Method for recovering mica, feldspar and quartz from molybdenum tailings
By using hydrocyclone grading, magnetic separation, and flotation processes, combined with specific reagents, the problem of separating mica, feldspar, and quartz in molybdenum tailings has been solved, achieving efficient and environmentally friendly resource recovery and improving resource utilization and product purity.
Patent Information
- Application Number
- CN202411103372.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional mineral processing techniques are difficult to effectively separate and recover mica, feldspar, and quartz from molybdenum tailings, leading to resource waste and environmental pollution, and existing methods pose environmental risks.
The process employs hydrocyclone classification, magnetic separation for iron removal, and flotation, combined with the use of specific reagents, to achieve efficient separation and recovery of mica, feldspar, and quartz. This includes pre-classification, magnetic separation, mica flotation, feldspar flotation, and quartz flotation, using conventional equipment and environmentally friendly reagents.
It achieves high-grade recovery of mica, feldspar and quartz, reduces impurity content, reduces reagent usage and environmental pollution, and improves the comprehensive utilization rate of resources. It is suitable for the resource utilization of molybdenum tailings and other tailings.
Smart Images

Figure CN118874665A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of tailings treatment, in particular to a method for recovering mica, feldspar and quartz from molybdenum tailings. Background Art
[0002] Molybdenum is a metal element that was discovered relatively late. Because metal molybdenum has the advantages of high strength, high melting point, corrosion resistance, wear resistance, etc., it has been widely used in industry. There are many metal impurities and non-metallic minerals in molybdenum tailings. The non-metallic minerals are mainly mica, feldspar (potassium feldspar and sodium feldspar), quartz, etc. After recovering the valuable metals in the tailings, traditional metal mines will directly discard the tailings without recovering the non-metallic mineral resources. The non-metallic minerals in the molybdenum tailings are very important raw materials for building materials. Ignoring non-metallic minerals not only affects the economic benefits of enterprises and wastes mineral resources, but also greatly reduces the service life of the tailings pond and causes serious harm to the environment. Moreover, with the over-exploitation of non-metallic mines in recent years, the rich ore resources of non-metallic minerals have been continuously reduced. A large number of low-grade mineral resources in molybdenum tailings have certain development prospects, and also provide a new way out for the comprehensive utilization and application of tailings in metal mines. It has important significance for reducing the waste of mineral resources, reducing the discharge of solid waste from mines, and avoiding excessive mining of non-metallic mines.
[0003] However, there are many types of impurities in molybdenum tailings, and the composition is complex. Due to the reasons of mineral processing technology and equipment, there are problems such as foam weakness and poor selectivity when flotating mica, and some feldspars belonging to the same silicate will be floated out, resulting in low recovery rates of feldspar and quartz minerals; some impurities in molybdenum tailings are similar to the floatability of feldspar or quartz, which has a great impact on the separation process and the quality of the separated products; feldspar and quartz have similar surface properties, and the flotation separation of the two has always been a research hotspot and difficulty in the field of mineral processing. Among them, the method of flotation separation of feldspar and quartz by HF process has been strictly prohibited by the environmental protection department. Based on the above reasons, traditional mineral processing technology cannot effectively separate, recycle and resource these low-grade non-metallic minerals in molybdenum tailings, which greatly limits the comprehensive utilization of non-metallic mineral resources in tailings in actual production. Therefore, it is an urgent problem to study a method for recovering mica, feldspar and quartz from molybdenum tailings with high industrial application feasibility, complete process, green and efficient. Summary of the invention
[0004] The present invention provides a method for recovering mica, feldspar and quartz from molybdenum tailings, which has good collector selectivity, low agent dosage, high product concentrate grade, strong applicability and can achieve "zero" discharge of solid waste, so as to solve the above technical problems.
[0005] To achieve the above-mentioned object, the present invention provides a method for recovering mica, feldspar and quartz from molybdenum tailings, comprising: a pre-classification process of taking the molybdenum tailings as the processing object and using a cyclone to perform classification treatment to obtain an overflow slurry; a magnetic separation process of performing magnetic separation and iron removal on the overflow slurry to obtain a magnetic separation slurry; a mica flotation process of performing flotation on the magnetic separation slurry to obtain a mica concentrate and a mica flotation tailing; a flotation process of performing flotation on the mica flotation tailing to obtain a feldspar concentrate and a feldspar flotation tailing. feldspar flotation process; and, a quartz flotation process of flotating the feldspar flotation tailings to obtain a quartz concentrate; in the pre-classification process, a two-stage series cyclone is used for classification treatment; in the magnetic separation process, the field strength of the magnetic separator is 1-1.2T; in the mica concentrate, the mica content is ≥98.5%; in the feldspar concentrate, the total content of K2O+Na2O is ≥11.5%; in the quartz concentrate, the SiO2 content is ≥99.5%.
[0006] The present invention determines reasonable recycling procedures and steps based on the characteristics of molybdenum tailings, and ultimately accurately and efficiently recycles valuable non-metallic substances such as mica, feldspar and quartz in the tailings, thereby solving the technical shortcomings and deficiencies of previous recycling of specific minerals. The quartz concentrate recovered in the present invention meets the standards of refined quartz sand (the silicon dioxide grade reaches more than 99%), and can be used in ceramics, glass and other industries, and the mica concentrate, feldspar concentrate and quartz concentrate are directly sold as final products, thereby realizing the full utilization of the molybdenum tailings.
