the characteristics of high reactivity, high specific surface area and high cycle performance. Due to its low raw material cost, it also has both economic and environmental benefits.
[0006] The material preparation method of the present invention and the process of degrading pollutants thereof include the following steps:
[0007] Step 1: Weigh the organic phosphorus source, zero-valent iron and ferrophosphorus powder in a certain mass ratio, mix them, and add them into a ball mill jar pre-placed with ball mill steel balls of the same mass, wherein the weight of the steel balls is four times that of the powder mixture.
[0008] Step 2: Add a certain amount of ethanol to each of the four ball mills for lubrication, and use a planetary ball mill to rotate the mixed powder in the ball mill forward and reverse, and stir and grind it thoroughly for 2 hours.
[0009] Step 3: Place the ground powder in an oven and dry it at temperature T1 for 2 to 3 hours to obtain a completely dry mixed powder.
[0010] Step 4: The obtained mixed powder is mechanically sieved on an oscillator through a 200-mesh sieve for 10 minutes and then falls into an iron plate for collection.
[0011] Step 5: Use the SLM280 3D printer to place the stainless steel plate on the molding tank and level it so that the molding tank is completely horizontal. Then install the powder spreading scraper and lower it until it is basically attached to the stainless steel plate on the molding tank. Place the powder collected by the iron plate into the powder spreading tank and lower it to a suitable height to prepare for the next step of printing.
[0012] Step 6: Open the argon gas bottle and cooling water tank in turn, supply argon gas to reduce the dissolved oxygen content in the printer body to about 300ppm and the water tank temperature to 20℃, open and download the pre-modeled 3D model (the scanning strategy uses 75° rotation and alternating scanning in the X and Y directions with equal spacing, the scanning speed range is 800-1000mm / s, the laser power range is 180-220W, the scanning spacing is 0.06-0.12mm, and the powder layer thickness is 0.03mm), set the peak value to 100, and print after turning on the laser.
[0013] Step 7: Cut the finished material from the stainless steel plate, soak it in anhydrous ethanol and perform ultrasonic treatment for 5 minutes, repeating 2 to 3 times to remove the oil stains on the surface.
[0014] Step 8: Prepare pollutants with a concentration of C1 and catalyst materials with a concentration of C2 and add them into a beaker for degradation experiments.
[0015] Step 9: At different reaction times t, 1 ml of the reaction solution was added to a 2 ml liquid phase vial, and a sodium thiosulfate solution with a concentration of C3 was added to terminate the reaction. The reaction solution was placed in a high performance liquid chromatograph to detect the residual concentration of the pollutant.
[0016] In step 1: the organic phosphorus source includes but is not limited to one of triphenyl phosphine, tributyl phosphine and tricyclohexyl phosphine.
[0017] In step 3: the oven temperature T1 is 50°C to 60°C.
[0018] In step 8: the pollutant concentration C1 is 5-20 ppm, and the catalyst concentration is 1-3 g / L
[0019] In step nine: the reaction time t is 0 to 30 min, and the concentration C3 of the added sodium thiosulfate is 3 mol / L.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The 3D printed zero-valent iron-doped ferrophosphorus composite material prepared by the present invention has excellent physical and chemical properties, such as more concentrated pore structure, high porosity, high specific surface area and high reactivity.
[0022] 2. The 3D printed zero-valent iron-doped ferrophosphorus composite material prepared by the present invention has good recycling performance, and the industrial degradation feasibility of organic pollutants such as carbamazepine is high.
[0023] 3. In the process of preparing the 3D printed porous zero-valent iron-doped phosphorus-iron composite material, the organic phosphorus source releases phosphorus under high temperature of the laser, which promotes the phosphating reaction and further purifies the FeP / Fe 0 Composite materials.
[0024] 4. The 3D printed zero-valent iron-doped phosphorus-iron composite material prepared by the present invention has a low degree of oxidative corrosion after the reduction effect of PH3 generated by high-temperature pyrolysis.
[0025] 5. The 3D printed zero-valent iron-doped ferrophosphorus composite material prepared by the present invention is easier to collect and reuse than traditional metal powder catalyst materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a comparison of the physical image and electron microscope image of the 3D material and powder material.
[0027] Figure 2 Comparison of carbamazepine degradation patterns of 3D material and powder material.
[0028] Figure 3 This is a comparison of the degradation patterns of carbamazepine under different laser high temperatures.
