One-step synthesis method and application of carbon dot composite MOF photocatalyst

The carbon dot composite MOF photocatalyst was synthesized by one-step hydrothermal method, and the problems of long preparation period and low catalytic efficiency of MIL-88A materials were solved, and efficient alkaline lignin degradation was achieved, with a degradation rate of 70%.

CN118874546AActive Publication Date: 2024-11-01HARBIN UNIV OF SCI & TECH

Patent Information

Application Number
CN202410911796.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing carbon doped iron-based metal organic frame MIL-88A materials have long preparation periods, complex steps, and low catalytic efficiency when used for photolysis of lignin.

Method used

A one-step hydrothermal method was used to synthesize carbon dot composite MOF photocatalysts, which were dispersed by 2-methylimidazole, H2O2 and ethylenediamine under ultrasonic wave, and then mixed with fumaric acid and ferric chloride hexahydrate in a constant temperature hydrothermal reaction. , simplifies the preparation process and improves the activity of the catalyst.

Benefits of technology

The rapid synthesis of carbon dot composite MOF photocatalyst with stable structure is achieved, the catalytic efficiency is improved, and the alkaline lignin degradation rate can reach 70% within 4 hours, significantly shortening the degradation time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874546A_ABST
    Figure CN118874546A_ABST
Patent Text Reader

Abstract

The invention discloses a one-step synthesis method and application of a carbon dot composite MOF (Metal Organic Framework) photocatalyst, relates to a preparation method and application of a carbon dot composite MOF photocatalyst, and aims to solve the technical problems of long preparation period, complex steps and low catalytic efficiency of an existing preparation method of a carbon dot doped iron-based metal organic framework. The method comprises the following steps: putting a mixed solution of 2-methylimidazole, H2O2 and ethylenediamine into an ultrasonic cell crusher for crushing and dispersing, then mixing a dispersion solution with fumaric acid and ferric chloride hexahydrate, transferring the mixed solution into a reaction kettle for hydrothermal reaction, centrifuging, washing and drying to obtain the carbon dot composite MOF photocatalyst. When the photocatalyst prepared by treating 2-methylimidazole serving as a raw material with an ultrasonic cell disruptor is used for photocatalytic degradation of alkaline lignin, the degradation rate of lignin reaches 70% after 4 hours, and the photocatalyst can be used in the field of lignin degradation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of a carbon dot composite MOF photocatalyst, and belongs to the field of photocatalytic functional materials. Background Art

[0002] my country is rich in plant resources, but most of the lignin is still burned directly in the form of waste or as low-grade fuel, which has caused a waste of lignin resources to a certain extent. The current technologies for lignin depolymerization include thermal depolymerization, ionic liquid depolymerization, photoelectrocatalytic depolymerization, etc. However, most depolymerizations have problems such as slow efficiency, low selectivity, high cost, difficult reagent recovery, high energy consumption, and easy pollution. In order to solve the above problems, a new catalytic lignin depolymerization technology with mild reaction conditions, high efficiency, low cost and no pollution is needed. Compared with other lignin depolymerization technologies, photocatalytic technology has outstanding advantages such as no pollution, stable and controllable, which not only makes effective use of lignin, but also alleviates the resource crisis and maintains sustainable development.

[0003] Metal-organic frameworks (MOFs) have the characteristics of large specific surface area, large pore volume, controllable structure, and high concentration of active metal sites, and have been widely used in catalysis and sensing. In the past decade, the iron-based MOF MIL-88A has been applied to water treatment such as heavy metal removal, chemical hydrogen storage such as hydrogen evolution reaction and oxygen evolution reaction, photochemical and electrochemical energy storage and conversion. However, the potential application of MIL-88A in photocatalysis and luminescent sensors faces serious challenges such as charge recombination, low solar energy utilization, low quantum yield, and limited charge transfer between metal ions / clusters and ligands. Recent studies have shown that the rational introduction of carbon dots (CDs) with excellent optical properties, unique quantum confinement, and high conductivity can greatly enhance the function of MIL-88A. The existing methods for preparing CDs-composite MIL-88A materials all adopt a two-step method, that is, first preparing MIL-88A and CDs separately, and then compounding the two. This method has a long preparation cycle and cumbersome steps. At the same time, when the material obtained by this method is used for photolysis of lignin, the photocatalytic effect is poor. This technology mainly solves the above problems and adopts a one-step hydrothermal method to prepare CDs composite MIL-88A material, which has a short preparation cycle, simple steps and high catalytic efficiency. Summary of the invention

[0004] The present invention aims to solve the technical problems of the existing preparation method of carbon dot doped iron-based metal organic framework, such as long preparation cycle, complicated steps and low catalytic efficiency when used for photolysis of lignin, and proposes a one-step synthesis method and application of carbon dot composite MOF photocatalyst.

