Laminated bullet-proof glass and preparation process thereof

Through the design of polyurethane layer and modified PVB film, the problem of low thickness and light transmittance of laminated bulletproof glass in the prior art is solved, high impact strength, good transparency and heat resistance are achieved, and waterproofness and flame retardancy are taken into account. Performance improves overall performance.

CN118876522APending Publication Date: 2024-11-01侯凯莉
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410938392.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

While improving bulletproof performance, existing laminated bulletproof glass increases thickness and weight, low light transmittance, and difficult to take into account both flame retardancy and aging resistance.

Method used

Polytetrahydrofuran ether glycol is covalently bonded with isocyanate to form a polyurethane layer and is connected to diols and chlorinated phosphate to improve elasticity and flame retardant properties; organic acids and plasticizers are introduced into polyethylene butyral, Improve the impact strength and light transmittance of PVB film; use cured adhesives to improve waterproofness and transparency, reasonably arrange the thickness and order of semi-tempered glass, polycarbonate plates and polyurethane layers, and control the heat resistance of laminated bulletproof glass and impact strength.

Benefits of technology

The high impact strength, good transparency, heat resistance and water resistance of laminated bulletproof glass is achieved, reducing the overall weight and maintaining excellent bulletproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118876522A_ABST
    Figure CN118876522A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of bullet-proof glass, in particular to laminated bullet-proof glass and a preparation process thereof. The laminated bulletproof glass structurally comprises surface-treated semi-tempered glass, a PVB (Polyvinyl Butyral) film, a surface-treated semi-tempered glass, an adhesive, a polycarbonate plate, a polyurethane layer and a polycarbonate plate from top to bottom, and the laminated bulletproof glass is obtained through lamination, pre-pressing, glue injection, lamination and high-temperature treatment processes. Polyurethane is obtained by introducing polytetrahydrofuran ether glycol, isocyanate, dihydric alcohol and chlorinated phosphate, and the polyurethane is high in elasticity modulus and good in flame retardance; the polyvinyl butyral is synthesized by using the solid acid, so that the acetalization degree is high; the PVB film obtained by introducing the organic acid containing rigid groups into polyvinyl butyral molecules has high impact strength; the cured waterproof agent obtained after the adhesive is dried is good in hydrophobicity and good in light transmission; by controlling the thickness of each layer of raw material of the laminated bulletproof glass, the T95% of the laminated bulletproof glass is 395-519 DEG C, the impact strength is 1671-2112J / cm < 2 >, and the light transmittance is 81.9%-85.1%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bulletproof glass, in particular to a laminated bulletproof glass and a preparation process thereof. Background Art

[0002] Glass, as a transparent ceramic-like material, has attracted the attention of military scientists and technicians. Bulletproof glass has a bulletproof effect, but ordinary glass has poor compressive strength and tensile strength. In addition, it cannot withstand high-speed impact of materials, so ordinary glass cannot be used directly as bulletproof glass. Bulletproof glass is generally a polycarbonate material layer sandwiched between ordinary glass layers. Compared with traditional bulletproof glass, bulletproof glass with a laminated layer has a lower surface density than traditional bulletproof glass, and at the same time has a better bulletproof effect, providing a certain degree of protection against small arms shooting. The bullet shot at the bulletproof glass will penetrate the surface glass, and the polycarbonate material layer absorbs the energy of the bullet shooting. The bullet is deflected by the interlayer and finally shot at the rear glass; at the same time, the laminated bulletproof glass also has the appearance of ordinary glass and good light transmittance.

[0003] However, there are still many problems in the production raw materials and final performance of laminated bulletproof glass in the prior art. The first aspect is the colloid in the interlayer of laminated bulletproof glass, among which the more widely used materials include polyvinyl butyral (PVB) film, polycarbonate and polyurethane. PVB film is used for laminated bulletproof glass. When the outermost layer of glass is penetrated by a bullet, only irregular radial cracks will be formed at the impact point, and the glass fragments will still be firmly adhered to the PVB intermediate film, which can prevent the glass from splashing and falling off to cause secondary damage to the surrounding environment and human body. In addition, it can continue to be used without affecting the field of vision. Chinese patent CN201611121206.5 discloses "a polyvinyl butyral film and its preparation method", and the obtained PVB film is suitable for making the interlayer of laminated glass.