[0007] It is further configured that the operation process of the pre-classification step is as follows: the molybdenum tailings slurry with a concentration of 25-35% is sent to the first-level cyclone, the sludge therein is overflowed, and the underflow of the first-level cyclone is sent to the second-level cyclone. After cyclone classification in the second-level cyclone, the overflow slurry is reserved, the underflow of the second-level cyclone is sent to the ball mill for grinding treatment, and is repeatedly sent to the first-level cyclone.
[0008] It is further configured that the standard of the sludge overflowing from the first-stage cyclone is -400 mesh content greater than or equal to 80%; the standard of the overflow slurry from the above-mentioned second-stage cyclone is -200 mesh content of 60-70%.
[0009] The use of cyclones to form a two-stage series connection can achieve the pre-grading and desludging of molybdenum tailings slurry, remove some of the residual reagents for molybdenum selection, and effectively prevent over-grinding during grinding. It can not only grind the coarse-grained tailings slurry to the qualified particle size, but also protect the structure of mica, feldspar and quartz. Grinding treatment can destroy the mineral inclusion form of iron, titanium impurities and other impurities in the tailings, thereby facilitating subsequent magnetic separation and helping to reduce the impurity content in the final product. The non-metallic mineral content in the sludge is low, so it is discarded, which also reduces the processing load of subsequent processes.
[0010] It is further configured that the operation process of the magnetic separation process is as follows: the overflow pulp obtained by pre-classification is sent to the magnetic separator for magnetic separation and iron removal, and the field strength of the magnetic separator is 1-1.2T to separate the magnetic minerals and magnetic separation pulp. Magnetic separation can use magnetic separation equipment to remove impurities and purify the overflow pulp, avoiding the influence of magnetic mineral components such as iron and titanium impurities on subsequent flotation processes, and ensuring the purity of each product.
[0011] It is further configured that the operation process of the mica flotation process is as follows: the magnetic slurry is sent into the mica flotation equipment, and a roughing process is performed to obtain mica roughing tailings and mica roughing concentrates. The mica roughing tailings are subjected to a scavenging process to obtain mica flotation tailings and mica scavenging slurry, and the mica scavenging slurry is sent back to the roughing process. The mica roughing concentrate is first subjected to concentration I to obtain mica concentration I concentrate and mica concentration I tailings, and the mica concentration I tailings are sent back to the roughing process. The mica concentration I concentrate is then subjected to concentration II to obtain mica concentrate and mica concentration II tailings, and the mica concentration II tailings are sent back to the concentration I step. The mica flotation tailings are subjected to inclined plate concentration and dehydration, and the inclined plate bottom flow after inclined plate concentration enters the feldspar flotation process. The inclined plate bottom flow after inclined plate concentration can ensure that the subsequent feldspar flotation concentration is ≥30%. The role of the inclined plate concentration and dehydration of the mica flotation tailings is to reduce the amount of acid used in the subsequent feldspar flotation process.
[0012] It is further configured that in the mica flotation process, the reagents and their usage amounts in the roughing step are as follows: 600-800g / t of water glass, 4000-5000g / t of sodium carbonate, and 80-100g / t of cationic collector; the reagents and their usage amounts in the concentrating step I are as follows: 500-800g / t of sodium carbonate; and the reagents and their usage amounts in the concentrating step II are as follows: 100-200g / t of sodium carbonate. While adjusting the pH of the pulp with sodium carbonate, the selectivity and adsorption of the cationic collector to mica can be enhanced, thereby improving the flotation efficiency and flotation yield, and obtaining mica concentrate with higher yield and grade.
[0013] It is further set that in the mica flotation process, the time for roughing, scavenging and cleaning is 2-5 minutes respectively.
[0014] It is further configured that the operation process of the feldspar flotation step is as follows: the inclined plate bottom flow is sent to the feldspar flotation equipment, a roughing selection is performed to obtain feldspar roughing tailings and feldspar roughing concentrate, the feldspar roughing tailings are scavenged to obtain feldspar flotation tailings and feldspar scavenging slurry, the feldspar scavenging slurry is sent back to the roughing step, the feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings, the feldspar concentration I tailings are sent back to the roughing step, the feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings, the feldspar concentration II tailings are sent back to the concentration I step, and the feldspar flotation tailings enter the quartz flotation process.
[0015] It is further configured that in the feldspar flotation process, the reagents and their usage amounts in the roughing step are as follows: 800-1000g / t of oxalic acid, 400-600g / t of sulfuric acid, 200-500g / t of sodium dodecyl sulfate, and the pH of the pulp is adjusted to 2-3 after acid addition; the reagents and their usage amounts in the selection step I are as follows: 200-400g / t of oxalic acid; the reagents and their usage amounts in the selection step II are as follows: 100-200g / t of oxalic acid. When the pH value (2-3) is near the zero charge point of quartz, the surface of feldspar is negatively charged, and the surface of quartz is uncharged. The collector sodium dodecyl sulfate can be adsorbed on the surface of feldspar, so that the feldspar can float, achieving the purpose of flotation separation of quartz and feldspar.
