Coal slime flotation collecting agent and preparation method and application thereof
The surface properties of the coal slime flotation collector are improved by combining biodiesel, isolong loam ethyl ether, methyl isobutyl methanol and fatty alcohol polyoxyethylene ether, and the large amount of traditional collectors used and volatile The problem of emission of organic compounds has achieved efficient and environmentally friendly coal slime flotation effect.
Patent Information
- Application Number
- CN202411246876.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-01
AI Technical Summary
Traditional coal slime flotation collectors are used in large quantities, accompanied by high drug consumption costs, and release pungent odors and volatile organic compounds during operation, affecting the environment and operator health, and the flotation effect is poor.
The combination of biodiesel, isolong luol ethyl ether, methyl isobutyl methanol and fatty alcohol polyoxyethylene ether is used to improve the surface properties of coal particles and gangue particles through synergistic effects and improve the flotation efficiency and quality.
It significantly reduces the consumption of agents, reduces the emission of volatile organic compounds, improves the recovery rate and flotation efficiency of refined coal, concentrate yield ≥69.11%, and ash content <11%, improving the flotation operation environment.
Smart Images

Figure BDA0005031034630000021 
Figure BDA0005031034630000041 
Figure BDA0005031034630000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coal flotation, and in particular to a coal slime flotation collector and a preparation method and application thereof. Background Art
[0002] At present, hydrocarbon oils such as diesel or kerosene are traditionally widely used as collectors in coal slime flotation operations.
[0003] CN105964410A discloses a method for preparing a coal slime flotation collector, the preparation method comprising mixing diesel and kerosene with clean coal particles from the same origin to be floated by the coal slime flotation collector, allowing effective components in the raw materials to be adsorbed on the surface of the clean coal particles, and then desorbing the effective components adsorbed on the surface of the clean coal, thereby obtaining a flotation collector suitable for flotation of coal slime from a specific origin.
[0004] CN103143449A A method for flotation of coal slime using oxidized kerosene. The flotation of coal slime using oxidized kerosene is carried out in a flotation tank. The kerosene is first catalytically oxidized with potassium permanganate and sulfuric acid to form oxidized kerosene. The oxidized kerosene is then added into the flotation tank together with 2-octanol as a foaming agent, stirred and aerated at room temperature, and then flotation is performed to obtain clean coal. The clean coal is then filtered and dried to obtain clean coal.
[0005] However, with the increasing awareness of resource conservation and environmental protection, the application bottlenecks of these traditional collectors have gradually emerged. First of all, the large amount of collectors such as diesel and kerosene used, accompanied by high drug consumption costs, directly restricts the cost-effectiveness and sustainable development potential of coal processing enterprises. More seriously, the pungent odor and volatile organic compounds released by these hydrocarbon collectors during operation not only seriously affect the air quality of the working environment, but also pose a risk to the health of front-line operators that cannot be ignored, and also aggravate the problem of environmental pollution. At the same time, there is also the defect of poor flotation effect.
[0006] In view of this, targeting coal slime, an important resource, developing an efficient and environmentally friendly flotation collector to achieve efficient flotation recovery of coal slime resources has become a difficult problem to be solved urgently in the field of coal flotation technology. Summary of the invention
[0007] In view of the problems existing in the prior art, the purpose of the present invention is to provide a coal slime flotation collector and its preparation method and use, so as to solve the problems of large usage of collectors used in coal flotation, release of volatile organic compounds during use and poor collection effect.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a coal slime flotation collector, the coal slime flotation collector comprising:
[0010] Biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether.
[0011] The coal slime flotation collector provided by the invention improves the surface properties of coal particles and gangue particles and improves the efficiency and quality of coal slime flotation through the synergistic effect of the combined agent of biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether.
[0012] Specifically, biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether are used in a coordinated manner. Each component acts together on the surface of coal particles and gangue particles to change their surface properties, making the surface of the coal particles more hydrophobic while the surface of the gangue particles remains hydrophilic. The coal particles can be separated from the coal slurry more effectively, thereby improving the recovery rate and flotation efficiency of the clean coal.