[0004] The second aspect is the final performance of the product. In order to improve the bulletproof performance of bulletproof glass, it is usually chosen to increase the thickness of the glass and stack multiple layers of materials. However, the total thickness of the obtained laminated bulletproof glass is too thick or the weight is too heavy, otherwise the bulletproof performance and impact resistance of the bulletproof glass cannot be guaranteed. Chinese patent CN202010340084.9 discloses "an impact-resistant high-strength bulletproof glass and its preparation method". The bulletproof glass is obtained by stacking five layers of materials, rolling, steaming and other steps. The overall self-weight of the bulletproof glass of this invention can be reduced by about 20%-30%, while the impact resistance and bulletproof performance remain unchanged.

[0005] To further improve the bulletproof effect, adhesives are used in the interlayer to strengthen the close connection between glass and various components. Chinese patent CN201410654839.7 "A light bulletproof glass and its preparation method" uses polyurethane glue to bond glass and polycarbonate plates, taking advantage of the flexibility and penetration resistance of the glue after curing, solving the problem that traditional bulletproof glass is thick and heavy and has low light transmittance, while also having a waterproof effect. In addition, with the gradual increase in the performance requirements for bulletproof glass, flame retardancy, aging resistance and other properties are also issues that need to be considered in the preparation of bulletproof glass.

[0006] Therefore, a laminated bulletproof glass and a preparation process thereof are proposed. Summary of the invention

[0007] The invention aims to provide a laminated bulletproof glass and a preparation process thereof. The invention comprises the following steps: polytetramethylene glycol is covalently bonded with two molecules of isocyanate, two ends of the two molecules of isocyanate are connected with two molecules of diol, and the diol is respectively connected with chlorophosphate to obtain polyurethane, the polyurethane has good elasticity and flame retardancy and is suitable for being used as an interlayer of the bulletproof glass; polyvinyl butyral is synthesized by using solid acid, the polyvinyl butyral obtained has high acetalization degree, and the production efficiency is improved; organic acid containing rigid groups is introduced into polyvinyl butyral molecules, and a plasticizer and a viscosity regulator are added to obtain a PVB film with high impact strength; an aqueous solution obtained by synthesizing an adhesive and then curing has good light transmittance and good waterproofness; the material prepared by the above process is used as an interlayer of the laminated bulletproof glass, the thickness of the semi-tempered glass, the above material and the polycarbonate plate is controlled within a reasonable range, and the semi-tempered glass, the above material and the polycarbonate plate are controlled to be arranged in a reasonable order, so that the laminated bulletproof glass obtained has good heat resistance, high impact strength, high glass strength, good transparency and good waterproofness.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] In one aspect, the present invention provides a process for preparing a laminated bulletproof glass, characterized in that it comprises the following steps:

[0010] Using a surface treatment agent to soak and dry the semi-tempered glass to obtain the surface-treated semi-tempered glass; in the order of the surface-treated semi-tempered glass, the PVB film and the surface-treated semi-tempered glass, push them into a dustproof room for lamination and bonding to obtain laminated glass; the laminated glass is pre-pressed to obtain a bullet-proof glass precursor 1; in the order of the polycarbonate plate, the polyurethane layer and the polycarbonate plate, the laminates are pre-pressed to obtain a bullet-proof glass precursor 2; brackets are placed at the four corners of the bullet-proof glass precursor 1, and the bullet-proof glass precursor 2 is placed above the bracket to obtain a bullet-proof glass intermediate; the layer where the bracket is located forms a space gap; the bullet-proof glass intermediate is placed vertically on the ground, wrapped with a rubber strip, an adhesive is injected into the space gap, vacuumed, cured and sealed to obtain a laminated bullet-proof glass intermediate; the laminated bullet-proof glass intermediate is placed in an autoclave, heated, kept and cooled to obtain a laminated bullet-proof glass;

[0011] The thickness of the surface treated semi-tempered glass is 0-12 mm, the thickness of the PVB film is 0.73-1.70 mm, the thickness of the polycarbonate plate is 0-2.4 mm, and the thickness of the polyurethane layer is 0.86-2.15 mm;

[0012] The polyurethane layer contains polyether polyol, isocyanate, polytetramethylene ether glycol, diol and 0-0.28 mol chlorophosphate;

[0013] The PVB film contains a solid catalyst, an emulsifier, PVB, n-butyraldehyde, an organic acid, a plasticizer and a viscosity regulator;

[0014] The adhesive contains 0.42-0.49 mol of bis(4-hydroxyphenyl)chlorophosphate and 0.6-0.9 mol of silicone oil.