[0016] It is further set that in the feldspar flotation process, the time for roughing, scavenging and cleaning is 2-5 minutes respectively.
[0017] It is further configured that the operation process of the quartz flotation process is as follows: the feldspar flotation tailings are sent to the quartz flotation equipment, and a roughing process is performed to obtain waste ore and quartz roughing concentrate, the quartz roughing concentrate is finely concentrated to obtain quartz concentrate and quartz fine tailings, and the quartz fine tailings are sent back to the roughing process. In the quartz flotation process, the acid leaching process that uses hydrofluoric acid is not used, which avoids the pollution of acid leaching, has significant environmental benefits, and has low requirements for flotation equipment, which can reduce the cost of production equipment and facilitate large-scale industrial application.
[0018] It is further configured that in the quartz flotation process, the reagents and usage amounts of the roughing step are as follows: sodium carbonate 1000-1500 g / t, adjusting the pulp pH to 6-7, and cationic collector 400-500 g / t.
[0019] It is further set that in the quartz flotation process, the time for roughing, scavenging and cleaning is 2-10 minutes respectively.
[0020] It is further configured that the cationic collector is at least one of dodecylamine, octadecylamine, mixed amines, and coconut amine. The collector added in the flotation process can separate the target product (such as mica, feldspar and quartz) from other minerals faster and more accurately, thereby improving the purity of the product.
[0021] The method for recovering mica, feldspar and quartz from molybdenum tailings provided by the present invention has the following advantages and beneficial effects:
[0022] 1) In the present invention, the molybdenum tailings are graded and deslimed by using cyclones in series, which can reduce the impurity content in the final product. The magnetic minerals are removed in advance by magnetic separation, which also ensures the purity and grade of the product. The subsequent steps of preferentially flotating mica, then flotating feldspar, and finally flotating quartz realize the comprehensive recovery of non-metallic minerals mica, feldspar, and quartz in the molybdenum tailings, which is also beneficial to reducing the dosage of reagents and improving the grade of each concentrate. In addition, the fluorine-free purification method of quartz is adopted, which reduces the probability of environmental pollution.
[0023] 2) The present invention determines reasonable recycling processes and steps based on the characteristics of molybdenum tailings, and finally obtains mica, feldspar and quartz products, which solves the technical shortcomings and deficiencies of previous recycling of specific minerals, accurately and efficiently recycles valuable non-metallic substances such as mica, feldspar and quartz in the tailings, and mica concentrate, feldspar concentrate and quartz concentrate are directly sold as final products. The ore mud, waste ore, magnetic minerals, etc. generated in the recycling process can be used to prepare building materials, achieving "zero" discharge of solid waste, avoiding waste of resources, and greatly improving the comprehensive utilization rate of resources.
[0024] 3) The process flow of the present invention is simple, the collector selectivity is good, the equipment used is conventional mineral processing equipment, the production equipment cost is low, and industrial production is easy to achieve; the water used in magnetic separation and flotation can be recycled, and the amount of reagents used can be appropriately reduced when the water used in flotation is recycled to avoid environmental pollution; the molybdenum tailings can be recycled and harmless to the greatest extent, and the tailings resources can be recovered and utilized to achieve economic, environmental and social benefits. The method of the present invention has strong applicability and a wide range of applicability, and can also be widely used in other tailings to recover mica, feldspar and quartz, such as tantalum tailings, tungsten tailings, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 A flow chart of a method for recovering mica, feldspar and quartz from molybdenum tailings provided in one embodiment of the present invention. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work also fall within the scope of protection of the present invention.
[0028] The following examples use conventional instruments and equipment in the art. Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources, and their specifications are conventional specifications in the art. If no specific techniques or conditions are specified in the following examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0029] It should be noted that, in the present invention and the following embodiments, concentrations, ratios, etc. not otherwise specified are all weight concentrations, weight ratios, etc., "%" means weight percentage, and "parts" means parts by weight, which are common writing habits used by those skilled in the art and are therefore not described in detail in the present invention.
[0030] As a further improvement of the above technical solution, in the roughing step of the feldspar flotation process, the reagent also includes 100-200g / t of triethanolamine oleate and 50-100g / t of semicarbazide hydrochloride. After the addition of triethanolamine oleate and semicarbazide hydrochloride, they are synergistically adsorbed on the mineral surface, and can use their hydrophilic groups to increase the hydrophilicity of ore particles in the slurry, promote the increase of their dispersion, thereby increasing the probability of contact with the collector, and use the anionic active particles on them to adsorb the cationic collector, so that the cationic collector can be more easily and firmly adsorbed on the surface of feldspar, making the hydrophobicity of feldspar better than quartz, increasing the efficiency and yield of feldspar flotation, and also being conducive to improving the grade of feldspar concentrate and quartz concentrate respectively.
[0031] In the embodiment of the present invention, the magnetic separation device is a magnetic separator; and the flotation uses a mechanical stirring flotation machine, but this is not a limitation of the present invention. In the implementation of the present invention, any device that can achieve the effect of magnetic separation or flotation can be used.
[0032] The present invention is further described in detail below in conjunction with the examples. However, it should be understood that the examples are for illustrative purposes only and are not intended to limit the scope of the present invention.