[0013] As a preferred technical solution of the present invention, the coal slime flotation collector comprises, by weight:
[0014]
[0015] As a preferred technical solution of the present invention, the carbon chain R of the fatty alcohol polyoxyethylene ether is C7-C9.
[0016] As a preferred technical solution of the present invention, the polymerization degree of the fatty alcohol polyoxyethylene ether is 5-8.
[0017] In a second aspect, the present invention provides a method for preparing the coal slime flotation collector as described in the first aspect, the preparation method comprising:
[0018] According to the weight ratio, biodiesel, isophylline ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether are mixed to obtain the coal slime flotation collector.
[0019] As a preferred technical solution of the present invention, stirring is performed for 30-60 minutes during the mixing.
[0020] In a third aspect, the present invention provides a use of the coal slime flotation collector as described in the first aspect, the use comprising:
[0021] The coal slime flotation collector is used to float the coal slime.
[0022] As a preferred technical solution of the present invention, the flotation comprises:
[0023] A frother and the coal slime flotation collector are added to the coal slime slurry for flotation.
[0024] As a preferred technical solution of the present invention, the concentration of the coal slime slurry is 60-100 g / L.
[0025] As a preferred technical solution of the present invention, the addition amount of the coal slime flotation collector in the flotation is 100-800g / t.
[0026] Preferably, the amount of frother added in the flotation is 40-400 g / t.
[0027] Preferably, the frother used in the flotation comprises secondary octanol and / or octanol.
[0028] Compared with the prior art solutions, the present invention has the following beneficial effects:
[0029] The collector provided by the invention has high selectivity for coal slime and strong collecting ability through the synergistic effect of biodiesel, isostearyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether. The concentrate yield is ≥69.11% and the ash content is <11%. The disadvantages of traditional diesel, kerosene and the like in the process of coal slime recovery, such as large reagent consumption, strong odor and high emission of volatile organic compounds, are overcome, and the flotation operation environment is significantly improved. DETAILED DESCRIPTION
[0030] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:
[0031] The present embodiment provides a coal slime flotation collector, which includes: biodiesel, isophylline ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether.
[0032] Specifically, the coal slime flotation collector comprises, by weight:
[0033]
[0034] In the present invention, the biodiesel in the coal slime flotation collector is 50-70 parts by weight, for example, it can be 50 parts, 51 parts, 52 parts, 53 parts, 54 parts, 55 parts, 56 parts, 57 parts, 58 parts, 59 parts, 60 parts, 61 parts, 62 parts, 63 parts, 64 parts, 65 parts, 66 parts, 67 parts, 68 parts, 69 parts or 70 parts, but is not limited to the listed values, and other values not listed within this range also meet the requirements.
[0035] In the present invention, if the weight proportion of the biodiesel is less than 50 parts, the capture capacity becomes weak and the clean coal yield is reduced; if it is greater than 70 parts, it is not conducive to the recovery of coal slime.
[0036] In the present invention, the weight percentage of isophylline ethyl ether in the coal slime flotation collector is 20-40 parts, for example, it can be 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, 26 parts, 27 parts, 28 parts, 29 parts, 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, 36 parts, 37 parts, 38 parts, 39 parts or 40 parts, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0037] In the present invention, when the weight proportion of isophylline ethyl ether is less than 20 parts, the collecting ability of the collector becomes weak; when it is greater than 40 parts, the foam viscosity becomes larger, which will lead to an increase in ash content in the clean coal.
[0038] In the present invention, the methyl isobutyl carbinol in the coal slime flotation collector is 5-10 parts by weight, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts or 10 parts, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0039] In the present invention, when the methyl isobutyl carbinol content is less than 5 parts, the foaming ability becomes weak, the collecting ability decreases, and the clean coal yield is low; when the methyl isobutyl carbinol content is greater than 10 parts, the foam viscosity becomes larger, which will lead to an increase in the ash content in the clean coal.