[0015] Preferably, the preparation method of the polyurethane layer is as follows: drying the polyether polyol under vacuum conditions for 48 hours to remove moisture, dissolving 0.2 mol of the isocyanate in 50 mL of DMF to obtain an isocyanate solution; weighing 0.12 mol of the polytetrahydrofuran ether diol in a three-necked flask, adding the isocyanate solution to the three-necked flask under stirring to obtain a mixture; adding 150 μL of an organic tin catalyst to the mixture, controlling the reaction temperature to 80° C. and reacting for 2 hours to obtain an intermediate product 1; cooling the intermediate product 1 to 60° C., adding 0.22 mol of the diol is reacted for 2 hours, and after the reaction is complete, 25 mL of DMF is added for viscosity dilution to obtain intermediate product 2; 0.1 mol of triethylamine is added to the intermediate product 2 and stirred evenly to obtain the reactant; then 0.18-0.28 mol of the chlorophosphate is added dropwise to the reactant, refluxed and condensed at 60° C. for 6 hours, filtered, the precipitate is washed with deionized water 3 times, the organic phase is collected and dried with anhydrous sodium sulfate, and finally vacuum dried to obtain polyurethane; the polyurethane is put into an extruder and extruded to obtain the polyurethane layer.

[0016] Preferably, the isocyanate is any one of 4,4-diisocyanate dicyclohexylmethane, 1-isocyanate-4-[(4-isocyanate cyclohexyl)methyl]-2-methylcyclohexane, 3,12-diisocyanato-2,13-dimethyltetradecane, hexamethylene diisocyanate and isophorone diisocyanate.

[0017] Preferably, the diol is any one of polypropylene glycol 2000, polypropylene glycol 400, cis-1,2-dihydroxymethylethylene, 1,4-butanediol and cis,cis-2,4-hexadiene-1,6-diol.

[0018] Preferably, the chlorophosphate is any one of diphenyl chlorophosphate, phenyl phosphoryl chloride and phosphoryl chloride, di-1-naphthyl ester (9Cl).

[0019] Preferably, the preparation method of the PVB film is as follows: the washed and dried peanut shells are crushed using a crusher and passed through a 60-mesh sieve to obtain shell powder; 70 parts of the shell powder, 0-40 parts of carbon nanotubes and 5 parts of TNWDIS are mixed evenly in deionized water to obtain carbon liquid; the carbon liquid is placed in a tube furnace for carbonization at 500° C. for 3 hours to obtain carbon powder; the carbon powder is placed in concentrated sulfuric acid for 17 hours for sulfonation to obtain a powder to be washed, and the soaking temperature is 135-175° C.; the powder to be washed is washed to neutrality and dried to obtain the solid catalyst;

[0020] Accurately weigh 5.0 parts of polyvinyl alcohol into a four-necked flask, add 100 mL of 90% ethanol aqueous solution, and add 0.01 parts of the emulsifier and 0-0.8 parts of the PVB, and obtain a uniform solution under stirring at 90° C.; after the uniform solution is cooled to 30° C., 0.65-1.50 parts of the solid catalyst and 11.0-14.0 parts of the n-butyraldehyde are added to obtain a reaction liquid; the reaction liquid is heated to 60-100° C. and reacted for 15 hours to obtain a product; 0-44.9 parts of the organic acid are added to the product, and the reaction is continued for 1 hour to obtain a PVB resin;

[0021] The plasticizer and the PVB resin are uniformly mixed in a mass ratio of 1:4, and 4 wt % of the viscosity modifier is added and mixed to obtain a mixed material; the mixed material is put into an extruder and extruded to obtain the PVB film; the inlet temperature of the extruder is 50° C. and the outlet temperature is 170° C.