[0033] Embodiment 1:
[0034] A method for recovering mica, feldspar and quartz from molybdenum tailings comprises the following steps:
[0035] The tailings of a copper-molybdenum mine in Inner Mongolia Autonomous Region are used as raw materials, and the main components of the tailings are: mica content 16.55%, quartz content 42.25%, K2O content in feldspar 3.84%, and Na2O content 2.61%.
[0036] 1) Pre-classification: The molybdenum tailings slurry with a concentration of 25% is sent to the first-level cyclone, and the sludge in it overflows. The bottom flow of the first-level cyclone is sent to the second-level cyclone. After the cyclone classification of the second-level cyclone, the overflow slurry is reserved, and the bottom flow of the second-level cyclone is sent to the ball mill for grinding and repeatedly sent to the first-level cyclone. The sludge standard of the overflow of the first-level cyclone is -400 mesh content greater than or equal to 80%. The overflow slurry standard of the second-level cyclone is -200 mesh content of 60-70%.
[0037] 2) Magnetic separation: The overflow pulp obtained by pre-classification is sent to a magnetic separator for magnetic separation and iron removal. The field strength of the magnetic separator is 1T, and magnetic minerals and magnetic separation pulp are separated.
[0038] 3) Mica flotation: The magnetic slurry is fed into the mica flotation equipment, and a roughing selection is performed once to obtain mica roughing tailings and mica roughing concentrate. The mica roughing tailings are subjected to a scavenging selection once to obtain mica flotation tailings and mica scavenging slurry. The mica scavenging slurry is sent back to the roughing step. The mica roughing concentrate is first subjected to concentration I to obtain mica concentration I concentrate and mica concentration I tailings. The mica concentration I tailings are sent back to the roughing step. The mica concentration I concentrate is then subjected to concentration II to obtain mica concentrate and mica concentration II tailings. The mica concentration II tailings are sent back to the concentration I step. The mica flotation tailings are subjected to inclined plate concentration and dehydration to ensure that the subsequent feldspar flotation concentration is ≥30%. The inclined plate underflow after inclined plate concentration enters the feldspar flotation process.
[0039] The reagents and their usage in the roughing step are as follows: 600g / t of water glass, 4000g / t of sodium carbonate, and 80g / t of cationic collector. The cationic collector is a mixed amine. The reagents and their usage in the fine selection step I are as follows: 500g / t of sodium carbonate. The reagents and their usage in the fine selection step II are as follows: 100g / t of sodium carbonate. The time for roughing, scavenging and fine selection is 2-5min respectively.
[0040] 4) Feldspar flotation: The inclined plate bottom flow is sent to the feldspar flotation equipment. After adding the reagent, the feldspar flotation concentration is 32.5%. Then a roughing is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step. The feldspar flotation tailings enter the quartz flotation process.
[0041] The reagents and their usage in the roughing step are as follows: 800g / t oxalic acid, 400g / t sulfuric acid, 200g / t sodium dodecyl sulfonate. After adding acid, the pH of the pulp is adjusted to 2.4. The reagents and their usage in the concentrating step I are as follows: 200g / t oxalic acid. The reagents and their usage in the concentrating step II are as follows: 100g / t oxalic acid. The time for roughing, scavenging and concentrating is 2-5min respectively.
[0042] 5) Quartz flotation: The feldspar flotation tailings are sent to the quartz flotation equipment for a roughing process to obtain waste ore and quartz roughing concentrate. The quartz roughing concentrate is then finely concentrated to obtain quartz concentrate and quartz fine tailings. The fine quartz tailings are sent back to the roughing process.
[0043] The reagents and their usage in the roughing step are as follows: 1000g / t of sodium carbonate, adjusting the pulp pH to 6.5, 400g / t of cationic collector. The cationic collector is a mixed amine. The time for roughing, scavenging and cleaning is 2-10min respectively.
[0044] Finally, a mica concentrate with a grade of 98.8% and a recovery rate of 68.12% was obtained; a feldspar concentrate with a K2O content of 8.74%, a Na2O content of 5.18%, a K2O recovery rate of 56.10%, a Na2O recovery rate of 48.92%, and a total K2O+Na2O content of 13.92% was obtained; and a quartz concentrate with a grade of 99.6% and a recovery rate of 85.76% was obtained.
[0045] The yield, recovery rate and main component content of the raw ore and the final product concentrate are summarized in Table 1. The results are shown in the following table.
[0046] Table 1
[0047]
[0048] Embodiment 2:
[0049] A method for recovering mica, feldspar and quartz from molybdenum tailings comprises the following steps:
[0050] The tailings of a copper-molybdenum mine in Inner Mongolia Autonomous Region are used as raw materials, and the main components of the tailings are: mica content 18.34%, quartz content 42.16%, K2O content in feldspar 3.63%, and Na2O content 2.94%.
[0051] 1) Pre-classification: The molybdenum tailings slurry with a concentration of 35% is sent to the first-level cyclone, and the sludge in it overflows. The bottom flow of the first-level cyclone is sent to the second-level cyclone. After the cyclone classification of the second-level cyclone, the overflow slurry is reserved, and the bottom flow of the second-level cyclone is sent to the ball mill for grinding and repeatedly sent to the first-level cyclone. The sludge standard of the overflow of the first-level cyclone is -400 mesh content greater than or equal to 80%. The overflow slurry standard of the second-level cyclone is -200 mesh content of 60-70%.