[0040] In the present invention, the fatty alcohol polyoxyethylene ether in the coal slime flotation collector is 1-5 parts by weight, for example, it can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 3.5 parts, 4 parts, 4.5 parts or 5 parts, but is not limited to the listed values, and other unlisted values within this range also meet the requirements.
[0041] In the present invention, when the weight proportion of the fatty alcohol polyoxyethylene ether is less than 1 part, the solubility, fluidity and dispersibility of the collector deteriorate; when it is greater than 5 parts, a large amount of flotation foam is caused, and the flotation process is difficult to control.
[0042] Specifically, the carbon chain R of the fatty alcohol polyoxyethylene ether is C7-C9.
[0043] In the present invention, the carbon chain R may be a straight chain hydrocarbon group or a branched hydrocarbon group.
[0044] Specifically, the polymerization degree of the fatty alcohol polyoxyethylene ether is 5-8, for example, 5, 6, 7 or 8, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0045] Furthermore, this embodiment provides a method for preparing the above-mentioned coal slime flotation collector, the preparation method comprising:
[0046] According to the weight ratio, biodiesel, isophylline ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether are mixed to obtain the collector.
[0047] Specifically, the mixing is stirred for 30-60 min, for example, 30 min, 32 min, 34 min, 36 min, 38 min, 40 min, 42 min, 44 min, 46 min, 48 min, 50 min, 52 min, 54 min, 56 min, 58 min, 60 min, etc., but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0048] Furthermore, this embodiment provides a use of the above-mentioned coal slime flotation collector, and the use includes: using the above-mentioned coal slime flotation collector to float coal slime.
[0049] Specifically, the flotation comprises: adding a frother and the coal slime flotation collector into the coal slime slurry to perform flotation.
[0050] Specifically, the concentration of the coal slime slurry is 60-100g / L, for example, it can be 60g / L, 62g / L, 64g / L, 66g / L, 68g / L, 70g / L, 72g / L, 74g / L, 76g / L, 78g / L, 80g / L, 82g / L, 84g / L, 86g / L, 88g / L, 90g / L, 92g / L, 94g / L, 96g / L, 98g / L or 100g / L, but is not limited to the listed values, and other values not listed within the range also meet the requirements.
[0051] Specifically, the addition amount of the coal slime flotation collector in the flotation is 100-800 g / t, for example, it can be 100 g / t, 200 g / t, 300 g / t, 400 g / t, 500 g / t, 600 g / t, 700 g / t or 800 g / t, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0052] Specifically, the addition amount of the frother in the flotation is 40-400 g / t, for example, it can be 40 g / t, 60 g / t, 80 g / t, 100 g / t, 150 g / t, 200 g / t, 250 g / t, 300 g / t, 350 g / t or 400 g / t, but is not limited to the listed values, and other unlisted values within the range also meet the requirements.
[0053] Specifically, the frother used in the flotation includes secondary octanol and / or octanol, for example, it can be, but not limited to the listed values, and other values not listed within the range also meet the requirements.
[0054] In the present invention, the unit of addition amount "g / t" means that a certain amount of reagent is added per t of raw ore.
[0055] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0056] Further, in order to illustrate that the present invention provides a coal slime flotation collector that can achieve a good flotation effect when flotating coal slime, the following actual example is used for illustration, as follows:
[0057] Example 1
[0058] The present invention provides a coal slime flotation collector, the coal slime flotation collector comprising:
[0059] 60 parts of biodiesel, 30 parts of isopropyl alcohol ethyl ether, 8 parts of methyl isobutyl carbinol and 3 parts of fatty alcohol polyoxyethylene ether (JFC-2).
[0060] The specific preparation process is as follows:
[0061] The ingredients were formulated in parts by weight, biodiesel, isophylline ethyl ether and methyl isobutyl carbinol were mixed at room temperature of 25° C., fatty alcohol polyoxyethylene ether was added, and the mixture was stirred for 45 minutes to obtain a coal slime flotation collector.
[0062] Example 2
[0063] The present invention provides a coal slime flotation collector, the coal slime flotation collector comprising:
[0064] 65 parts of biodiesel, 28 parts of isopropyl alcohol ethyl ether, 7 parts of methyl isobutyl carbinol and 2 parts of fatty alcohol polyoxyethylene ether (JFC-2).
