Preparation method and application of China rose-shaped silver powder with Raman enhancement effect

Through the liquid phase chemical reduction method combined with the preparation of aminoacetic acid and dispersant buffer, rose-like silver powder with excellent Raman enhancement effect was prepared, which solved the problem of complex and unenvironmental protection in the existing technology and achieved stability and high efficiency silver powder preparation and good Raman enhancement effect.

CN118875306AActive Publication Date: 2024-11-01XIAMEN UNIV

Patent Information

Application Number
CN202410911548.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The process of preparing micro-nano-scale flower-shaped silver powder in the prior art has the disadvantages of complexity, uneco-friendly, high energy consumption, poor repeatability and unstable morphology and dimensions, and lacks a simple, green, low-cost and excellent repeatability.

Method used

The silver glue solution was prepared by preparing the mixture of silver nitrate solution and aminoacetic acid, combined with dispersant and buffering agent, and the liquid phase chemical reduction method was used to prepare the silver glue solution, and the rose-like silver powder was formed through titration reaction, which was self-assembled and molded, avoiding the additional adjustment of the system pH and The temperature achieves a stable sheet structure and a good Raman enhancement effect.

Benefits of technology

The prepared rose-like silver powder has excellent Raman enhancement effect, stable structural morphology, good dispersion, simple and efficient process, suitable for commercial mass production, and meets green chemistry requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875306A_ABST
    Figure CN118875306A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of China rose-shaped silver powder with a Raman enhancement effect, which comprises the following steps of: (1) preparing a silver nitrate solution, and then adding glycine into the silver nitrate solution for fully dissolving to obtain a precursor solution; (2) preparing a reducing agent solution; adding a dispersing agent and a buffering agent into the reducing agent solution, heating and uniformly stirring to obtain a reducing agent-dispersing agent-buffering pair mixed solution; (3) in a dark environment at 22-26 DEG C, dropwise adding the precursor solution into the reducing agent-dispersing agent-buffer pair mixed solution while stirring, and continuously reacting after titration to obtain a silver colloid solution; and (4) the silver colloid solution is centrifuged, washed and dried in sequence, and the China rose-shaped silver powder is obtained. The method has the advantages of being simple, efficient, low in cost, large in process window and the like, and subsequent commercialized mass production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conductive material preparation, and in particular relates to a preparation method of rose-shaped silver powder with Raman enhancement effect and application thereof. Background Art

[0002] In 1974, Fleischmann L et al. found that the Raman signal intensity of pyridine molecules on the rough silver electrode surface was greatly enhanced, thus developing the surface enhanced Raman scattering (SERS) technology. SERS has broad application prospects in solid surface chemistry and trace analysis due to its high resolution and sensitivity. Among the metals with SERS, the study found that silver has the best enhancement effect.

[0003] At present, the liquid phase chemical reduction method is often used in the existing technology to prepare micro-nano scale flower-shaped silver powder. However, most reaction systems have the disadvantages of complicated process flow, environmental unfriendliness, high energy consumption, poor repeatability and unstable morphology and size of the prepared flower-shaped silver powder. Therefore, a method for preparing flower-shaped silver powder with simple process, green, energy-saving, low cost and excellent repeatability is urgently needed to be developed. Summary of the invention

[0004] The present invention aims to overcome the defects of the prior art and provide a method for preparing rose-shaped silver powder with Raman enhancement effect.

[0005] Another object of the present invention is to provide an application of the rose-shaped silver powder prepared by the above preparation method.

[0006] The technical solution of the present invention is as follows:

[0007] A method for preparing rose-shaped silver powder with Raman enhancement effect comprises the following steps:

[0008] (1) preparing a silver nitrate solution, and then adding glycine (Gly) to the silver nitrate solution to fully dissolve the silver nitrate solution to obtain a precursor solution;

[0009] (2) preparing a reducing agent solution; then mixing the dispersant, the buffer and the reducing agent in deionized water, heating the mixture to 58-62° C. and stirring evenly, and then cooling the mixture to 22-26° C. to obtain a reducing agent-dispersant-buffer mixed solution;

[0010] (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a volume ratio of 1:1 and a rate of 9 to 11 mL / s under stirring at 22 to 26° C. in a light-proof environment; after the titration is completed, the reaction is continued at 22 to 26° C. for 10 to 20 minutes to obtain a silver colloid solution;

[0011] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain the rose-shaped silver powder.