[0029] Figure 4 This is a comparison chart of the catalyst specific surface area bar graphs under different laser high temperatures. DETAILED DESCRIPTION
[0030] In order to better explain the present invention, the following is a detailed description of a specific method for preparing a 3D printed zero-valent iron-doped ferrophosphorus composite material and actual application scenarios in combination with specific embodiments of the present invention, but the protection scope of the present invention is not limited to the following contents.
[0031] The material preparation method of the present invention and the process of degrading pollutants thereof include the following steps:
[0032] Step 1: Weigh the organic phosphorus source, zero-valent iron and ferrophosphorus powder in a certain mass ratio, mix them, and add them into a ball mill jar pre-placed with ball mill steel balls of the same mass, wherein the weight of the steel balls is four times that of the powder mixture.
[0033] Step 2: Add a certain amount of ethanol to each of the four ball mills for lubrication, and use a planetary ball mill to rotate the mixed powder in the ball mill forward and reverse, and stir and grind it thoroughly for 2 hours.
[0034] Step 3: Place the ground powder in an oven and dry it at temperature T1 for 2 to 3 hours to obtain a completely dry mixed powder.
[0035] Step 4: The obtained mixed powder is mechanically sieved on an oscillator through a 200-mesh sieve for 10 minutes and then falls into an iron plate for collection.
[0036] Step 5: Use the SLM280 3D printer to place the stainless steel plate on the molding tank and level it so that the molding tank is completely horizontal. Then install the powder spreading scraper and lower it until it is basically attached to the stainless steel plate on the molding tank. Place the powder collected by the iron plate into the powder spreading tank and lower it to a suitable height to prepare for the next step of printing.
[0037] Step 6: Open the argon gas bottle and cooling water tank in turn, supply argon gas to reduce the dissolved oxygen content in the printer body to about 300ppm and the water tank temperature to 20℃, open and download the pre-modeled 3D model (the scanning strategy uses 75° rotation and alternating scanning in the X and Y directions with equal spacing, the scanning speed range is 800-1000mm / s, the laser power range is 180-220W, the scanning spacing is 0.06-0.12mm, and the powder layer thickness is 0.03mm), set the peak value to 100, and print after turning on the laser.
[0038] Step 7: Cut the finished material from the stainless steel plate, soak it in anhydrous ethanol and perform ultrasonic treatment for 5 minutes, repeating 2 to 3 times to remove the oil stains on the surface.
[0039] Step 8: Prepare pollutants with a concentration of C1 and catalyst materials with a concentration of C2 and add them into a beaker for degradation experiments.
[0040] Step 9: At different reaction times t, 1 ml of the reaction solution was added to a 2 ml liquid phase vial, and a sodium thiosulfate solution with a concentration of C3 was added to terminate the reaction. The reaction solution was placed in a high performance liquid chromatograph to detect the residual concentration of the pollutant.
[0041] In the present invention, the present invention uses an SLM 280 3D printer device for batch printing, and performs real-time temperature monitoring by adjusting different laser powers and a built-in wide-range infrared thermometer to obtain catalyst materials prepared under different laser high temperatures.
[0042] Embodiment 1:
[0043] A 3D printed zero-valent iron-doped ferrophosphorus composite material for homogeneous Fenton reaction degradation of carbamazepine.
[0044] The material preparation method is as follows:
[0045] (1) Weigh 6 g of triphenylphosphine powder, 6 g of ferrous phosphide powder and 112 g of
[0046] Zero-valent iron powder is placed in a ball mill. Prepare four ball mills in total and add steel balls at a material-ball ratio of 1:4. Finally, add 2 ml of ethanol (lubricant) to each jar.
[0047] (2) Place the four ball mills in step (1) into a planetary ball mill and perform high-energy ball milling at a speed of 550 r / min for 2 h.
[0048] (3) The powder obtained by ball milling in step (2) was placed in an oven at 60° C. and dried for 3 h until the powder reached a constant weight.
[0049] (4) The dried powder in step (3) was mechanically sieved on an oscillator for 10 minutes and passed through a 200-mesh sieve to obtain a fine powder.
[0050] (5) Use Hanbang SLM280 3D printer equipment, place the metal stainless steel plate on the molding tank and level it so that the molding tank is completely horizontal, then install the powder spreading scraper and lower it until it is basically attached to the metal stainless steel plate on the molding tank. Place the powder refined by ball milling in step (4) into the powder spreading tank and lower it to a suitable height.
