Preparation method of low-oxygen metal titanium powder
Through the mixing pressing of rare earth metal chloride and titanium dioxide and thermal reduction of alkali metal, combined with vacuum distillation, the problems of high cost and complex operation in the Kroll method are solved, and the efficient preparation of low-oxygen metal titanium powder is achieved, reducing the oxygen content and process time .
Patent Information
- Application Number
- CN202410957071.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The Kroll method has problems such as high corrosion equipment requirements, high power consumption, high cost and difficult operation in the production of metal titanium, especially in the process of chlorination and magnesium electrolysis.
The mixture of rare earth metal chloride and titanium dioxide is made by mixing pressing, and the alkali metal thermal reduction and vacuum distillation are carried out to directly obtain low-oxygen metal titanium powder, avoiding the chlorination treatment step and simplifying the process flow.
It significantly reduces production costs, shortens the process flow time, improves production efficiency, and realizes the metal thermal reduction reaction at a lower temperature to obtain high-purity low-oxygen metal titanium powder with an oxygen content of <500ppm.
Smart Images

Figure CN118875310A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal titanium powder preparation, and particularly relates to a method for preparing low-oxygen metal titanium powder. Background Art
[0002] Titanium metal has the advantages of high specific strength, good biocompatibility, and strong corrosion resistance, and is widely used in aerospace and other fields. At present, the Kroll process is widely used in industry to produce titanium metal. The Kroll process mainly includes three steps: chlorination refining, reduction distillation, and magnesium electrolysis. The specific process is shown in Figure 1 First, TiO 2 Conversion to TiCl 4 , and then use liquid magnesium to reduce TiCl 4 Titanium sponge is obtained, and finally MgCl is electrolyzed 2 Chlorine and magnesium are recovered.
[0003] The Kroll process first requires chlorination of the raw materials during production. Although this method can remove the impurity oxygen in the raw materials to the greatest extent, chlorine is highly corrosive to the equipment, so the material and performance requirements of the equipment are extremely high. In addition, in the subsequent MgCl 2 The electrolysis process consumes a lot of electricity, which further increases the production cost. The use of magnesium as a reducing agent is relatively expensive, and due to the low melting point of magnesium, the production process must strictly control the temperature, which increases the difficulty of operation. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a method for preparing low-oxygen titanium metal powder. The preparation method provided by the present invention does not require chlorination treatment, has low cost and is simple to operate.
[0005] In order to achieve the above object, the present invention provides the following scheme:
[0006] The present invention provides a method for preparing low-oxygen titanium metal powder, comprising the following steps:
[0007] Mixing rare earth metal chloride and titanium dioxide, and pressing and molding to obtain mixed compacts;
[0008] The mixed compact is subjected to metal thermal reduction by using an alkali metal, and the obtained reduction product is subjected to vacuum distillation to obtain low-oxygen metal titanium powder.
[0009] Preferably, the metal thermal reduction is carried out under normal pressure or vacuum conditions.
[0010] Preferably, when normal pressure is used, the temperature of the metal thermal reduction is 900-1000° C., and the time is 10-48 hours; when vacuum conditions are used, the temperature of the metal thermal reduction is 700-1000° C., and the time is 10-36 hours.
[0011] Preferably, the rare earth metal chloride comprises YCl 3 、LaCl 3 、CeCl 3 、NdCl 3 , HoCl 3 , GdCl 3 , DyCl 3 and PrCl 3 One or more of the .
[0012] Preferably, the mass ratio of the rare earth metal chloride to titanium dioxide is (5-10):1.
[0013] Preferably, the alkali metal comprises sodium and / or potassium.
[0014] Preferably, the compression molding pressure is 300-900 MPa.
[0015] Preferably, the mass ratio of the alkali metal to titanium dioxide is (2-10):1.
[0016] Preferably, the vacuum distillation temperature is 800-1000° C., the time is 2-10 hours, and the system pressure is 1-25 Pa.
[0017] Preferably, the oxygen content in the low-oxygen titanium metal powder is less than 500 ppm, and the purity is greater than 99%.
[0018] The present invention provides a method for preparing low-oxygen titanium metal powder, comprising the following steps:
[0019] The chloride of rare earth metal and titanium dioxide are mixed and pressed to obtain mixed compacts; the mixed compacts are subjected to metal thermal reduction by using alkali metals, and the obtained reduction products are subjected to vacuum distillation to obtain low-oxygen titanium metal powder.