[0005] The one-step synthesis method of a carbon dot composite MOF photocatalyst of the present invention is carried out according to the following steps:

[0006] 1. Dissolve 2-methylimidazole powder in deionized water, then add H2O2 and ethylenediamine (EDA), stir evenly to obtain a mixed solution; put the mixed solution into an ultrasonic cell disruptor, and perform ultrasonic disruption and dispersion for 10 to 30 minutes under the conditions of an ultrasonic frequency of 20 to 25 kHz, a power of 700 to 900 W, and an ice bath to obtain a dispersion;

[0007] 2. Dissolve fumaric acid in hot water, add the dispersion and mix evenly, then add ferric chloride hexahydrate to obtain a mixed solution; transfer the mixed solution to a reactor lined with polytetrafluoroethylene, and perform a constant temperature hydrothermal reaction at 150-160°C for 4-6 hours. After the reaction is completed, centrifuge and wash the solid phase with water and ethanol in turn, and put it in an oven to dry to obtain a carbon dot composite MOF photocatalyst.

[0008] Furthermore, the concentration of 2-methylimidazole in the mixed solution described in step 1 is 15-16 mg / mL.

[0009] Furthermore, the ratio of the mass of 2-methylimidazole to the volume of H2O2 in the mixed solution described in step 1 is 1g:(13-15)mL; the ratio of the volume of H2O2 to EDA is (9-10):1.

[0010] Furthermore, the ratio of the volume of the dispersion in step 2 to the amount of fumaric acid is 10 mL: (3-4) mmol.

[0011] Furthermore, in step 2, the molar ratio of the organic ligand fumaric acid to the metal ion ferric chloride hexahydrate is (1-1.3):1.

[0012] Furthermore, the temperature of the hot water in step 2 is 55-60° C., which is conducive to the complete dissolution of fumaric acid.

[0013] Furthermore, the rotation speed during the centrifugal separation in step 2 is 10000 r / min, and the centrifugal time is 5 to 10 min.

[0014] The application of the carbon dot composite MOF photocatalyst prepared by the above method is to use the carbon dot composite MOF photocatalyst for photocatalytic degradation of alkaline lignin. The details are as follows:

[0015] The carbon dot composite MOF photocatalyst is dispersed in an alkaline lignin aqueous solution and stirred for 0.5 to 4 hours under light conditions to complete the degradation of the alkaline lignin.

[0016] Furthermore, the added mass of the carbon dot composite MOF photocatalyst is 10% to 50% of the mass of the alkaline lignin.

[0017] Beneficial effects of the present invention:

[0018] 1. The present invention utilizes a one-step synthesis method to prepare a carbon dot composite MOF photocatalyst with a stable structure, simplifies the preparation process, improves the preparation efficiency, and the preparation process is controllable, the product purity is high, and it is easy to achieve large-scale synthesis, making it possible to quickly prepare carbon dot composite MOF materials.

[0019] 2. Carbon dots were prepared using 2-methylimidazole as the carbon source. The carbon dots were distributed on the surface of MIL-88A and embedded in the internal structure through a one-step hydrothermal synthesis method, producing more active sites. The carbon dots had better electrical conductivity and effectively accelerated the separation of photogenerated charges, inhibiting the recombination of photogenerated electrons and holes. The photocatalytic degradation of alkaline lignin was achieved. After 4 hours of photocatalytic degradation, the degradation rate of lignin reached 70%, shortening the degradation time. The carbon dots are a reliable heterogeneous catalytic material with outstanding technical advantages and can be used in the field of lignin degradation. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a physical picture of the carbon dot composite MOF photocatalyst prepared in Example 1;

[0021] Figure 2 This is a SEM image of the carbon dot composite MOF photocatalyst prepared in Example 1;