[0051] (6) Open the argon gas bottle and cooling water tank in turn, supply argon gas to reduce the dissolved oxygen content of the printer body to about 300ppm and the water tank temperature to 20℃, open and download the pre-modeled 3D model (the scanning strategy uses 75° rotation and alternating scanning in the X and Y directions with equal spacing, the scanning speed range is 800-1000mm / s, the laser power range is 180-220W, the scanning spacing is 0.06-0.12mm, and the powder layer thickness is 0.03mm), set the peak value to 100, and turn on the laser before printing. The whole printing process takes about 5 hours to obtain the finished material.
[0052] (7) The finished material of step (6) was cut from the stainless steel plate, and was soaked in anhydrous ethanol and ultrasonically treated for 5 min. This process was repeated 2 to 3 times to remove the oil stains on the surface.
[0053] Embodiment 2:
[0054] The 3D printed zero-valent iron-doped ferrophosphorus composite material prepared in Example 1 was used as a catalyst to degrade wastewater containing carbamazepine:
[0055] (8) Carbamazepine at a concentration of 10 ppm was added to a 150 ml beaker and water was added to the reaction volume of 100 ml.
[0056] (9) The 3D printed zero-valent iron-doped ferrophosphorus composite material with a concentration of 1 g / L was placed in a 1‰ HCl solution for ultrasonic pickling for 5 minutes and then poured into the beaker of step (8).
[0057] (10) After adding 1 mM hydrogen peroxide to the beaker in step (8), start timing. At 0, 0.5, 1, 2, 3, 5, 7, 10, 20, and 30 hours, take 1 ml of the reaction solution and put it into a 2 ml liquid phase vial. Add 20 μl of 3 M sodium thiosulfate solution to terminate the reaction.
[0058] (11) The reaction solution obtained in step (10) is placed in a high performance liquid chromatograph to detect the residual concentration of pollutants.
[0059] (12) Metal Fe 0 / FeP metal powder material replaces the 3D printed zero-valent iron-doped ferrophosphorus composite material and repeats the above steps (9) to (11). After comparison, it can be found that the material of the present invention has better degradation performance than the original Fe / FeP material powder material.
[0060] like Figure 1 As shown, the 3D printed zero-valent iron-doped ferrophosphorus composite material prepared by the present invention is easier to recycle and reuse than the powdered iron-based material, and more pores can be seen in the 3D printed material under an electron microscope, which will lead to an increase in the active sites of the material, thereby improving the reaction activity.
[0061] like Figure 2 As shown, the zero-valent iron of the powder material and the 3D printed material is basically unable to degrade carbamazepine, with degradation rates of only 4.00% and 7.43%. The degradation rates of carbamazepine in the 3D printed zero-valent iron-doped phosphide-iron composite material prepared by the present invention and doped with iron phosphide are increased to 30.45% and 81.19%, indicating that the iron phosphide-doped zero-valent iron material can highly activate hydrogen peroxide to degrade carbamazepine.
[0062] like Figure 3 As shown in Figure 2, the degradation effect of the catalyst increases with the increase of laser temperature. This may be because the organic phosphorus source is continuously pyrolyzed at high temperature, and the released phosphorus improves the active sites of the catalyst and optimizes the overall performance of the catalyst.
[0063] like Figure 4 As shown, the specific surface area of the catalyst increases with the increase of laser temperature, which further verifies that the improvement of the catalytic activity of the catalyst by laser high temperature depends on the phosphorus and PH3 released by the high-temperature pyrolysis of the organic phosphorus source. The phosphorus phosphating reaction can improve the catalytic performance of the catalyst material, and PH3 can expand the catalyst pores and increase the specific surface area of the catalyst. The 3D printed zero-valent iron doped phosphorus iron composite material prepared by the present invention has excellent physical and chemical properties, such as more concentrated pore structure, high porosity, high specific surface area and high reactivity.