[0020] The preparation method provided by the present invention does not require chlorination treatment; the raw material used in the present invention is titanium dioxide, which is low in cost; the preparation process is short, the energy consumption is low, and therefore the cost is low; the preparation method provided by the present invention is simple to operate.
[0021] The Kroll method takes more than 10 days to produce metallic titanium in the whole process. The present invention reduces titanium dioxide to metallic titanium in one step in only 10 to 48 hours, which greatly shortens the process flow and improves production efficiency. At the same time, low-oxygen metallic titanium powder with an oxygen content of less than 500 ppm can also be obtained.
[0022] The metal thermal reduction reaction of the present invention is simple and has no side reactions, which significantly improves the efficiency of the preparation process.
[0023] Furthermore, the present invention can smoothly carry out the metal thermal reduction reaction at a relatively low temperature (700-1000° C.), thereby improving the feasibility of the method. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0025] Figure 1 This is the process flow chart of Kroll method;
[0026] Figure 2 A flow chart of preparing low-oxygen titanium metal powder according to the present invention;
[0027] Figure 3 This is the XRD spectrum of the low-oxygen titanium powder obtained in Example 1 of the present invention;
[0028] Figure 4 This is a schematic diagram of a reaction device for preparing low-oxygen titanium metal powder according to the present invention. DETAILED DESCRIPTION
[0029] The present invention provides a method for preparing low-oxygen titanium metal powder, comprising the following steps:
[0030] Mixing rare earth metal chloride and titanium dioxide, and pressing and molding to obtain mixed compacts;
[0031] The mixed compact is subjected to metal thermal reduction by using an alkali metal, and the obtained reduction product is subjected to vacuum distillation to obtain low-oxygen metal titanium powder.
[0032] Unless otherwise specified, the raw materials and equipment used in the present invention are commercially available.
[0033] The invention mixes rare earth metal chloride and titanium dioxide, and performs compression molding to obtain a mixed compact.
[0034] In the present invention, the rare earth metal chloride preferably includes YCl 3 、LaCl 3 、CeCl 3 、NdCl 3 , HoCl 3 , GdCl 3 , DyCl 3 and PrCl 3In the present invention, the mass ratio of the rare earth metal chloride to titanium dioxide is preferably (5-10):1, and more preferably (6-8):1. In the present invention, the pressure of the press molding is preferably 300-900 MPa, and more preferably 400-800 MPa.
[0035] After obtaining the mixed compact, the present invention uses an alkali metal to perform metal thermal reduction on the mixed compact, and the obtained reduction product is subjected to vacuum distillation to obtain low-oxygen metal titanium powder.
[0036] The present invention preferably places the alkali metal at the bottom of the crucible, and places the mixed compact on the alkali metal for metal thermal reduction, specifically: placing the alkali metal at the bottom of the titanium crucible, and then placing a titanium foil with small holes on it, and placing the mixed compact on the titanium foil, covering it with a titanium lid, and placing the crucible containing the alkali metal and the mixed compact in a muffle furnace for metal thermal reduction.
[0037] In the present invention, the mass ratio of the alkali metal to titanium dioxide is preferably (2-10):1, and more preferably (3-8):1.
[0038] In the present invention, the metal thermal reduction reaction is preferably carried out under normal pressure or vacuum conditions. When normal pressure is used, the temperature of the metal thermal reduction is preferably 900°C to 1000°C, more preferably 930°C to 980°C; the time is preferably 10 to 48 hours, more preferably 20 to 40 hours.
[0039] When vacuum conditions are used, the temperature of the metal thermal reduction is preferably 700-1000° C., more preferably 800-850° C.; the time is preferably 10-36 hours, more preferably 15-36 hours.
[0040] In the process of the metal thermal reduction reaction of the present invention, the alkali metal is converted into vapor and then contacts with the mixed compact to reduce the titanium dioxide in the mixed compact.