[0022] Figure 3 XRD pattern of pure MIL-88A prepared in Comparative Example 1;

[0023] Figure 4 XRD spectrum of the carbon dot composite MOF photocatalyst prepared in Example 1;

[0024] Figure 5 TEM image of the carbon dot composite MOF photocatalyst prepared in Example 1;

[0025] Figure 6 The XRD spectrum of the product obtained in Comparative Example 5;

[0026] Figure 7 This is a comparison chart of the results of photocatalytic degradation of alkaline lignin by the photocatalyst prepared in Example 1 and Comparative Example 5;

[0027] Figure 8 These are photos of alkaline lignin before and after degradation by the carbon dot composite MOF photocatalyst prepared in Example 1. DETAILED DESCRIPTION

[0028] Use the following examples to verify the beneficial effects of the present invention:

[0029] Example 1: The one-step synthesis method of the carbon dot composite MOF photocatalyst of this example is carried out according to the following steps:

[0030] 1. Dissolve 0.75 g of 2-methylimidazole powder in 50 mL of deionized water, then add 10 mL of H2O2 and 1 mL of LEDA, stir evenly to obtain a mixed solution; put the mixed solution into an ultrasonic cell disruptor, and perform ultrasonic disruption and dispersion for 30 minutes under the conditions of an ultrasonic frequency of 25 KHz, a power of 720 W, and an ice bath to obtain a dispersion;

[0031] 2. Dissolve 0.58 g of fumaric acid in 50 mL of hot water at 55°C, add 10 mL of the dispersion prepared in step 1, mix well, then add 1.35 g of ferric chloride hexahydrate to introduce metal ions, mix well to obtain a mixed solution; transfer the mixed solution to a reactor lined with polytetrafluoroethylene, and perform a constant temperature hydrothermal reaction at 150°C for 4 hours. After the reaction is completed, centrifuge at a speed of 10000 r / min for 5 minutes, wash the solid phase with water and ethanol for 3 times each, and then dry it in an oven at 60°C for 12 hours to obtain a carbon dot composite MOF photocatalyst, recorded as CDs / MIL.

[0032] Comparative Example 1: This comparative example is to prepare pure MIL-88A, and its specific steps are as follows: 0.58g of fumaric acid is dissolved in 40mL of hot water at a temperature of 55°C, and then 1.35g of ferric chloride hexahydrate is added and mixed evenly, and the mixed solution is transferred to a reactor lined with polytetrafluoroethylene, and a constant temperature hydrothermal reaction is carried out at a temperature of 150°C for 4h. After the reaction is completed, high-speed centrifugation is carried out at a speed of 10000r / min for 5min, and the solid phase is washed with water and ethanol for 3 times each, and then placed in an oven at a temperature of 60°C for drying for 12h to obtain pure MIL-88A.

[0033] The actual photo of the carbon dot composite MOF photocatalyst prepared in Example 1 is as follows Figure 1 As shown, it is a dark brick red sticky powder with a fine texture.

[0034] The scanning electron microscope photo of the carbon dot composite MOF photocatalyst prepared in Example 1 is as follows: Figure 2 As shown, from Figure 2 It can be seen that the carbon dot composite MOF photocatalyst prepared in Example 1 has the traditional structure of MIL-88A, and the doping of carbon dots does not change the special structure of MIL-88A.

[0035] Figure 3 This is the XRD spectrum of pure MIL-88A prepared in Comparative Example 1. Figure 4 is the XRD spectrum of the carbon dot composite MOF photocatalyst prepared in Example 1. Figure 3 and Figure 4It can be seen that the carbon dot composite MOF photocatalyst prepared in Example 1 shows the characteristic peak of carbon dots at 2θ=21°C, indicating that MIL-88A contains the characteristic peak of carbon dots, realizing the composite of MIL-88A with carbon dots.

[0036] Figure 5 The transmission electron microscope (TEM) image of the carbon dot composite MOF photocatalyst prepared in Example 1 is shown in FIG. Figure 5 In B, it can be seen that the carbon dots are successfully composited on MIL-88A and are evenly distributed. Figure 5 C It can be seen that the carbon dots are not only distributed on the surface of MIL-88A, but also embedded in the structure of MIL-88A. This composite structure not only improves the adsorption performance of the material, but also greatly improves the photocatalytic performance.