[0022] Preferably, the emulsifier is any one of sodium dioctyl sulfosuccinate and sodium dibutylnaphthalene sulfonate; the organic acid is any one of 2-methylcyclopropanecarboxylic acid, 3-oxocyclobutanecarboxylic acid, cyclohexanecarboxylic acid, rosin acid, 1-adamantaneacetic acid and chenodeoxycholic acid; the plasticizer is any one of triethyl acetyl citrate, tributyl acetyl citrate and epoxy soybean oil; the viscosity modifier is any one of povidone, methyl cellulose and polyvinyl alcohol.

[0023] Preferably, the preparation method of the adhesive is as follows: adding 0.40-0.49 mol of the bis(4-hydroxyphenyl)chlorophosphate to the reactant to obtain hydroxy polyurethane; uniformly mixing the hydroxy polyurethane with the product to obtain mixture one; adding 0.6-0.9 mol of the silicone oil and 0.02 mol of polyvidone to the mixture one to obtain mixture two; stirring the mixture two at 75° C. for 15 hours, and washing and drying to obtain the adhesive;

[0024] The raw materials of the reactants include: the polyether polyol, 0.2 mol hexamethylene diisocyanate, 0.12 mol polytetramethylene ether diol, and 0.22 mol polypropylene glycol 2000;

[0025] The product comprises: 1.50 parts of the solid catalyst, sodium diisooctyl sulfosuccinate and 14 parts of n-butyraldehyde obtained by soaking 25 parts of carbon nanotubes as raw materials at 155°C;

[0026] The adhesive is dried to obtain a cured waterproofing agent.

[0027] Preferably, the silicone oil is any one of carboxyl-terminated silicone oil and polydimethylsiloxane; the surface treatment agent is any one of anhydrous ethanol, 3% sulfuric acid, 5% sodium hydroxide and toluene.

[0028] On the other hand, the present invention provides a laminated bulletproof glass, characterized in that: the laminated bulletproof glass is composed of the surface treated semi-tempered glass, the PVB film, the polycarbonate board, the adhesive and the polyurethane layer; the structure of the laminated bulletproof glass is the surface treated semi-tempered glass, the PVB film, the surface treated semi-tempered glass, the adhesive, the polycarbonate board, the polyurethane layer and the polycarbonate board from top to bottom; the laminated bulletproof glass is prepared by the preparation process according to any one of claims 1 to 9; the elastic modulus of the polyurethane is 38-163MPa, and the LOI value is 19.5%-36.5%; the acetal degree of the PVB resin is 72.9%-83.1%; the impact strength of the PVB film is 481.1-546.8J / cm 2 The water contact angle of the cured waterproofing agent is 113°-129°, and the light transmittance is 82.1%-92.5%; the laminated bulletproof glass T 95% The temperature is 395-519℃, and the impact strength is 1671-2112J / cm 2 , the light transmittance is 81.9%-85.1%.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1. The present invention combines polytetramethylene glycol with two molecules of isocyanate by covalent bonds, and the two ends of the two molecules of isocyanate are connected to two molecules of diol, and the diol is respectively connected to chlorophosphate to obtain polyurethane. The polyurethane contains repeated -NHCOO- groups and unsaturated double bonds, and its elastic modulus is in the range of 38-163MPa; diphenyl chlorophosphate contains benzene rings, and in addition, phosphoric acid compounds are produced during the combustion stage to prevent the combustion reaction from proceeding. The LOI value of the polyurethane is 19.5%-36.5%. The polyurethane has good elasticity and flame retardant properties, and is suitable for use as an interlayer of bulletproof glass.

[0031] 2. Peanut shell powder and carbon nanotubes are burned to obtain carbon powder, which is then sulfonated to form solid acid. The solid acid is used to catalyze the reaction of n-butyraldehyde and polyvinyl alcohol to generate polyvinyl butyral, and polyvinyl butyral is added to the reaction system in advance. The acetalization degree of the generated polyvinyl butyral is in the range of 72.9%-83.1%. On the one hand, the use of organic acids such as hydrochloric acid to corrode equipment is avoided, and on the other hand, the acetalization degree is increased, which indirectly reduces production costs and improves production efficiency.

[0032] 3. By introducing an organic acid containing a rigid group into the polyvinyl butyral molecule, the amount of organic acid added is controlled within the range of 11.5-44.9 parts, and the type of plasticizer and viscosity modifier are controlled during the preparation of the PVB film. The impact strength of the resulting PVB film is 481.1-546.8 J / cm 2 The obtained PVB film can be applied to laminated bulletproof glass. After the bullet breaks through the glass layer, some glass fragments enter the PVB film. The bullet deforms after passing through the PVB film, and the kinetic energy of the bullet is consumed, which plays a role of toughening and buffering.

