TiAl intermetallic compound linear friction welding joint destressing method

Through the slow cooling and forging pressure control of multiple slow cooling stages, the problem of linear friction welded joints being prone to cracks or cracks is solved, and the formation and production efficiency of high-quality welded joints are improved.

CN118875461APending Publication Date: 2024-11-01AVIC BEIJING AERONAUTICAL MFG TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411231716.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

TiAl intermetallic compound welded joints formed by linear friction welding are prone to cracking or lateral cracks, resulting in poor welding.

Method used

Multiple slow cooling stages are used to slowly cool the weld joint from the welding temperature to the preset temperature, and then cool it naturally to room temperature. By maintaining the forging pressure and controlling the temperature drop amplitude and insulation time, the residual stress in the weld area is reduced and crack formation is avoided. .

Benefits of technology

Effectively reduce residual stress in the weld area, eliminate crack tendencies, simplify process steps, improve production efficiency, and form high-quality welded joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875461A_ABST
    Figure CN118875461A_ABST
Patent Text Reader

Abstract

The invention provides a TiAl intermetallic compound linear friction welding joint destressing method which comprises the following steps: mounting a first weldment and a second weldment on linear friction welding equipment, applying upsetting pressure with a first preset numerical value to the first weldment, carrying out linear friction welding, and then applying upsetting pressure with a second preset numerical value to the second weldment; the first weldment and the second weldment are welded and connected to form a welded joint; and after linear friction welding is completed, the upsetting pressure of a second preset numerical value is maintained, the welding joint is slowly cooled to the preset temperature from the welding temperature in multiple slow cooling stages, then the welding joint is naturally cooled to the room temperature from the preset temperature, the temperature reduction amplitude of every two adjacent stages is not larger than 100 DEG C, and the heat preservation time of each stage is not shorter than 10 min. The welded joint prepared by the destressing method provided by the invention is good in quality, and has no crack defect inside.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of linear friction welding, and more specifically to a stress relief method for a TiAl intermetallic compound linear friction welding joint. Background Art

[0002] Linear friction welding is a welding method that has developed rapidly in recent years and is mainly used in the manufacture of titanium alloy parts.

[0003] Linear friction welding is a solid phase welding process that can obtain high-performance, high-quality welds with dense forging structures. It is suitable for welding materials with good plasticity such as titanium alloys.

[0004] For TiAl intermetallic compounds, linear friction welding cools down very quickly after welding. The welding temperature is about 1200℃. The temperature of the weld zone can be reduced to below 200℃ within one or two minutes after welding. The room temperature plasticity of this material is low, the welding residual stress is high, and the cooling speed after welding is fast, which leads to direct cracking or transverse cracks in the specimen after welding. It is difficult to form a good welding joint. Figure 1 , Figure 2 As shown, in Figure 1 In the welding joint, good connection is not achieved. Figure 2 In the process, obvious transverse cracks appear on the welded joint. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] The technical problem to be solved by the present invention is that a welded joint formed by linear friction welding is prone to cracking or generating transverse cracks.

[0007] (II) Technical solution

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for relieving stress of a TiAl intermetallic linear friction welding joint is provided, comprising the following steps:

[0010] Mounting the first weldment and the second weldment on a linear friction welding device, applying a first preset value of upsetting pressure to the first weldment, and performing linear friction welding, so that the first weldment and the second weldment are welded and connected to form a welded joint;

[0011] After linear friction welding is completed, the top forging pressure of the second preset value is maintained, and the weld joint is slowly cooled from the welding temperature to the preset temperature in multiple slow cooling stages, and then naturally cooled from the preset temperature to room temperature, wherein the temperature drop between two adjacent stages is not greater than 100°C, and the insulation time of each stage is not less than 10 minutes.

[0012] Preferably, the linear friction welding comprises the following steps:

[0013] Applying a first preset value of upsetting pressure to the first weldment along a first direction, so that the first weldment contacts the second weldment, and the second weldment vibrates linearly along a second direction to generate heat, providing a welding heat source, wherein the second direction is perpendicular to the first direction;

[0014] When the linear friction welding temperature of the first weldment and the second weldment reaches a preset welding temperature, the second weldment stops vibrating and maintains applying a second preset value of upsetting pressure, and the first weldment and the second weldment are welded together to form a weld joint.

[0015] Preferably, the holding time for each stage is 10-15 min.