[0052] 2) Magnetic separation: The overflow pulp obtained by pre-classification is sent to a magnetic separator for magnetic separation and iron removal. The field strength of the magnetic separator is 1.1T, and magnetic minerals and magnetic separation pulp are separated.
[0053] 3) Mica flotation: The magnetic slurry is fed into the mica flotation equipment, and a roughing selection is performed once to obtain mica roughing tailings and mica roughing concentrate. The mica roughing tailings are subjected to a scavenging selection once to obtain mica flotation tailings and mica scavenging slurry. The mica scavenging slurry is sent back to the roughing step. The mica roughing concentrate is first subjected to concentration I to obtain mica concentration I concentrate and mica concentration I tailings. The mica concentration I tailings are sent back to the roughing step. The mica concentration I concentrate is then subjected to concentration II to obtain mica concentrate and mica concentration II tailings. The mica concentration II tailings are sent back to the concentration I step. The mica flotation tailings are subjected to inclined plate concentration and dehydration to ensure that the subsequent feldspar flotation concentration is ≥30%. The inclined plate underflow after inclined plate concentration enters the feldspar flotation process.
[0054] The reagents and their usage in the roughing step are as follows: 800g / t of water glass, 5000g / t of sodium carbonate, and 100g / t of cationic collector. The cationic collector is octadecylamine. The reagents and their usage in the fine selection step I are as follows: 800g / t of sodium carbonate. The reagents and their usage in the fine selection step II are as follows: 200g / t of sodium carbonate. The time for roughing, scavenging and fine selection is 2-5min respectively.
[0055] 4) Feldspar flotation: The inclined plate bottom flow is sent to the feldspar flotation equipment. After adding the reagent, the feldspar flotation concentration is 33.7%. Then a roughing is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step. The feldspar flotation tailings enter the quartz flotation process.
[0056] The reagents and their usage in the roughing step are as follows: 1000g / t oxalic acid, 600g / t sulfuric acid, 500g / t sodium dodecyl sulfonate. After adding acid, the pH of the pulp is adjusted to 2.7. The reagents and their usage in the concentrating step I are as follows: 400g / t oxalic acid. The reagents and their usage in the concentrating step II are as follows: 200g / t oxalic acid. The time for roughing, scavenging and concentrating is 2-5min respectively.
[0057] 5) Quartz flotation: The feldspar flotation tailings are sent to the quartz flotation equipment for a roughing process to obtain waste ore and quartz roughing concentrate. The quartz roughing concentrate is then finely concentrated to obtain quartz concentrate and quartz fine tailings. The fine quartz tailings are sent back to the roughing process.
[0058] The reagents and their usage in the roughing step are as follows: 1500g / t of sodium carbonate, adjusting the pulp pH to 6.7, 500g / t of cationic collector. The cationic collector is octadecylamine. The time for roughing, scavenging and cleaning is 2-10min respectively.
[0059] Finally, a mica concentrate with a grade of 98.9% and a recovery rate of 66.71% was obtained; a feldspar concentrate with a K2O content of 8.53%, a Na2O content of 5.42%, a K2O recovery rate of 59.55%, a Na2O recovery rate of 46.72%, and a total K2O+Na2O content of 13.95% was obtained; and a quartz concentrate with a grade of 99.7% and a recovery rate of 89.06% was obtained.
[0060] The yield, recovery rate and main component content of the raw ore and the final product concentrates are summarized in Table 2. The results are shown in the following table.
[0061] Table 2
[0062]
[0063]
[0064] Embodiment 3:
[0065] A method for recovering mica, feldspar and quartz from molybdenum tailings, such as Figure 1 As shown, the following steps are included:
[0066] Tailings from a copper-molybdenum mine in Inner Mongolia Autonomous Region, the main components of the tailings are: mica content 17.13%, quartz content 43.16%, K2O content in feldspar 3.71%, Na2O content 2.88%.
[0067] 1) Pre-classification: The molybdenum tailings slurry with a concentration of 30% is sent to the first-level cyclone, and the sludge in it overflows. The bottom flow of the first-level cyclone is sent to the second-level cyclone. After the cyclone classification of the second-level cyclone, the overflow slurry is reserved, and the bottom flow of the second-level cyclone is sent to the ball mill for grinding and repeatedly sent to the first-level cyclone. The sludge standard of the overflow of the first-level cyclone is -400 mesh content greater than or equal to 80%. The overflow slurry standard of the second-level cyclone is -200 mesh content of 60-70%.
[0068] 2) Magnetic separation: The overflow pulp obtained by pre-classification is sent to a magnetic separator for magnetic separation and iron removal. The field strength of the magnetic separator is 1.2T, and magnetic minerals and magnetic separation pulp are separated.
[0069] 3) Mica flotation: The magnetic slurry is fed into the mica flotation equipment, and a roughing selection is performed once to obtain mica roughing tailings and mica roughing concentrate. The mica roughing tailings are subjected to a scavenging selection once to obtain mica flotation tailings and mica scavenging slurry. The mica scavenging slurry is sent back to the roughing step. The mica roughing concentrate is first subjected to concentration I to obtain mica concentration I concentrate and mica concentration I tailings. The mica concentration I tailings are sent back to the roughing step. The mica concentration I concentrate is then subjected to concentration II to obtain mica concentrate and mica concentration II tailings. The mica concentration II tailings are sent back to the concentration I step. The mica flotation tailings are subjected to inclined plate concentration and dehydration to ensure that the subsequent feldspar flotation concentration is ≥30%. The inclined plate underflow after inclined plate concentration enters the feldspar flotation process.