[0033] 4. Bis(4-hydroxyphenyl) chlorophosphate is introduced to prepare polyurethane, and the carboxyl-terminated silicone oil is connected to the hydroxyl groups in the polyurethane and the hydroxyl groups in polyvinyl butyral through the carboxyl groups at both ends of the molecule to obtain an adhesive, which is then cured to obtain a waterproofing agent. The obtained waterproofing agent has a water contact angle in the range of 113°-129° and good hydrophobicity; the light transmittance of the waterproofing agent is in the range of 82.1%-92.5%, and good light transmittance.

[0034] 5. According to the order of surface treated semi-tempered glass, PVB film, surface treated semi-tempered glass, polycarbonate board, polyurethane layer and polycarbonate board, stack, combine and press the sheets, inject adhesive into the space formed between the surface treated semi-tempered glass and the polycarbonate board and cure, and finally react in an autoclave to obtain a laminated bulletproof glass. The thickness of the surface treated semi-tempered glass is controlled to be 5-12mm, the thickness of the PVB film is 0.73-1.70mm, the thickness of the polycarbonate board is 0-4.8mm, and the thickness of the polyurethane layer is 0.86-2.15mm. The test results of the obtained laminated bulletproof glass T A show that T 95% In the range of 395-519℃, the impact strength is 1671-2112J / cm 2 The range of light transmittance is 81.9%-85.1%; by controlling the different reagents for treating the semi-tempered glass, the peel strength of the obtained laminated bulletproof glass is in the range of 386-435MPa. Laminated bulletproof glass has good heat resistance, high impact strength, high glass strength, good transparency and good waterproofness. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a graph showing the test results of thermal gravimetric analysis of laminated bulletproof glass of Examples 45-49 of the present invention;

[0036] Figure 2 This is a graph showing the peel strength results of the laminated bulletproof glass of Examples 51-54 of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] See also Figure 1 to Figure 2 The present invention provides a laminated bulletproof glass and a preparation process thereof, and the technical scheme is as follows:

[0039] The material information used in the examples is as follows:

[0040] 4,4-diisocyanatodicyclohexylmethane CAS No. 5124-30-1; 1-isocyanato-4-[(4-isocyanatocyclohexyl)methyl]-2-methylcyclohexane CAS No. 91458-04-7; 3,12-diisocyanato-2,13-dimethyltetradecane CAS No. 101410-84-8; Hexamethylene diisocyanate CAS No. 822-06-0; Isophorone diisocyanate CAS No. 4098-71-9; Cis-1,2-dihydroxymethylethylene CAS No. 6117-80-2; 1,4-Butanediol CAS No. 110-63-4; Cis, cis-2,4-hexadiene-1,6-diol CAS No. 63621-96-5;

[0041] Carboxyl-terminated silicone oil (PDMS-COOH2) was purchased from Gelest, USA, with analytical grade and a viscosity of 30 mPa·s at 25°C.

[0042] Diphenyl chlorophosphate CAS No. 2524-64-3; Phosphorus oxychloride, di-1-naphthyl ester (9Cl) CAS No. 38330-00-6; Bis (4-hydroxyphenyl) chlorophosphate CAS No. 1287268-11-4;

[0043] Sodium dibutylnaphthalene sulfonate CAS No. 25417-20-3; 2-methylcyclopropanecarboxylic acid CAS No. 29555-02-0; 3-oxocyclobutanecarboxylic acid CAS No. 23761-23-1; cyclohexanecarboxylic acid CAS No. 98-89-5; rosin acid CAS No. 514-10-3; 1-adamantaneacetic acid CAS No. 4942-47-6; chenodeoxycholic acid CAS No. 474-25-9.