[0016] Preferably, the welded joint is slowly cooled from a preset welding temperature to 500° C. in four slow cooling stages.

[0017] Preferably, the holding temperatures and holding times of the four slow cooling stages are:

[0018] The first slow cooling stage: the holding temperature is 850℃-800℃, and the holding time is 10-15min;

[0019] The second slow cooling stage: the holding temperature is 750℃-700℃, and the holding time is 10-15min;

[0020] The third slow cooling stage: the holding temperature is 650℃-600℃, and the holding time is 10-15min;

[0021] The fourth slow cooling stage: the holding temperature is 550℃-500℃, and the holding time is 10-15min.

[0022] Preferably, the materials of the first weldment and the second weldment are both titanium-aluminum intermetallic compounds.

[0023] Preferably, the multiple slow cooling stages are all carried out in an insulated box with adjustable temperature.

[0024] Preferably, the second preset value is not less than the first preset value.

[0025] Preferably, the preset temperature is 500°C.

[0026] (III) Beneficial effects

[0027] The above technical solution of the present invention has at least the following advantages:

[0028] In the present invention, after the first weldment and the second weldment are linearly friction welded to form a welded joint, the welded joint is slowly cooled from the welding temperature to a preset temperature in multiple slow cooling stages, and then naturally cooled from the preset temperature to room temperature; through the above technical solution, the residual stress in the weld zone can be better reduced and the crack tendency can be eliminated. Moreover, the welded joint formed after welding does not need to be subjected to a separate post-weld heat treatment, which simplifies the process steps and improves production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 It is one of the schematic diagrams of the post-welding state of a linear friction welding joint in the prior art.

[0031] Figure 2 This is the second schematic diagram of the post-welding state of the linear friction welding joint in the prior art.

[0032] Figure 3 It is a schematic diagram of the implementation principle of linear friction welding provided by an embodiment of the present invention.

[0033] Figure 4 It is a schematic flow chart of a stress relief method for a TiAl intermetallic compound linear friction welding joint provided in an embodiment of the present invention.

[0034] Figure 5 It is a schematic diagram of the post-welding state of the linear friction welding joint provided by an embodiment of the present invention.

[0035] The reference numerals in the figures are:

[0036] 1. First weldment; 2. Second weldment. DETAILED DESCRIPTION

[0037] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0038] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it may be directly located on the other element or indirectly located on the other element. When an element is referred to as being "connected to" another element, it may be directly connected to the other element or indirectly connected to the other element.

[0039] It should be understood that the terms "length", "width", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" etc., indicating directions or positional relationships, are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention, and do not indicate that a device or element must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.

[0040] In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating relative importance or indicating the number of technical features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The specific implementation of the present invention is described in more detail below in conjunction with specific embodiments:

[0041] like Figure 3 and Figure 4 As shown, an embodiment of the present invention provides a method for relieving stress of a TiAl intermetallic compound linear friction welding joint, comprising the following steps:

[0042] The first weldment 1 and the second weldment 2 are mounted on a linear friction welding device, and a first preset value of upsetting pressure p is applied to the first weldment 1 to perform linear friction welding, so that the first weldment 1 and the second weldment 2 are welded and connected to form a welded joint;

[0043] After the linear friction welding is completed, the forging pressure of the second preset value is maintained, and the weld joint is slowly cooled from the welding temperature to the preset temperature in multiple slow cooling stages, and then naturally cooled from the preset temperature to room temperature, wherein the temperature drop between two adjacent stages is not greater than 100°C, and the insulation time of each stage is not less than 10 minutes. The preset temperature value is determined according to the characteristics of the material. Preferably, the plasticity of the material is good within the range from the preset temperature to the welding temperature. The room temperature plasticity of TiAl material is low, and the elongation is about 2%, but at a high temperature of 900°C, the elongation can reach about 10%. Based on this material with low room temperature plasticity but good high temperature plasticity, and from the perspective of post-weld joint formation, in the linear friction welding process, the plastic metal flows sufficiently and flash can be formed, indicating that the cold cracks or direct cracks are caused by the excessively fast cooling speed after welding. Therefore, the cooling speed is reduced by slow cooling after welding to avoid cold cracks or direct cracks caused by sudden cooling.