[0070] The reagents and their usage in the roughing step are as follows: 680g / t of water glass, 4400g / t of sodium carbonate, and 90g / t of cationic collector. The cationic collector is dodecylamine. The reagents and their usage in the fine selection step I are as follows: 580g / t of sodium carbonate. The reagents and their usage in the fine selection step II are as follows: 120g / t of sodium carbonate. The time for roughing, scavenging and fine selection is 2-5min respectively.
[0071] 4) Feldspar flotation: The inclined plate bottom flow is sent to the feldspar flotation equipment. After adding the reagent, the feldspar flotation concentration is 31.4%. Then a roughing is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step. The feldspar flotation tailings enter the quartz flotation process.
[0072] The reagents and their usage in the roughing step are as follows: 860g / t oxalic acid, 410g / t sulfuric acid, 200g / t sodium dodecyl sulfonate, and the pH of the pulp is adjusted to 2.2 after adding acid. The reagents and their usage in the concentrating step I are as follows: 210g / t oxalic acid. The reagents and their usage in the concentrating step II are as follows: 120g / t oxalic acid. The time for roughing, scavenging and concentrating is 2-5min respectively.
[0073] 5) Quartz flotation: The feldspar flotation tailings are sent to the quartz flotation equipment for a roughing process to obtain waste ore and quartz roughing concentrate. The quartz roughing concentrate is then finely concentrated to obtain quartz concentrate and quartz fine tailings. The fine quartz tailings are sent back to the roughing process.
[0074] The reagents and their usage in the roughing step are as follows: 1100g / t of sodium carbonate, adjusting the pulp pH to 6.8, 410g / t of cationic collector. The cationic collector is dodecylamine. The time for roughing, scavenging and cleaning is 2-10min respectively.
[0075] Finally, a mica concentrate with a grade of 98.91% and a recovery rate of 68.42% was obtained; a feldspar concentrate with a K2O content of 8.63%, a Na2O content of 5.51%, a K2O recovery rate of 55.62%, a Na2O recovery rate of 45.74%, and a total K2O+Na2O content of 14.14% was obtained; and a quartz concentrate with a grade of 99.85% and a recovery rate of 83.19% was obtained.
[0076] The yield, recovery rate and main component content of the raw ore and the final product concentrates are summarized in Table 3. The results are shown in the following table.
[0077] Table 3
[0078]
[0079] Embodiment 4:
[0080] A method for recovering mica, feldspar and quartz from molybdenum tailings, based on Example 3, differs only in the following steps:
[0081] 4) Feldspar flotation: The inclined plate bottom flow is sent to the feldspar flotation equipment. After adding the reagent, the feldspar flotation concentration is 31.4%. Then a roughing is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step. The feldspar flotation tailings enter the quartz flotation process.
[0082] The reagents and their usage in the roughing step are as follows: 860g / t oxalic acid, 410g / t sulfuric acid, 200g / t sodium dodecyl sulfonate, 130g / t triethanolamine oleate, 75g / t semicarbazide hydrochloride, and the pH of the pulp is adjusted to 2.2 after adding acid. The reagents and their usage in the concentrating step I are as follows: 210g / t oxalic acid. The reagents and their usage in the concentrating step II are as follows: 120g / t oxalic acid. The time for roughing, scavenging and concentrating is 2-5min respectively.
[0083] Finally, a mica concentrate with a grade of 98.9% and a recovery rate of 68.36% was obtained; a feldspar concentrate with a K2O content of 8.72%, a Na2O content of 5.63%, a K2O recovery rate of 56.67%, a Na2O recovery rate of 47.13%, and a total K2O+Na2O content of 14.35% was obtained; and a quartz concentrate with a grade of 99.91% and a recovery rate of 82.94% was obtained.
[0084] The yield, recovery rate and main component content of the raw ore and the final product concentrates are summarized in Table 4. The results are shown in the following table.
[0085] Table 4
[0086]
[0087] Comparing Example 3 with Example 4, it is found that although the yield of the quartz concentrate in Example 4 is reduced, the grade is higher, the K2O and Na2O contents in the feldspar concentrate are increased, and the yield and recovery rate are also significantly increased, indicating that the reagents triethanolamine oleate and semicarbazide hydrochloride added in the feldspar flotation process in Example 4 can play a synergistic role, so that the cationic collector can be more easily and firmly adsorbed on the surface of the feldspar, making the hydrophobicity of the feldspar better than that of quartz, so that the feldspar and quartz that are difficult to separate can be separated more thoroughly, thereby improving the grades of the feldspar concentrate and the quartz concentrate, respectively.
[0088] Comparative Example 1:
[0089] A method for recovering mica, feldspar and quartz from molybdenum tailings, based on Example 3, differs only in the following steps:
[0090] 1) Pre-classification: The molybdenum tailings slurry with a concentration of 30% is sent to the first-level cyclone, and the sludge in it overflows. The bottom flow of the first-level cyclone is directly sent to the magnetic separation process. The standard of the sludge overflowing from the first-level cyclone is -400 mesh content greater than or equal to 80%. That is, in the pre-classification process, only the sludge is separated out, and the larger ore particles are not ground.