[0064] The 3D printed zero-valent iron doped ferrophosphorus composite material prepared by the present invention has good cycle performance, and the industrial degradation feasibility of organic pollutants such as carbamazepine is high. In the process of preparing the 3D printed porous zero-valent iron doped ferrophosphorus composite material by the present invention, the organic phosphorus source releases phosphorus element under the high temperature of the laser, which promotes the phosphating reaction and further purifies the FeP / Fe 0 Composite material. The 3D printed zero-valent iron doped ferrophosphorus composite material prepared by the present invention has a low degree of oxidative corrosion after the reduction effect of PH3 generated by high-temperature pyrolysis. Compared with traditional metal powder catalyst materials, the 3D printed zero-valent iron doped ferrophosphorus composite material prepared by the present invention is easy to collect and reuse. In the present invention, a specific method and application for preparing a 3D printed zero-valent iron doped ferrophosphorus composite material is provided. The present invention uses a customized built-in wide-range infrared thermometer to monitor the temperature of the printing molding tank in real time, so that the printing temperature can be controlled. In subsequent experiments, the doped catalyst material-organic phosphorus source will produce different degradation effects due to high-temperature decomposition at different laser temperatures. It is also verified that different laser high temperatures may affect the release of phosphorus and PH3, thereby improving the degradation efficiency of the catalyst. At the same time, the present invention uses the high temperature of the SLM280 laser to allow the added organic phosphorus source to undergo controllable phosphorus decomposition and release, so that the prepared catalyst has higher active sites and degradation effects.
Claims
1. A method for preparing a 3D printed zero-valent iron-doped phosphorus-iron composite material, comprising the following steps: Step 1: Weigh the organic phosphorus source, zero-valent iron and ferrophosphorus powder according to a certain mass ratio, and add them into a ball milling jar pre-placed with ball milling steel balls of the same mass, wherein the weight of the steel balls is four times that of the powder mixture; Step 2: Add a certain amount of ethanol to each of the four ball mills for lubrication, and use a planetary ball mill to rotate the mixed powder in the ball mill forward and reverse, and fully stir and grind for 2 hours; Step 3: Place the ground powder in an oven and dry it at temperature T1 for 2 to 3 hours to obtain a completely dry mixed powder; Step 4: The obtained mixed powder is mechanically sieved on an oscillator through a 200-mesh screen for 10 minutes and then falls into an iron plate for collection; Step 5: Use the SLM280 3D printer to place the stainless steel plate on the molding tank and level it so that the molding tank is completely horizontal. Then install the powder scraper and lower it until it is basically attached to the stainless steel plate on the molding tank. Step 6: Open the argon gas bottle and cooling water tank in turn, supply argon gas to reduce the dissolved oxygen content of the printer body to about 300ppm and the water tank temperature to 20℃, open and download the pre-built 3D model (the scanning strategy adopts 75° rotation and alternating scanning in X and Y directions with equal spacing, the scanning speed range is 800-1000mm / s, the laser power range is 180-220W, the scanning spacing is 0.06-0.12mm, and the powder layer thickness is 0.03mm), set the peak value to 100, and print after turning on the laser; Step 7: Cut the finished material from the stainless steel plate, soak it in anhydrous ethanol and ultrasonically treat it for 5 minutes, repeat 2 to 3 times to remove the oil on the surface; Step 8: Prepare pollutants with a concentration of C1 and catalyst materials with a concentration of C2 and add them into a beaker for degradation experiment; Step nine: At different reaction times t, take 1 ml of the reaction solution and add it into a 2 ml liquid phase vial, and add sodium thiosulfate solution with a concentration of C3 to terminate the reaction.
2. The method according to claim 1, characterized in that: In step 1: the organic phosphorus source includes but is not limited to one of triphenyl phosphine, tributyl phosphine and tricyclohexyl phosphine.
3. The method according to claim 1, characterized in that: In step 3: the oven temperature T1 is 50°C to 60°C.
4. The method according to claim 1, characterized in that: In step eight: the pollutant concentration C1 is 5 to 20 ppm, and the catalyst concentration is 1 to 3 g / L.
5. The method according to claim 1, characterized in that: In step nine: the reaction time t is 0 to 30 min, and the concentration C3 of the added sodium thiosulfate is 3 mol / L.
6. A 3D printed zero-valent iron-doped phosphorus-iron composite material, characterized in that Prepared according to the method according to any one of claims 1 to 5.
7. Application of a 3D printed zero-valent iron-doped ferrophosphorus composite material in organically contaminated wastewater.
Citation Information
Patent Citations
Transition metal phosphide modified nano-iron composite material, preparation method and application thereof
CN113649034A
Method for preparing porous micron zero-valent iron-doped ferrous sulfide composite material by applying 3D printing technology and application of porous micron zero-valent iron-doped ferrous sulfide composite material
CN115400769A
Phosphorus-doped zero-valent iron modified material, preparation method thereof and method for efficiently reducing and removing pollutants by using phosphorus-doped zero-valent iron modified material
CN115784412A
Phosphorized zero-valent iron material with core-shell structure as well as preparation method and application of phosphatized zero-valent iron material
CN116351445A