[0037] Comparative Example 2: This comparative example is different from Example 1 in that an ordinary stirrer is used to replace the ultrasonic cell disruptor in step 1. The specific steps are as follows:

[0038] 1. Dissolve 0.75g of 2-methylimidazole powder in 50mL of deionized water, then add 10mL of H2O2 and 1mL of LEDA, stir evenly to obtain a mixed solution; put the mixed solution on a magnetic stirrer, stir at a stirring speed of 120 rpm for 30 minutes to obtain a dispersion;

[0039] 2. Dissolve 0.58 g of fumaric acid in 30 mL of hot water at 55°C, add 10 mL of the dispersion prepared in step 1, mix well, and then add 1.35 g of ferric chloride hexahydrate, mix well to obtain a mixed solution; transfer the mixed solution to a reactor lined with polytetrafluoroethylene, and perform a constant temperature hydrothermal reaction at 150°C for 4 hours. After the reaction is completed, centrifuge at a speed of 10,000 r / min for 5 minutes, wash the solid phase with water and ethanol for 3 times each, and then dry it in an oven at 60°C for 12 hours to obtain the product.

[0040] In comparative example 2, after the constant temperature hydrothermal reaction in step 2 is completed, a light green solution is obtained with a small amount of black particles. After the product is obtained after centrifugation and drying, a lignin photocatalytic degradation test is carried out, and it is found that the product has no photocatalytic effect at all, and the appearance color is completely different from that of the normal MIL-88A. The stirring conditions in step 1 have a significant impact on the product. The carbon dot precursor is crushed by an ultrasonic cell disruptor, and the damage of the precursor to the MOF construction is removed. Only in the subsequent hydrothermal reaction can the carbon dot composite MOF photocatalyst be synthesized in one step.

[0041] Comparative Example 3: This comparative example is different from Example 1 in that an ordinary ultrasonic cleaning machine is used to replace the ultrasonic cell disruptor in step 1. The specific steps are as follows:

[0042] 1. Dissolve 0.75g 2-methylimidazole powder in 50mL deionized water, then add 10mL H2O2 and 1mL LEDA, stir evenly to obtain a mixed solution; put the mixed solution into an ultrasonic cleaning machine, and ultrasonically treat it for 30min at a power of 600w and a frequency of 40KHz to obtain a dispersion;

[0043] 2. Dissolve 0.58 g of fumaric acid in 30 mL of hot water at 55°C, add 10 mL of the dispersion prepared in step 1, mix well, and then add 1.35 g of ferric chloride hexahydrate, mix well to obtain a mixed solution; transfer the mixed solution to a reactor lined with polytetrafluoroethylene, and perform a constant temperature hydrothermal reaction at 150°C for 4 hours. After the reaction is completed, centrifuge at a speed of 10,000 r / min for 5 minutes, wash the solid phase with water and ethanol for 3 times each, and then dry it in an oven at 60°C for 12 hours to obtain the product.

[0044] In comparative example 3, after the constant temperature hydrothermal reaction in step 2 is completed, a light green solution is obtained. After the product is obtained by centrifugation and drying, a lignin photocatalytic degradation test is performed, and it is found that the product has no photocatalytic effect at all. This indicates that the ordinary ultrasonic cleaning machine in step 1 cannot meet the conditions for synthesizing carbon dot composite MOF photocatalysts because of its low power and the inability to directly act due to the blocking of the cleaning machine and the container wall.

[0045] Comparative Example 4: This comparative example differs from Example 1 in that the 2-methylimidazole in step 1 of Example 1 is replaced by glucose, citric acid, amino acid and sodium citrate, respectively, and the other steps and parameters are the same as those in Example 1.

[0046] In comparative example 4, after the constant temperature hydrothermal reaction in step 2 is completed, a colored solution is obtained, which has no photocatalytic effect on lignin degradation, indicating that 2-methylimidazole is a necessary material for the synthesis of carbon dot precursors, and 2-methylimidazole can be selected as a raw material to synthesize carbon dot composite MOF photocatalysts.