[0065] The specific preparation process is as follows:
[0066] The ingredients were formulated in parts by weight, biodiesel, isophylline ethyl ether and methyl isobutyl carbinol were mixed at room temperature of 25° C., fatty alcohol polyoxyethylene ether was added, and the mixture was stirred for 30 minutes to obtain a coal slime flotation collector.
[0067] Example 3
[0068] The present invention provides a coal slime flotation collector, the coal slime flotation collector comprising:
[0069] 55 parts of biodiesel, 35 parts of isopropyl alcohol ethyl ether, 9 parts of methyl isobutyl carbinol and 1 part of fatty alcohol polyoxyethylene ether (JFC-2).
[0070] The specific preparation process is as follows:
[0071] The ingredients were formulated in parts by weight, biodiesel, isophylline ethyl ether and methyl isobutyl carbinol were mixed at room temperature of 25° C., fatty alcohol polyoxyethylene ether was added, and the mixture was stirred for 55 minutes to obtain a coal slime flotation collector.
[0072] Example 4
[0073] The present invention provides a coal slime flotation collector, the coal slime flotation collector comprising:
[0074] 70 parts of biodiesel, 25 parts of isothiocyanate ethyl ether, 7 parts of methyl isobutyl carbinol and 2 parts of fatty alcohol polyoxyethylene ether (JFC-2).
[0075] The specific preparation process is as follows:
[0076] The ingredients were formulated in parts by weight, biodiesel, isophylline ethyl ether and methyl isobutyl carbinol were mixed at room temperature of 25° C., fatty alcohol polyoxyethylene ether was added, and the mixture was stirred for 40 minutes to obtain a coal slime flotation collector.
[0077] Example 5
[0078] The only difference from Example 1 is that the weight proportion of biodiesel in the coal slime flotation collector is 80 parts.
[0079] Example 6
[0080] The only difference from Example 1 is that the weight portion of isophylline ethyl ether in the coal slime flotation collector is 60 parts.
[0081] Example 7
[0082] The only difference from Example 1 is that the weight proportion of methyl isobutyl carbinol in the coal slime flotation collector is 20 parts.
[0083] Example 8
[0084] The only difference from Example 1 is that the weight proportion of fatty alcohol polyoxyethylene ether in the coal slime flotation collector is 15 parts.
[0085] Comparative Example 1
[0086] The only difference from Example 1 is that isophylline ethyl ether is not added to the coal slime flotation collector.
[0087] Comparative Example 2
[0088] The only difference from Example 1 is that methyl isobutyl carbinol is not added to the coal slime flotation collector.
[0089] Comparative Example 3
[0090] The only difference from Example 1 is that fatty alcohol polyoxyethylene ether is not added to the coal slime flotation collector.
[0091] Comparative Example 4
[0092] The only difference from Example 1 is that the biodiesel in the coal slime flotation collector is replaced with an equal amount of diesel.
[0093] Comparative Example 5
[0094] The only difference from Example 1 is that the isophylline ethyl ether in the coal slime flotation collector is replaced by an equal amount of kerosene.
[0095] Comparative Example 6
[0096] The only difference from Example 1 is that the fatty alcohol polyoxyethylene ether in the coal slime flotation collector is replaced by an equal amount of alkylphenol polyoxyethylene ether (NP-10).
[0097] Comparative Example 7
[0098] The only difference from Example 1 is that the methyl isobutyl carbinol in the coal slime flotation collector is replaced by an equal amount of 2# oil.
[0099] Comparative Example 8
[0100] The only difference from Example 1 is that the biodiesel in the coal slime flotation collector is replaced by an equal amount of kerosene.
[0101] Comparative Example 9
[0102] The only difference from Example 1 is that the methyl isobutyl carbinol in the coal slime flotation collector is replaced by an equal amount of sec-octanol.
[0103] Comparative Example 10
[0104] This comparative example provides a collector, which is diesel.
[0105] Comparative Example 11
[0106] This comparative example provides a collector, which is kerosene.