[0012] In a preferred embodiment of the present invention, the molar ratio of aminoacetic acid to silver nitrate is 0.02-0.25:1.

[0013] In a preferred embodiment of the present invention, the reducing agent is at least one of glucose, ascorbic acid, sodium citrate and fatty acid.

[0014] Further preferably, the reducing agent is ascorbic acid and / or sodium citrate.

[0015] In a preferred embodiment of the present invention, the dispersant is at least one of Tween 20, oleic acid, tannin, polyvinyl pyrrolidone (PVP), polyethylene glycol-1000 (PEG-1000) and gelatin.

[0016] Further preferably, the dispersant is at least one of polyvinyl pyrrolidone (PVP), polyethylene glycol-1000 (PEG-1000) and gelatin.

[0017] In a preferred embodiment of the present invention, the buffer pair is tartaric acid-sodium tartrate, citric acid-sodium citrate or acetic acid-sodium acetate.

[0018] Further preferably, the buffer pair is acetic acid-sodium acetate.

[0019] A rose-shaped silver powder is prepared by the above preparation method.

[0020] Use of the rose-shaped silver powder in preparing a surface Raman enhancement composition.

[0021] The beneficial effects of the present invention are:

[0022] 1. The rose-shaped silver powder prepared by the present invention is formed by self-assembly of flaky silver with a thickness of 70nm to 110nm. The petals of the rose-shaped silver are deposited by a number of small flaky silver, and the surface is rough, the structure is rich, and there are a large number of Raman enhancement active sites, so it has excellent Raman enhancement effect.

[0023] 2. The present invention belongs to the liquid phase chemical reduction method. Gly is added to the precursor solution to control the system to form a continuous and stable sheet structure. Dispersants and buffers are added to the reducing agent solution to promote the self-assembly of the flower-shaped silver powder, effectively hinder the agglomeration of the formed silver powder, and maintain the stability of the solution pH at the initial stage of the reaction.

[0024] 3. The present invention does not introduce seed crystals, and self-assembles in one step. In addition, there is no need to adjust the system pH, temperature, etc. during the reaction process. The preparation method has the advantages of being simple and efficient, low cost, and having a large process window, which is conducive to subsequent commercial mass production.

[0025] 4. The chemical reagents involved in the present invention are all environmentally friendly reagents and have no or low harm to human body, meeting the requirements of green chemistry advocated today.

[0026] 5. The rose-shaped silver powder prepared by the present invention has a stable structure and morphology, good dispersibility and obvious Raman enhancement effect. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a 5000x SEM image of the rose-shaped silver powder prepared in Example 1 of the present invention (the scale bar in the figure represents 1 μm).

[0028] Figure 2 This is a 20,000-fold SEM image of the rose-shaped silver powder prepared in Example 1 of the present invention (the scale bar 1 in the figure represents 200 nm).

[0029] Figure 3 This is a 5000x SEM image of the comparative silver powder prepared in Comparative Example 1 of the present invention (the scale 1 small grid in the figure is 1 μm).

[0030] Figure 4 This is a 5000x SEM image of the comparative silver powder prepared in Comparative Example 2 of the present invention (the scale bar in the image represents 1 μm).

[0031] Figure 5 This is an XRD comparison chart of the rose-shaped silver powder prepared in Example 1 of the present invention and a standard silver card.

[0032] Figure 6 This is a Raman spectrum of the CV solution using the rose-shaped silver powder prepared in Example 1 of the present invention as an enhanced substrate.

[0033] Where a is Ag substrate +10 -6 SERS spectra of CV solution of M, b is 10 -4 a is the normal Raman spectrum of the CV solution of M, c is the Raman spectrum of the Ag substrate. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0035] Example 1

[0036] (1) Preparation of precursor solution: prepare 20 mL of 0.2 mol / L silver nitrate solution, then add 0.006 g of Gly to the silver nitrate solution and stir for 1 to 2 min until fully dissolved to obtain a precursor solution;

[0037] (2) Preparation of a reducing agent-dispersant-buffer mixed solution: prepare 20 mL of a 0.15 mol / L ascorbic acid solution; then add 0.025 g of gelatin, 0.002 g of PVP, 0.004 g of acetic acid and 0.03 g of sodium acetate to the ascorbic acid solution, heat to 60° C., stir for 10 min, and cool to 25° C. to obtain a reducing agent-dispersant-buffer mixed solution.