[0047] Comparative Example 5: This comparative example adopts a two-step method to prepare a carbon dot composite MOF photocatalyst, and the specific steps are as follows:

[0048] 1. Preparation of carbon dots: 0.75 g of 2-methylimidazole powder was dissolved in 50 mL of deionized water, and then 1 mL of LEDA was added and stirred to obtain a mixed solution; the mixed solution was placed in an ultrasonic cell disruptor, and ultrasonically crushed and dispersed for 30 min under an ultrasonic frequency of 25 KHz, a power of 720 W, and an ice bath condition; the solution was transferred to a reactor lined with polytetrafluoroethylene, and subjected to a constant temperature hydrothermal reaction at a temperature of 150° C. for 4 h; the solution was filtered through a 0.22 μm filter membrane for 3 times, and then dialyzed with deionized water through a 1000 Da dialysis membrane, and the water was changed every 12 hours until the deionized water had no color change, to obtain a carbon dot dispersion;

[0049] 2. Dissolve 0.58 g of fumaric acid in 30 mL of hot water at 55°C, add 10 mL of the carbon dot dispersion prepared in step 1, mix well, and then add 1.35 g of ferric chloride hexahydrate, mix well to obtain a mixed solution; transfer the mixed solution to a reactor lined with polytetrafluoroethylene, and perform a constant temperature hydrothermal reaction at 150°C for 4 hours. After the reaction is completed, perform high-speed centrifugation at a speed of 10,000 r / min for 5 minutes, wash the solid phase with water and ethanol for 3 times each, and then dry it in an oven at 60°C for 12 hours to obtain a product, which is recorded as two-step CDs / MIL.

[0050] The product obtained in Comparative Example 5 was a dark brick red powder, and its XRD pattern was as follows: Figure 6 As shown in Figure 2, a special peak of carbon dots also appeared at 2θ = 21°C, indicating successful doping. Figure 4 From the comparison of XRD patterns, it can be seen that the amount of carbon incorporated by the one-step method is more advantageous than that by the two-step method under the same conditions, and the effect of the one-step method is better. It can be seen that the one-step method can make the carbon dots and MIL-88A more evenly distributed. It is speculated that since the precursor of the one-step method not only has a small molecular weight, but also becomes even smaller after being crushed by a cell ultrasonic crusher, it is easier to be evenly distributed and doped with the MOF inside or on the surface during its construction, thereby making the performance expression better.

[0051] The carbon dot composite MOF photocatalysts prepared in Example 1 and Comparative Example 5 were used for photocatalytic degradation of alkaline lignin.

[0052] 20 mg of photocatalyst was dispersed in 50 mL of alkaline lignin with a concentration of 1000 mg / L by ultrasound for 3 minutes, and magnetically stirred in the dark for 30 minutes to reach adsorption-desorption equilibrium. Then turn on the xenon lamp, take 2 mL of suspension at 0 min, 10 min, 30 min, 60 min, 90 min, 150 min and 240 min, remove the catalyst through a 0.22 μm filter membrane, and then use an ultraviolet spectrophotometer to measure the absorbance of the sample taken in the experiment. Make a standard curve of the absorbance of lignin solutions of different concentrations at an incident wavelength of 280 nm, and obtain the corresponding formula regression equation: y = 0.298x + 0.0276. The lignin concentration is calculated according to the regression equation using the measured sample absorbance. The degradation efficiency is calculated based on the change in lignin concentration. The degradation efficiency is calculated by the following formula:

[0053] η=(1-Ct / C0)×100%

[0054] Where:

[0055] η——degradation efficiency, %

[0056] C0——initial concentration of lignin solution, mg / mL

[0057] Ct——Concentration of lignin solution at time t, mg / mL

[0058] The degradation results of alkaline lignin by the carbon dot composite MOF photocatalyst prepared in Example 1 and Comparative Example 5 are as follows: Figure 7 As shown, from Figure 7 It can be seen that the carbon dot composite MOF photocatalyst prepared in Example 1 has good photocatalytic performance and has good degradation efficiency in catalyzing alkaline lignin. After 4 hours of degradation, the degradation efficiency is as high as 70%, while the degradation efficiency of the two-step photocatalyst in Comparative Example 5 is only 30% after 4 hours of degradation.

[0059] Figure 8 The following are photos of alkaline lignin before degradation and after 4 hours of photocatalytic degradation using the carbon dot composite MOF photocatalyst prepared in Example 1. Figure 8 It can be seen that the alkaline lignin is a yellow slurry before degradation and a white slurry after degradation.