[0041] In the present invention, the alkali metal preferably includes sodium and / or potassium; when the alkali metal is sodium, the equation of the metal thermal reduction reaction is 3Na(g)+RECl 3 +3 / 4TiO 2 =3 / 4Ti+3NaCl+1 / 2RE 2 O 3 and 3Na(g)+3 / 2RECl 3 +3 / 4TiO 2 =3 / 2REOCl+3 / 4Ti+3NaCl. When the alkali metal is potassium, the equation for the metal thermal reduction reaction is 3K(g)+RECl 3 +3 / 4TiO 2=3 / 4Ti+3KCl+1 / 2RE 2 O 3 and 3K(g)+3 / 2RECl 3 +3 / 4TiO 2 =3 / 2REOCl+3 / 4Ti+3KCl.
[0042] Before the vacuum distillation, the present invention preferably further comprises quenching the obtained reduction product.
[0043] In the present invention, the temperature of the vacuum distillation is preferably 800-1000°C, more preferably 850-950°C; the time is preferably 2-10h, more preferably 3-8h; the system pressure is preferably 1-25Pa, more preferably 5-20Pa.
[0044] The present invention has no special requirements for the vacuum distillation method, and methods well known in the art can be used. In the present invention, since RECl 3 The saturated vapor pressure of non-titanium impurities such as Na, K and KCl is relatively large and can be separated from the target product titanium by vacuum distillation.
[0045] In the present invention, the oxygen content of the titanium powder is determined by measuring the oxygen content of the titanium wire as the oxygen content of the titanium powder.
[0046] After the vacuum distillation is completed, the present invention preferably further comprises grinding, acid washing and drying the obtained product in sequence. The present invention has no special requirements for the acid washing, and the method well known in the art can be used to remove REOCl, RE 2 O 3 In the present invention, the drying preferably includes vacuum drying to prevent the low-oxygen titanium metal powder from being oxidized.
[0047] In the present invention, the oxygen content in the low-oxygen titanium metal powder is preferably less than 500 ppm, preferably 50 ppm≤oxygen content≤450 ppm, and the purity is preferably >99%, and more preferably 99.24-99.83%.
[0048] Figure 2 The flowchart of the present invention for preparing low-oxygen titanium powder is shown in FIG. Figure 2 As shown, the present invention converts rare earth metal chloride (RECl 3 ) and titanium dioxide (TiO 2 ) are mixed and pressed to obtain a mixed compact; an alkali metal (Na vapor) is placed at the bottom of the crucible, and the mixed compact is placed above the alkali metal, and a metal thermal reduction reaction is carried out under normal pressure or vacuum conditions; after the reaction is completed, low-oxygen titanium metal powder is obtained by vacuum distillation (i.e., vacuum separation), washing and drying.
[0049] The preparation method provided by the present invention does not require chlorination treatment; the raw material used in the present invention is titanium dioxide, which is low in cost; the preparation process is short, the energy consumption is low, and therefore the cost is low; the preparation method provided by the present invention is simple to operate.
[0050] The Kroll method takes more than 10 days to produce metallic titanium in the whole process. The present invention reduces titanium dioxide to metallic titanium in one step in only 10 to 48 hours, which greatly shortens the process flow and improves production efficiency. At the same time, low-oxygen metallic titanium powder with an oxygen content of less than 500 ppm can also be obtained.
[0051] The metal thermal reduction reaction of the present invention is simple and has no side reactions, which significantly improves the efficiency of the preparation process; at the same time, the present invention can significantly smoothly carry out the metal thermal reduction reaction at a relatively low temperature (700-1000° C.), thereby improving the feasibility of the method.
[0052] In order to further illustrate the present invention, a method for preparing a low-oxygen titanium metal powder provided by the present invention is described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0053] Example 1
[0054] CeCl was added at a mass ratio of 5:1 3 and TiO 2 The mixture was uniformly mixed and pressed into a mixed compact with a diameter of 40 mm and a thickness of 12 mm under a pressure of 500 MPa. The total mass of the mixed compact was 6 g, CeCl 3 The mass is 5g, TiO 2 The mass is 1g.
[0055] Place 2g of metallic Na at the bottom of a titanium crucible (26mm outer diameter, 1mm thickness, 90mm height), then place a titanium foil with small holes on top, and place 6g of the mixed compact on the titanium foil, cover with a titanium lid, and then place it in a stainless steel crucible (90mm outer diameter, 3mm thickness, 100mm height). Finally, place the stainless steel crucible in a muffle furnace, set the temperature to 900°C, and react for 48h at normal pressure. After the reaction is completed, take the stainless steel out of the muffle furnace and put it in water for quenching. After the stainless steel crucible cools, take out the titanium-containing mixture. The reaction device is as follows: Figure 4 shown.