[0038] (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a rate of 10 mL / s under ultrasonic treatment in a light-proof environment at 25° C. After the addition is completed, the reaction is continued at 25° C. for 15 minutes to obtain a silver colloid solution;

[0039] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain the rose-shaped silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 70°C for 6h.

[0040] Example 2

[0041] (1) Preparation of precursor solution: prepare 20 mL of 0.2 mol / L silver nitrate solution, then add 0.006 g of Gly to the silver nitrate solution and stir for 1 to 2 min until fully dissolved to obtain a precursor solution;

[0042] (2) Preparation of a reducing agent-dispersant-buffer mixed solution: prepare 20 mL of 0.15 mol / L ascorbic acid solution; then add 0.006 g of sodium citrate, 0.025 g of gelatin, 0.002 g of PVP, 0.004 g of acetic acid and 0.03 g of sodium acetate to the ascorbic acid solution, heat to 60°C, stir for 10 min, and cool to 25°C to obtain a reducing agent-dispersant-buffer mixed solution.

[0043] (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a rate of 10 mL / s under ultrasonic treatment in a light-proof environment at 25° C. After the addition is completed, the reaction is continued at 25° C. for 15 minutes to obtain a silver colloid solution;

[0044] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain the rose-shaped silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 70°C for 6h.

[0045] Example 3

[0046] (1) Preparation of precursor solution: prepare 20 mL of 0.2 mol / L silver nitrate solution, then add 0.006 g of Gly to the silver nitrate solution and stir for 1 to 2 min until fully dissolved to obtain a precursor solution;

[0047] (2) Preparation of a reducing agent-dispersant-buffer mixed solution: prepare 20 mL of 0.15 mol / L ascorbic acid solution; then add 0.025 g of gelatin, 0.009 g of PEG-1000, 0.004 g of acetic acid and 0.03 g of sodium acetate to the ascorbic acid solution, heat to 60°C, stir for 10 min, and cool to 25°C to obtain a reducing agent-dispersant-buffer mixed solution.

[0048] (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a rate of 10 mL / s under ultrasonic treatment in a light-proof environment at 25° C. After the addition is completed, the reaction is continued at 25° C. for 15 minutes to obtain a silver colloid solution;

[0049] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain the rose-shaped silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 70°C for 6h.

[0050] Comparative Example 1

[0051] (1) Preparation of precursor solution: Prepare 20 mL of 0.2 mol / L silver nitrate solution to obtain a precursor solution;

[0052] (2) Preparation of a reducing agent-dispersant-buffer mixed solution: prepare 20 mL of a 0.15 mol / L ascorbic acid solution; then add 0.025 g of gelatin, 0.002 g of PVP, 0.004 g of acetic acid and 0.03 g of sodium acetate to the ascorbic acid solution, heat to 60° C., stir for 10 min, and cool to 25° C. to obtain a reducing agent-dispersant-buffer mixed solution.

[0053] (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a rate of 10 mL / s under ultrasonic treatment in a light-proof environment at 25° C. After the addition is completed, the reaction is continued at 25° C. for 15 minutes to obtain a silver colloid solution;

[0054] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain comparative silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 70°C for 6h.

[0055] The difference between Comparative Example 1 and Example 1 is that no Gly is added to the precursor solution.

[0056] Comparative Example 2

[0057] (1) Preparation of precursor solution: prepare 20 mL of 0.2 mol / L silver nitrate solution, then add 0.006 g of Gly to the silver nitrate solution and stir for 1 to 2 min until fully dissolved to obtain a precursor solution;

[0058] (2) Preparation of a reducing agent-dispersant-buffer mixed solution: prepare 20 mL of a 0.15 mol / L ascorbic acid solution; then add 0.025 g of gelatin and 0.002 g of PVP to the ascorbic acid solution, heat to 60° C., stir for 10 min, and cool to 25° C. to obtain a reducing agent-dispersant-buffer mixed solution.

[0059] (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a rate of 10 mL / s under ultrasonic treatment in a light-proof environment at 25° C. After the addition is completed, the reaction is continued at 25° C. for 15 minutes to obtain a silver colloid solution;

[0060] (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain comparative silver powder. The centrifugal parameters are 10000r / min for 3min; the washing method is 3 times of deionized water washing and 2 times of anhydrous ethanol washing; the drying condition is drying in a forced air drying oven at 70°C for 6h.

[0061] The difference between Comparative Example 2 and Example 1 is that no buffer pair is added to the reducing agent solution.