[0044] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0045] Example 1

[0046] The polyether polyol was dried under vacuum conditions for 48 hours to remove moisture, and 0.2 mol of isocyanate was dissolved in 50 mL of DMF to obtain an isocyanate solution; 0.12 mol of polytetrahydrofuran ether diol (relative molecular weight of 3000) was weighed in a three-necked flask, and the isocyanate solution was added to the three-necked flask under stirring to obtain a mixture; 150 μL of organotin was added to the mixture as a catalyst, and the reaction temperature was controlled to be 80° C. for reaction for 2 hours to obtain an intermediate product 1; the intermediate product 1 was cooled to 60° C., and 0.22 mol of diol was added to react for 2 hours, and after the reaction was complete, 25 mL of DMF was added for viscosity dilution to obtain an intermediate product 2; 0.1 mol of triethylamine was added to the intermediate product 2 and stirred evenly to obtain a product to be reacted; then 0.21 mol of chlorophosphate was added dropwise to the product to be reacted, refluxed and condensed at 60° C. for 6 hours, filtered, the precipitate was washed with deionized water 3 times, the organic phase was collected and dried with anhydrous sodium sulfate, and finally vacuum dried to obtain a polyurethane; the polyurethane was put into an extruder and extruded to obtain a polyurethane layer.

[0047] Example 2-13

[0048] Different from Example 1, the following preparation conditions are changed, as shown in Table 1.

[0049] Table 1 Changes in conditions during polyurethane preparation

[0050]

[0051]

[0052] Examples 12-13

[0053] The difference from Example 4 is that the chlorophosphates are phenylphosphoryl chloride, phosphoryl chloride, and di-1-naphthyl ester (9Cl).

[0054] Comparative Example 1

[0055] The difference from Example 4 is that the added amount of diphenyl chlorophosphate is 0 mol.

[0056] Comparative Example 2

[0057] The difference from Example 4 is that the diol is polypropylene glycol 400.

[0058] Embodiment 14

[0059] The polyurethanes prepared in Examples 1-13 and Comparative Examples 1-2 were tested for elasticity and fire resistance. The polymers were tested for mechanical properties using an intelligent electronic universal testing machine at a test speed of 300 mm / min. The fire resistance test was performed in accordance with GB / T2406-2009 Method for Determining Combustion Behavior of Plastics by Oxygen Index Method Part 2: Method for Room Temperature Test, and the limiting oxygen index (LOI) of the samples was tested using a YZS-8A oxygen index analyzer. The results are recorded in Table 2.

[0060] Table 2 Test results of aging performance and fire resistance of polyurethane

[0061]

[0062]

[0063] The elastic modulus of the polyurethane prepared by the present invention is between 38 and 163 MPa. The elastic modulus of Examples 1-5 is in the range of 71-142 MPa, wherein the elastic modulus of the polyurethane obtained in Example 4 is the highest at 142 MPa; compared with Example 4, the elastic modulus of the isocyanate in Example 3 is reduced due to the presence of a branched structure; the elasticity of the polyurethane obtained in Example 1 is lower than that of Examples 3 and 4, and the elasticity of the polyurethane obtained in Example 2 is the lowest among Examples 1-5. Compared with linear aliphatic isocyanates, the isocyanate structures in Examples 1, 2, and 5 are different, the strength is higher than the structure of the aforementioned substance, and the hard segment content is increased, resulting in increased brittleness and decreased elastic modulus of the prepared polyurethane; the elasticity of the polyurethane obtained in Examples 6-8 increases with the increase in the number of unsaturated double bonds in the diol; in Examples 9-11, the same type of isocyanate is added, and in the case of differences in the type and content of other substances added, the elastic modulus is between 138 and 141 MPa, with a small range of variation; compared with Example 4, the type of chlorophosphate in Example 12 changes, and the corresponding elastic modulus is increased and decreased respectively compared with Example 1. When the diol in Comparative Example 2 is polypropylene glycol 400, the elastic modulus decreases.

[0064] The LOI value of the obtained polyurethane is in the range of 19.5%-36.5%. The addition amount of diphenyl chlorophosphate in Examples 1-8 is the same, so the limiting oxygen index remains basically unchanged; compared with Example 4, in Examples 9-11, as the addition amount of diphenyl chlorophosphate decreases, the limiting oxygen index decreases and the flame retardant performance decreases; the addition amount of diphenyl chlorophosphate increases, and the flame retardancy improves. As shown in Example 9, the LOI value can reach up to 36.5%, and the matrix produces phosphoric acid compounds in the early pyrolysis, which can promote the formation of a protective carbon layer to protect the internal matrix from further combustion; after diphenyl chlorophosphate is replaced with phenyl phosphoryl chloride in Example 12, the flame retardant performance decreases, and the addition of benzene rings is beneficial to the improvement of the heat resistance and flame retardant performance of polyurethane; compared with Example 4, more unsaturated double bonds are introduced into the polyurethane of Example 13, so the flame retardant performance decreases. In Comparative Example 1, no diphenyl chlorophosphate is added, and the material cannot prevent the combustion process from proceeding.