[0056] Vacuum distillation (temperature 900 ° C, time 2 h, system pressure 10 Pa) was used to remove CeCl from the titanium-containing mixture. 3 and Na, and then the resulting reduction product was ground and washed with dilute nitric acid to remove Ce. 2 O 3 and NaCl, and dried in vacuum to obtain low-oxygen metallic titanium powder.
[0057] The phase of the product was determined by XRD. Figure 3 As shown, it can be seen that the experimental product is metallic titanium.
[0058] The oxygen content of the titanium wire was measured by LECO, and the oxygen content was 450 ppm with a purity of 99.24%.
[0059] Embodiments 2 to 5
[0060] The preparation steps are the same as those in Example 1, except that CeCl 3 Replaced by NdCl 3 , YCl 3 , HoCl 3 、LaCl 3 The product purity and oxygen content and reaction conditions of Examples 1 to 5 are summarized in Table 1.
[0061] Table 1 Summary of product purity, oxygen content and reaction conditions of Examples 1 to 5
[0062] serial number Main raw materials Reduction temperature ℃ Product purity % Oxygen content ppm Example 1 <![CDATA[CeCl 3 、TiO 2 、By]]> 900 99.24 450 Example 2 <![CDATA[NdCl 3 、TiO 2 、By]]> 900 99.78 130 Example 3 <![CDATA[YCl 3 、TiO 2 、By]]> 1000 99.80 100 Example 4 <![CDATA[HoCl 3 、TiO 2 、By]]> 950 99.53 220 Example 5 <![CDATA[LaCl 3 、TiO 2 、By]]> 950 99.66 150
[0063] Example 6
[0064] CeCl was added at a mass ratio of 9:1 3 and TiO 2 The mixture was uniformly mixed and pressed into a mixed compact with a diameter of 40 mm and a thickness of 15 mm under a pressure of 800 MPa. The total mass of the mixed compact was 10 g, CeCl 3 The mass is 9g, TiO 2 The mass is 1g.
[0065] Place 5g of metallic Na at the bottom of a titanium crucible (26mm outer diameter, 1mm thickness, 90mm height), then place a titanium foil with small holes on top, and place 10g of the mixed compact on the titanium foil, cover it with a titanium lid, and then place it in a stainless steel crucible (90mm outer diameter, 3mm thickness, 100mm height). Finally, place the stainless steel crucible in a muffle furnace, set the temperature to 1000°C, and react for 48h at normal pressure. After the reaction is completed, take the stainless steel out of the muffle furnace and put it in water for quenching. After the stainless steel crucible cools, take out the titanium-containing mixture. The reaction device is as follows: Figure 4 shown.
[0066] Vacuum distillation (temperature 900 ° C, time 2 h, system pressure 8 Pa) was used to remove CeCl from the titanium-containing mixture. 3 , Na, and then grind the obtained reduction product, wash it with dilute nitric acid to remove CeOCl and NaCl, and then vacuum dry it to obtain low-oxygen metal titanium powder.
[0067] The oxygen content of the titanium wire was measured by LECO, and the oxygen content was 100 ppm and the purity was 99.76%.
[0068] Embodiments 7 to 10
[0069] The preparation steps are the same as those in Example 6, except that CeCl 3 Replaced by NdCl 3 , YCl 3 , HoCl 3 、LaCl 3 The product purity and oxygen content and reaction conditions of Examples 7 to 10 are summarized in Table 2.