[0044] In one embodiment, linear friction welding includes the following steps:

[0045] Applying a first preset value of upsetting pressure to the first weldment 1 along a first direction, so that the first weldment 1 contacts the second weldment 2, and the second weldment 2 linearly vibrates along a second direction a to generate heat, the second direction being perpendicular to the first direction;

[0046] When the linear friction welding temperature of the first weldment 1 and the second weldment 2 reaches the preset welding temperature, the second weldment 2 stops vibrating, and the upsetting pressure of the second preset value is maintained, and the first weldment 1 and the second weldment 2 are welded together to form a welded joint. The second weldment 2 realizes linear vibration along the second direction a at a certain frequency and amplitude; the first weldment 1 contacts the end face of the weldment 2 under the action of the upsetting force along the first direction, and high-frequency friction occurs on the contact surface to generate heat. As the temperature rises, the contact surface material softens and is extruded. When the extrusion reaches a certain degree, the vibration is quickly stopped, and the upsetting force is applied to connect the two weldments into one, completing the welding process.

[0047] In one embodiment, the holding time of each stage is 10-15 minutes.

[0048] In one embodiment, the welded joint is slowly cooled from a preset welding temperature to 500° C. in four slow cooling stages.

[0049] In one embodiment, the holding temperatures and holding times of the four slow cooling stages are:

[0050] The first slow cooling stage: the holding temperature is 850℃-800℃, and the holding time is 10-15min;

[0051] The second slow cooling stage: the holding temperature is 750℃-700℃, and the holding time is 10-15min;

[0052] The third slow cooling stage: the holding temperature is 650℃-600℃, and the holding time is 10-15min;

[0053] The fourth slow cooling stage: the holding temperature is 550℃-500℃, and the holding time is 10-15min.

[0054] After four slow cooling stages and natural cooling to room temperature, the state of the welded joint is as follows Figure 5 As shown, it can be seen that the welded joint is of good quality and has no crack defects inside.

[0055] In one embodiment, the materials of the first weldment 1 and the second weldment 2 are both titanium-aluminum intermetallic compounds.

[0056] In one embodiment, the multiple slow cooling stages are performed in an incubator with adjustable temperature.

[0057] In one embodiment, the second preset value is not less than the first preset value.

[0058] In one embodiment, the preset temperature is 500°C.

[0059] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for relieving stress of a TiAl intermetallic linear friction welding joint, characterized in that: The following steps are involved: Mounting the first weldment and the second weldment on a linear friction welding device, applying a first preset value of upsetting pressure to the first weldment, and performing linear friction welding, so that the first weldment and the second weldment are welded and connected to form a welded joint; After linear friction welding is completed, the top forging pressure of the second preset value is maintained, and the weld joint is slowly cooled from the welding temperature to the preset temperature in multiple slow cooling stages, and then naturally cooled from the preset temperature to room temperature, wherein the temperature drop between two adjacent stages is not greater than 100°C, and the insulation time of each stage is not less than 10 minutes.

2. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: The linear friction welding comprises the following steps: Applying a first preset value of upsetting pressure to the first weldment along a first direction, so that the first weldment contacts the second weldment, and the second weldment linearly vibrates along a second direction to generate heat, wherein the second direction is perpendicular to the first direction; When the linear friction welding temperature of the first weldment and the second weldment reaches a preset welding temperature, the second weldment stops vibrating and maintains applying a second preset value of upsetting pressure, and the first weldment and the second weldment are welded together to form a weld joint.

3. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: The holding time for each stage is 10-15 minutes.

4. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: The welded joint is slowly cooled from the preset welding temperature to 500°C in four slow cooling stages.

5. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 4, characterized in that: The holding temperatures and holding times of the four slow cooling stages are: The first slow cooling stage: the holding temperature is 850℃-800℃, and the holding time is 10-15min; The second slow cooling stage: the holding temperature is 750℃-700℃, and the holding time is 10-15min; The third slow cooling stage: the holding temperature is 650℃-600℃, and the holding time is 10-15min; The fourth slow cooling stage: the holding temperature is 550℃-500℃, and the holding time is 10-15min.

6. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: The materials of the first weldment and the second weldment are both titanium-aluminum intermetallic compounds.

7. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: Multiple slow cooling stages are carried out in an incubator with adjustable temperature.

8. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: The second preset value is not less than the first preset value.

9. The TiAl intermetallic compound linear friction welding joint stress relief method according to claim 1, characterized in that: The preset temperature is 500°C.