[0065] Examples 15-25

[0066] The washed and dried peanut shells were crushed with a crusher and passed through a 60-mesh sieve to obtain shell powder; 70 parts of shell powder, 30 parts of carbon nanotubes and 5 parts of TNWDIS were mixed evenly in 200 mL of deionized water to obtain carbon liquid; under nitrogen protection, the carbon liquid was placed in a tube furnace for carbonization at 500°C for 3 hours to obtain carbon powder; the powder was immersed in concentrated sulfuric acid for 17 hours for sulfonation to obtain a powder to be washed, and the immersion temperature was 155°C; the powder to be washed was washed to neutrality and dried to obtain a solid catalyst;

[0067] Accurately weigh 5.0 parts of PVA into a four-necked flask, add 100 mL of 90% ethanol aqueous solution, and add 0.01 parts of emulsifier and 0.8 parts of PVB, and obtain a uniform solution under stirring at 90°C; after the uniform solution is cooled to 30°C, 1.28 parts of solid catalyst and 11.0 parts of n-butyraldehyde are added to obtain a reaction solution; the reaction solution is heated to 60°C and reacted for 15 hours to obtain a product; 44.9 parts of chenodeoxycholic acid are added to the product, and the reaction is continued for 1 hour to obtain a PVB resin;

[0068] Tributyl acetyl citrate and PVB resin are added in a mass ratio of 1:4, and 4 wt % of polyvidone is added and mixed to obtain a mixture, and the mixture is put into an extruder for extrusion to obtain a PVB film; the inlet temperature of the extruder is 50° C., and the outlet temperature is 170° C.

[0069] The material information and preparation conditions involved in the preparation of PVB resin are shown in Table 3.

[0070] Table 3 Preparation conditions of PVB resin

[0071]

[0072] Embodiment 25

[0073] Different from Example 18, the immersion time of carbon powder in concentrated sulfuric acid is 15 hours, and the amount of PVB added is 1.28 parts.

[0074] Comparative Example 3

[0075] The difference from Example 18 is that the amount of carbon nanotubes added is 0 parts, the amount of PVB added is 0 parts, and the reaction solution is heated to 100° C. and reacted for 15 hours to obtain the product.

[0076] Embodiment 26

[0077] The acetalization rate of the PVB resins prepared in Examples 15-25 and Comparative Example 3 was tested. The acetalization rate was determined using the hydroxylamine hydrochloride method, and the test results are recorded in Table 4.

[0078] Table 4 PVB resin acetal degree test results

[0079]

[0080]

[0081] The acetal degree of PVB resin is in the range of 72.9%-83.1%. In Examples 15-18, as the amount of carbon nanotubes added increases, the acetal degree shows a trend of gradually increasing. This is because carbon nanotubes have an adsorption effect. After the shell powder is attached to its surface and cavity and then sulfonated, the specific surface area of ​​the obtained solid catalyst increases. The products generated in the primary reaction stage are evenly dispersed on the surface of the solid catalyst, which does not affect the subsequent further reaction of PVA and butyraldehyde, so the acetal degree increases; but considering factors such as cost, the amount of carbon nanotubes added is selected to be 25 parts; Comparison of the test results of Examples 19 and 20 shows that the acetal degree decreases when the immersion temperature is 175°C. This may be because too high a sulfonation temperature will cause the pore structure of the carbon powder to be destroyed, resulting in a reduction in the number of positions on which the sulfonic acid groups can be bonded; when immersed at 135°C, the acetal degree also decreases; Comparison of the results of Examples 18, 21 and 22 shows that when the emulsifier is sodium dioctyl sulfosuccinate, the acetalization degree is the highest; compared with the results of Example 18, it can be seen that too low or too high an amount of solid catalyst added in Examples 23 and 24 is not conducive to the reaction; compared with Example 18, the acetalization degree of the PVB resin obtained when the immersion time of carbon powder in concentrated sulfuric acid is 15h and the amount of PVB added is 1.28 parts is reduced; the acetalization degree of Comparative Example 3 is the lowest compared with the examples, which is because no carbon nanotubes are added and no PVB is added to the raw materials, resulting in the initial generation of PVB agglomeration, and n-butyraldehyde cannot react further; and the reaction temperature is too high, the reverse reaction rate of the acetalization reaction is accelerated, and the influence of side reactions reduces the acetalization degree of the PVB resin