[0070] Table 2 Summary of product purity, oxygen content and reaction conditions of Examples 6 to 10
[0071] serial number Main raw materials Reduction temperature ℃ Product purity % Oxygen content ppm Example 6 <![CDATA[CeCl 3 、TiO 2 、By]]> 1000 99.76 100 Example 7 <![CDATA[NdCl 3 、TiO 2 、By]]> 900 99.68 120 Example 8 <![CDATA[YCl 3 、TiO 2 、By]]> 1000 99.83 50 Example 9 <![CDATA[HoCl 3 、TiO 2 、By]]> 950 99.82 80 Example 10 <![CDATA[LaCl 3 、TiO 2 、By]]> 950 99.50 120
[0072] Embodiment 11
[0073] CeCl was added at a mass ratio of 8:1 3 and TiO 2 The mixture was uniformly mixed and pressed into a mixed compact with a diameter of 40 mm and a thickness of 15 mm under a pressure of 500 MPa. The total mass of the mixed compact was 9 g, CeCl 3 The mass is 8g, TiO 2 The mass is 1g.
[0074] 4g of metal K is placed at the bottom of a titanium crucible (26mm outer diameter, 1mm thickness, 90mm height), and then a titanium foil with small holes is placed on top, and 9g of the mixed compact is placed on the titanium foil, covered with a titanium lid, and then placed in a stainless steel crucible (90mm outer diameter, 3mm thickness, 100mm height). Finally, the stainless steel crucible is placed in a muffle furnace, and the temperature is set to 950°C, and the reaction time is 36h at normal pressure. After the reaction is completed, the stainless steel is taken out of the muffle furnace and placed in water for quenching. After the stainless steel crucible is cooled, the titanium-containing mixture is taken out. The reaction device is as follows: Figure 4 shown.
[0075] Vacuum distillation (temperature 900 ° C, time 2.5 h, system pressure 20 Pa) was used to remove CeCl from the titanium-containing mixture. 3 , KCl, K, and then grind the obtained reduction product, wash it with dilute nitric acid to remove CeOCl, and vacuum dry it to obtain low-oxygen metal titanium powder.
[0076] The oxygen content of the titanium wire was measured by LECO, and the oxygen content was 320 ppm, with a purity of 99.54%.
[0077] Embodiments 12 to 13
[0078] The preparation steps are the same as those in Example 11, except that CeCl 3 Replaced with YCl 3 、LaCl 3 .
[0079] The product purity and oxygen content and reaction conditions of Examples 11 to 13 are summarized in Table 3.
[0080] Table 3 Summary of product purity, oxygen content and reaction conditions of Examples 11 to 13
[0081]
[0082]
[0083] It can be seen from Table 1, Table 2 and Table 3 that the low-oxygen titanium powder prepared by the present invention has high purity (>99%) and an oxygen content of <500 ppm.
[0084] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing low-oxygen titanium metal powder, characterized in that: The following steps are involved: Mixing rare earth metal chloride and titanium dioxide, and pressing and molding to obtain mixed compacts; The mixed compact is subjected to metal thermal reduction by using an alkali metal, and the obtained reduction product is subjected to vacuum distillation to obtain low-oxygen metal titanium powder.
2. The preparation method according to claim 1, characterized in that: The metal thermal reduction is carried out under normal pressure or vacuum conditions.
3. The preparation method according to claim 2, characterized in that: When normal pressure is used, the temperature of the metal thermal reduction is 900-1000° C. and the time is 10-48 hours; when vacuum conditions are used, the temperature of the metal thermal reduction is 700-1000° C. and the time is 10-36 hours.
4. The preparation method according to claim 1, characterized in that: The rare earth metal chloride includes one or more of YCl3, LaCl3, CeCl3, NdCl3, HoCl3, GdCl3, DyCl3 and PrCl3.
5. The preparation method according to claim 1 or 4, characterized in that: The mass ratio of the rare earth metal chloride to titanium dioxide is (5-10):
1.
6. The preparation method according to claim 1, characterized in that: The alkali metal includes sodium and / or potassium.
7. The preparation method according to claim 1 or 2, characterized in that: The pressure of the pressing molding is 300-900 MPa.
8. The preparation method according to claim 1 or 6, characterized in that: The mass ratio of the alkali metal to titanium dioxide is (2-10):
1.
9. The preparation method according to claim 1 or 2, characterized in that: The temperature of the vacuum distillation is 800-1000° C., the time is 2-10 hours, and the system pressure is 1-25 Pa.
10. The preparation method according to claim 1, characterized in that: The oxygen content of the low-oxygen titanium metal powder is less than 500 ppm, and the purity is greater than 99%.
Citation Information
Cited By
Preparation method of low-oxygen titanium-containing powder
CN119819922A