[0091] Finally, a mica concentrate with a grade of 98.36% and a recovery rate of 66.20% was obtained; a feldspar concentrate with a K2O content of 6.71%, a Na2O content of 3.61%, a K2O recovery rate of 40.55%, a Na2O recovery rate of 28.10%, and a total K2O+Na2O content of 10.32% was obtained; and a quartz concentrate with a grade of 98.64% and a recovery rate of 76.01% was obtained.
[0092] The yield, recovery rate and main component content of the raw ore and each final product concentrate are summarized in Table 5. The results are shown in the following table.
[0093] Table 5
[0094]
[0095] By comparing the results of Example 3 and Comparative Example 1, it can be seen that only desludging is performed in the pre-classification process without performing secondary classification and grinding treatment on large-particle ore particles, which will seriously affect the grade of each product concentrate and its yield and recovery rate. The separation of mica, feldspar and quartz in large-particle ore is difficult, and they cannot be completely captured and separated in the subsequent flotation stages, thereby affecting the production operation results.
[0096] Comparative Example 2:
[0097] A method for recovering mica, feldspar and quartz from molybdenum tailings, based on Example 3, differs only in the following steps:
[0098] 4) Feldspar flotation: The inclined plate bottom flow is sent to the feldspar flotation equipment. After adding the reagent, the feldspar flotation concentration is 31.4%. Then a roughing is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step. The feldspar flotation tailings enter the quartz flotation process.
[0099] The reagents and their usage in the roughing step are as follows: 860g / t oxalic acid, 410g / t sulfuric acid, 200g / t sodium dodecyl sulfonate, 205g / t triethanolamine oleate. After adding acid, the pH of the pulp is adjusted to 2.2. The reagents and their usage in the concentrating step I are as follows: 210g / t oxalic acid. The reagents and their usage in the concentrating step II are as follows: 120g / t oxalic acid. The time for roughing, scavenging and concentrating is 2-5min respectively.
[0100] Finally, a mica concentrate with a grade of 98.93% and a recovery rate of 68.49% was obtained; a feldspar concentrate with a K2O content of 8.64%, a Na2O content of 5.53%, a K2O recovery rate of 55.73%, a Na2O recovery rate of 45.95%, and a total K2O+Na2O content of 14.17% was obtained; and a quartz concentrate with a grade of 99.83% and a recovery rate of 83.11% was obtained.
[0101] The yield, recovery rate and main component content of the raw ore and the final product concentrates are summarized in Table 6. The results are shown in the following table.
[0102] Table 6
[0103]
[0104] Comparative Example 3:
[0105] A method for recovering mica, feldspar and quartz from molybdenum tailings, based on Example 3, differs only in the following steps:
[0106] 4) Feldspar flotation: The inclined plate bottom flow is sent to the feldspar flotation equipment. After adding the reagent, the feldspar flotation concentration is 31.4%. Then a roughing is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step. The feldspar flotation tailings enter the quartz flotation process.
[0107] The reagents and their usage in the roughing step are as follows: 860g / t oxalic acid, 410g / t sulfuric acid, 200g / t sodium dodecyl sulfonate, 205g / t hydrochloric acid semicarbazide, and the pH of the pulp is adjusted to 2.2 after adding acid. The reagents and their usage in the concentrating step I are as follows: 210g / t oxalic acid. The reagents and their usage in the concentrating step II are as follows: 120g / t oxalic acid. The time for roughing, scavenging and concentrating is 2-5min respectively.
[0108] Finally, a mica concentrate with a grade of 98.91% and a recovery rate of 68.42% was obtained; a feldspar concentrate with a K2O content of 8.72%, a Na2O content of 5.63%, a K2O recovery rate of 56.67%, a Na2O recovery rate of 47.13%, and a total K2O+Na2O content of 14.23% was obtained; and a quartz concentrate with a grade of 99.91% and a recovery rate of 82.94% was obtained.
[0109] The yield, recovery rate and main component content of the raw ore and each final product concentrate are summarized in Table 7. The results are shown in the following table.
[0110] Table 7
[0111]
[0112] By comparing Comparative Example 1, Comparative Example 2, Example 3 and Example 4, it is found that when an equal amount of additional reagents is added, the difference between Comparative Example 3 and Example 1 is not significant, and the grade of the feldspar concentrate and the quartz concentrate in Comparative Example 2 is slightly improved, but not as significant as the improvement effect of the combination of the two in Example 4, indicating that under the condition of equal amounts, the combination of triethanolamine oleate and semicarbazide hydrochloride in Example 4 has the best effect and can save the most reagent use cost.
[0113] It should be noted that in the present invention, the detailed steps of some operations are not described in detail, but belong to the prior art known to those skilled in the art, so they will not be repeated here. In addition, in the present invention, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for simplicity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible secondary ranges and individual values (including integers and fractions) within the range.