[0107] The coal slime flotation collectors provided in the above examples and comparative examples were used to test the flotation performance of coal slime, as follows:
[0108] Coal slime (-0.30 mm particle size material, ash content 25.7%) was added with water to form a flotation pulp with a concentration of 80 g / L, and a frother (octanol, added in an amount of 80 g / t) and the collector of the aforementioned embodiment and comparative example (added in an amount of 400 g / t) were added to carry out a flotation treatment. The specific test results are shown in Table 1.
[0109] Table 1
[0110]
[0111]
[0112] Furthermore, the coal slime (-0.30 mm particle size material, ash content 15%) was added with water to form a flotation pulp with a concentration of 80 g / L, and a frother (octanol, added in an amount of 80 g / t) and the collector of the aforementioned embodiment and comparative example (added in an amount of 400 g / t) were added to carry out a flotation treatment. The specific test results are shown in Table 2.
[0113] Table 2
[0114]
[0115] As can be seen from Table 1 above, the collector provided by the present invention can enhance the flotation recovery of coal slime by compounding biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether, and the concentrate yield is ≥69.11%, and the ash content is <11%; under the preferred embodiment, the concentrate yield is ≥71.38%, and the ash content is ≤10.42%.
[0116] Comparison of Examples 1-4 with Examples 5-8 shows that the recovery effect of coal slime is better when biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether are within a specific content range.
[0117] By comparing Example 1 with Comparative Examples 1-9, it can be seen that compared with conventional collectors, the collector using a combination of biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether has an increased concentrate yield and reduced ash content after flotation. When one of the components is removed or replaced by other agents, the concentrate yield decreases and the ash content increases.
[0118] By comparing Table 1 and Table 2, it can be seen that the coal slime flotation collector provided by the present invention can still have a good flotation effect when the ash content in the coal slime is high.
[0119] In summary, the collector provided by the present invention forms a specific ratio through biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether, which can not only improve the concentrate yield and reduce the concentrate ash content, but also overcome the disadvantages of traditional diesel, kerosene and the like that may exist in the process of coal slime recovery, such as large agent consumption, strong odor, high emission of volatile organic compounds, low recovery rate, etc., and provides a new way for the efficient recovery of coal slime resources.
[0120] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0121] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0122] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A coal slime flotation collector, characterized in that: The coal slime flotation collector comprises: Biodiesel, isopropyl alcohol ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether.
2. The coal slime flotation collector according to claim 1, characterized in that: The coal slime flotation collector comprises, by weight:
3. The coal slime flotation collector according to claim 1, characterized in that: The carbon chain R of the fatty alcohol polyoxyethylene ether is C7-C9.
4. The coal slime flotation collector according to claim 1, characterized in that: The polymerization degree of the fatty alcohol polyoxyethylene ether is 5-8.
5. A method for preparing a coal slime flotation collector according to any one of claims 1 to 4, characterized in that: The preparation method comprises: According to the weight ratio, biodiesel, isophylline ethyl ether, methyl isobutyl carbinol and fatty alcohol polyoxyethylene ether are mixed to obtain the coal slime flotation collector.
6. The preparation method according to claim 5, characterized in that: The mixture is stirred for 30-60 min.
7. Use of the coal slime flotation collector according to any one of claims 1 to 4, characterized in that: The uses include: The coal slime flotation collector is used to float the coal slime.
8. The use according to claim 7, characterized in that The flotation comprises: A frother and the coal slime flotation collector are added to the coal slime slurry for flotation.
9. The use according to claim 7 or 8, characterized in that The concentration of the coal slime slurry is 60-100 g / L.
10. The use according to claim 7 or 8, characterized in that The amount of the coal slime flotation collector added in the flotation is 100-800 g / t; Preferably, the amount of frother added in the flotation is 40-400 g / t; Preferably, the frother used in the flotation comprises secondary octanol and / or octanol.
Citation Information
Patent Citations
Method for realizing flotation of coal slime with use of oxidized kerosene
CN103143449A
Preparation method of coal slime flotation collector
CN105964410A