[0060] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A one-step synthesis method of carbon dot composite MOF photocatalyst, It is characterized in that The method proceeds as follows:

1. Dissolve 2-methylimidazole powder in deionized water and then add H 2 O 2 and ethylenediamine, stirring evenly to obtain a mixed solution; placing the mixed solution in an ultrasonic cell disruptor, and performing ultrasonic disruption and dispersion for 10 to 30 minutes under the conditions of an ultrasonic frequency of 20 to 25 kHz, a power of 700 to 900 W, and an ice bath to obtain a dispersion; 2. Dissolve fumaric acid in hot water, add the dispersion and mix evenly, then add ferric chloride hexahydrate to obtain a mixed solution; transfer the mixed solution to a reactor lined with polytetrafluoroethylene, and perform a hydrothermal reaction at a temperature of 150-160°C for 4-6 hours. After the reaction is completed, centrifuge and wash the solid phase with water and ethanol in turn, and dry it in an oven to obtain a carbon dot composite MOF photocatalyst.

2. A one-step synthesis method of a carbon dot composite MOF photocatalyst according to claim 1, It is characterized in that The concentration of 2-methylimidazole in the mixed solution in step 1 is 15-16 mg / mL.

3. A one-step synthesis method of a carbon dot composite MOF photocatalyst according to claim 1 or 2, It is characterized in that The mass of 2-methylimidazole in the mixed solution in step 1 is equal to H 2 O 2 The volume ratio is 1g: (13-15)mL; H 2 O 2 The volume ratio to EDA is (9-10):

1.

4. A one-step synthesis method of a carbon dot composite MOF photocatalyst according to claim 1 or 2, It is characterized in that The ratio of the volume of the dispersion in step 2 to the amount of fumaric acid is 10 mL: (3-4) mmol.

5. A one-step synthesis method of a carbon dot composite MOF photocatalyst according to claim 1 or 2, It is characterized in that The molar ratio of fumaric acid to ferric chloride hexahydrate in step 2 is (1-1.3):

1.

6. A one-step synthesis method of a carbon dot composite MOF photocatalyst according to claim 1 or 2, It is characterized in that The temperature of the hot water in step 2 is 55-60°C.

7. A one-step synthesis method of a carbon dot composite MOF photocatalyst according to claim 1 or 2, It is characterized in that The rotation speed during the centrifugal separation in step 2 is 10000r / min, and the centrifugal time is 5 to 10min.

8. Application of a carbon dot composite MOF photocatalyst prepared by the method of claim 1, Features This application is to use carbon dot composite MOF photocatalyst for photocatalytic degradation of alkaline lignin.

9. The use of a carbon dot composite MOF photocatalyst according to claim 8, Features The method of photocatalytically degrading alkaline lignin using a carbon dot composite MOF photocatalyst is as follows: dispersing the carbon dot composite MOF photocatalyst into an alkaline lignin aqueous solution, stirring for 0.5 to 4 hours under light conditions, and completing the degradation of the alkaline lignin.

10. The use of a carbon dot composite MOF photocatalyst according to claim 9, It is characterized in that The added mass of the carbon dot composite MOF photocatalyst is 10% to 50% of the mass of the alkaline lignin.

Citation Information

Patent Citations

  • Preparation method and application of carbon quantum dot / metal organic skeleton catalyst

    CN107754861A

  • Z-type ternary photocatalyst TiO2 / MIL-88A (Fe) / g-C3N4 as well as preparation method and application thereof

    CN116273201A

  • R-MIL-88A / OV-BiOBr photo-Fenton catalyst rich in oxygen vacancies as well as preparation method and application of r-MIL-88A / OV-BiOBr photo-Fenton catalyst

    CN116984029A

  • Ternary composite photocatalyst containing carbon quantum dots as well as preparation method and application of ternary composite photocatalyst

    CN117160514A

  • CDs (at) NH2-MIL-88B (at) rMIP nano-enzyme and colorimetric-fluorescence dual-mode sensing method thereof

    CN117929331A

Cited By

  • Bacteria-algae sewage treatment method and functional carrier material for bacterial-algae sewage treatment

    CN119191572A

  • Manganese-based MOF organic-inorganic hybrid catalyst and preparation method thereof

    CN120079446A