[0114] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. In the present invention, not all possible combinations of the various technical features in the various embodiments or embodiments are described. As long as there is no contradiction in the combination of these technical features, the various technical features in the various embodiments or embodiments can be arbitrarily combined, and all possible combinations should be considered to be within the scope of this specification. Although the present invention has been described in detail with reference to the aforementioned embodiments, a person of ordinary skill in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some or all of the technical features therein can be replaced by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for recovering mica, feldspar and quartz from molybdenum tailings, characterized in that: include: The molybdenum tailings are treated as the object, and a pre-classification process is performed by using a hydrocyclone to perform classification treatment to obtain overflow slurry; a magnetic separation process is performed on the overflow slurry to remove iron by magnetic separation to obtain magnetic separation slurry; a mica flotation process is performed on the magnetic separation slurry to obtain mica concentrate and mica flotation tailings; a feldspar flotation process is performed on the mica flotation tailings to obtain feldspar concentrate and feldspar flotation tailings; and a quartz flotation process is performed on the feldspar flotation tailings to obtain quartz concentrate; In the pre-classification process, two-stage cyclones connected in series are used for classification treatment; In the magnetic separation process, the field strength of the magnetic separator is 1-1.2T; In the mica concentrate, the content of mica is ≥98.5%; in the feldspar concentrate, the total content of K2O+Na2O is ≥11.5%; in the quartz concentrate, the content of SiO2 is ≥99.5%.
2. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 1, characterized in that: The operation process of the pre-grading process is as follows: The molybdenum tailings slurry with a concentration of 25-35% is sent to the first-level cyclone, and the sludge in it overflows. The bottom flow of the first-level cyclone is sent to the second-level cyclone. After cyclone classification in the second-level cyclone, the overflow slurry is reserved for use. The bottom flow of the second-level cyclone is sent to the ball mill for grinding treatment and repeatedly sent to the first-level cyclone.
3. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 2, characterized in that: The standard of the overflow sludge of the first-stage cyclone is -400 mesh content greater than or equal to 80%; the standard of the overflow slurry of the second-stage cyclone is -200 mesh content of 60-70%.
4. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 1, characterized in that: The operation process of the mica flotation process is as follows: The magnetic separation slurry is sent to the mica flotation equipment for a roughing selection to obtain mica roughing tailings and mica roughing concentrate. The mica roughing tailings are subjected to a scavenging selection to obtain mica flotation tailings and mica scavenging slurry. The mica scavenging slurry is sent back to the roughing step. The mica roughing concentrate is first subjected to concentration I to obtain mica concentration I concentrate and mica concentration I tailings. The mica concentration I tailings are sent back to the roughing step. The mica concentration I concentrate is then subjected to concentration II to obtain mica concentrate and mica concentration II tailings. The mica concentration II tailings are sent back to the concentration I step. The mica flotation tailings are subjected to inclined plate concentration and dehydration. The inclined plate underflow after inclined plate concentration enters the feldspar flotation process.
5. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 4, characterized in that: In the mica flotation process, the reagents and their usage amounts in the roughing step are as follows: 600-800 g / t of water glass, 4000-5000 g / t of sodium carbonate, and 80-100 g / t of cationic collector; the reagents and their usage amounts in the fine selection step I are as follows: 500-800 g / t of sodium carbonate; and the reagents and their usage amounts in the fine selection step II are as follows: 100-200 g / t of sodium carbonate.
6. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 1, characterized in that: The operation process of the feldspar flotation process is as follows: The inclined plate bottom flow is sent to the feldspar flotation equipment, and a roughing selection is carried out to obtain feldspar roughing tailings and feldspar roughing concentrate. The feldspar roughing tailings are subjected to a scavenging selection to obtain feldspar flotation tailings and feldspar scavenging slurry. The feldspar scavenging slurry is sent back to the roughing step. The feldspar roughing concentrate is first subjected to concentration I to obtain feldspar concentration I concentrate and feldspar concentration I tailings. The feldspar concentration I tailings are sent back to the roughing step. The feldspar concentration I concentrate is then subjected to concentration II to obtain feldspar concentrate and feldspar concentration II tailings. The feldspar concentration II tailings are sent back to the concentration I step, and the feldspar flotation tailings enter the quartz flotation process.
7. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 6, characterized in that: In the feldspar flotation process, the reagents and their usage amounts in the roughing step are as follows: 800-1000 g / t of oxalic acid, 400-600 g / t of sulfuric acid, 200-500 g / t of sodium dodecyl sulfonate, and the pH of the pulp is adjusted to 2-3 after acid addition; the reagents and their usage amounts in the selection step I are as follows: 200-400 g / t of oxalic acid; the reagents and their usage amounts in the selection step II are as follows: 100-200 g / t of oxalic acid.
8. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 1, characterized in that: The operation process of the quartz flotation process is as follows: The feldspar flotation tailings are sent to the quartz flotation equipment for a roughing process to obtain waste ore and quartz roughing concentrate. The quartz roughing concentrate is then finely concentrated to obtain quartz concentrate and quartz fine tailings. The fine quartz tailings are sent back to the roughing process.
9. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 8, characterized in that: In the quartz flotation process, the reagents and their usage amounts in the roughing step are as follows: 1000-1500 g / t of sodium carbonate, adjusting the pH of the ore pulp to 6-7, and 400-500 g / t of a cationic collector.
10. The method for recovering mica, feldspar and quartz from molybdenum tailings according to claim 5 or 9, characterized in that: The cationic collector is at least one of dodecylamine, octadecylamine, mixed amines and coconut amine.