[0062] 0.02 g of the rose-shaped silver powder prepared in Example 1 was dispersed in 2 mL of deionized water, dropped on a clean 1 cm × 1 cm silicon wafer, and dried at 60 ° C under vacuum for 12 h to obtain a simple substrate, which was then immersed in a 10 -6 The samples were placed in a CV solution of 100 M for 6 h and then taken out for Raman enhancement effect test.

[0063] Depend on Figure 1 and Figure 2 It can be seen that the rose-shaped silver powder prepared in Example 1 of the present invention has a stable flower shape and good particle dispersion. The rose-shaped silver powder is formed by self-assembly of flaky silver with a thickness of 70nm to 110nm, wherein the large silver flakes are deposited by a number of small silver flakes, so the surface is rough and the structure is rich.

[0064] Depend on Figure 3 and Figure 4It can be seen that in Comparative Example 1, Gly was not added, and the comparative silver powder was spherical as a whole. In Comparative Example 2, no buffer was added, and the morphology of the comparative silver powder was not stable enough, and the flaky silver failed to self-assemble into a good rose-shaped silver powder.

[0065] Depend on Figure 5 It can be seen that the rose-shaped silver powder prepared in Example 1 of the present invention has excellent crystallinity and no other crystalline impurities are produced, indicating that the rose-shaped silver powder prepared in Example 1 of the present invention has a high purity.

[0066] Depend on Figure 6 It can be seen that the characteristic peaks of a are significantly stronger than those of b, that is, the rose-shaped silver powder prepared by Example 1 of the present invention has an obvious Raman enhancement effect.

[0067] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. A method for preparing rose-shaped silver powder with Raman enhancement effect, characterized in that: The steps include: (1) preparing a silver nitrate solution, and then adding aminoacetic acid to the silver nitrate solution to fully dissolve it, thereby obtaining a precursor solution; (2) preparing a reducing agent solution; then mixing the dispersant, the buffer and the reducing agent in deionized water, heating the mixture to 58 to 62° C. and stirring evenly, and then cooling the mixture to 22 to 26° C. to obtain a reducing agent-dispersant-buffer mixed solution; (3) adding the precursor solution to the reducing agent-dispersant-buffer mixed solution at a volume ratio of 1:1 and a rate of 9 to 11 mL / s under stirring at 22 to 26° C. in a light-proof environment; after the titration is completed, the reaction is continued at 22 to 26° C. for 10 to 20 minutes to obtain a silver colloid solution; (4) The silver colloid solution is centrifuged, washed and dried in sequence to obtain the rose-shaped silver powder.

2. The preparation method according to claim 1, characterized in that: The molar ratio of aminoacetic acid to silver nitrate is 0.02-0.25:

1.

3. The preparation method according to claim 1 or 2, characterized in that: The reducing agent is at least one of glucose, ascorbic acid, sodium citrate and fatty acid.

4. The preparation method according to claim 3, characterized in that: The reducing agent is ascorbic acid and / or sodium citrate.

5. The preparation method according to claim 1 or 2, characterized in that: The dispersant is at least one of Tween 20, oleic acid, tannin, polyvinyl pyrrolidone, polyethylene glycol-1000 and gelatin.

6. The preparation method according to claim 5, characterized in that: The dispersant is at least one of polyvinyl pyrrolidone, polyethylene glycol-1000 and gelatin.

7. The preparation method according to claim 1 or 2, characterized in that: The buffer pair is tartaric acid-sodium tartrate, citric acid-sodium citrate or acetic acid-sodium acetate.

8. The preparation method according to claim 7, characterized in that: The buffer pair is acetic acid-sodium acetate.

9. A rose-shaped silver powder, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8.

10. Use of the rose-shaped silver powder according to claim 9 in preparing a surface Raman enhancement composition.

Citation Information

Patent Citations

  • Method for preparing cauliflower nano gold-silver alloy with surface-enhanced Raman scattering activity

    CN101786170A

  • Method for preparing surface enhanced Raman scattering active substrate with three-dimensional silver micro-nano structure

    CN102221543A

  • Multi-branched gold and silver composite nanomaterial having excellent surface enhanced Raman scattering characteristics and preparation method thereof

    CN106853523A

  • Nano-silver controled particles size and preparing thereof

    KR1020100115201A

Cited By

  • Silver powder and preparation method thereof

    CN121870100A

  • Silver powder and its preparation method

    CN121870100B