[0082] Examples 27-36

[0083] The washed and dried peanut shells were crushed with a crusher and passed through a 60-mesh sieve to obtain shell powder; 70 parts of carbon powder, 25 parts of carbon nanotubes and 5 parts of TNWDIS were mixed evenly in 200 mL of deionized water to obtain carbon liquid; under nitrogen protection, the carbon liquid was placed in a tube furnace for carbonization at 500° C. for 3 h to obtain carbon powder; the powder was immersed in concentrated sulfuric acid for 17 h for sulfonation to obtain a powder to be washed, and the immersion temperature was 155° C.; the powder to be washed was washed to neutrality and dried to obtain a solid catalyst;

[0084] Accurately weigh 5.0 parts of PVA into a four-necked flask, add 100 mL of 90% ethanol aqueous solution, and add 0.01 parts of sodium diisooctyl sulfosuccinate and 0.8 parts of PVB, and obtain a uniform solution under stirring at 90° C.; after the uniform solution is cooled to 30° C., 1.35 parts of a solid catalyst and 11.0 parts of n-butyraldehyde are added to obtain a reaction solution; the reaction solution is heated to 60° C. and reacted for 15 hours to obtain a product; 11.5 parts to 44.9 parts of an organic acid are added to the product, and the reaction is continued for 1 hour to obtain a PVB resin;

[0085] The plasticizer and the PVB resin are added in a mass ratio of 1:4, and 4 wt % of a viscosity modifier is added and mixed to obtain a mixed material, and the mixed material is put into an extruder for extrusion to obtain a PVB film; the inlet temperature of the extruder is 50° C., and the outlet temperature is 170° C.

[0086] The detailed information in the preparation process of the present invention is shown in Table 5.

[0087] Embodiment 37

[0088] The PVB films prepared in Examples 27-36 and Comparative Example 4 were subjected to mechanical property tests. The polymers were subjected to mechanical property tests using a Zhiqu electronic universal testing machine at a test speed of 300 mm / min. The test results are shown in Table 5.

[0089] The test results show that the impact strength of the PVB film prepared in the embodiment is 481.1-546.8 J / cm 2 The impact strength is high because the hydroxyl groups on the main chain of PVE can react with organic acid to remove a molecule of water to form a PVB resin with an organic acid structure. In Examples 27-29, as the organic acid structure changes from a three-membered ring and a four-membered ring to a six-membered ring, the mechanical properties gradually improve and the impact strength increases. In Examples 29-32, the PVB resin obtained by using chenodeoxycholic acid as an organic acid in Example 32 has the highest impact strength of 546.8 J / cm 2; Therefore, no organic acid is added in Comparative Example 4, and the impact strength of the obtained PVB resin is the worst. The test results of Examples 32-34 show that, when the addition amount is the same, the plasticizing effect of acetyl tributyl citrate as a plasticizer is better than that of acetyl triethyl citrate and epoxy soybean oil, and the side chain length of acetyl tributyl citrate is better than that of acetyl triethyl citrate, which can achieve a better plasticizing effect; due to the presence of more epoxy groups in epoxy soybean oil, it is unstable during the subsequent high-temperature extrusion process, resulting in a decrease in the impact strength of the final PVB resin. Comparison of the results of Example 32 with those of Examples 35 and 36 shows that the PVB resin obtained by using polyvidone as a viscosity regulator has higher impact strength and good mechanical properties. Overall, the PVB film prepared by the present invention has good mechanical properties. When the bullet breaks through the glass layer, part of the glass debris enters the PVB film, and the bullet is deformed after passing through the PVB film. At the same time, the kinetic energy of the bullet is consumed, which plays a role of toughening and buffering, and is suitable for the application of materials in bulletproof glass interlayers.

[0090] Table 5

[0091]

[0092]

[0093] Embodiment 38

[0094] The polyether polyol was dried under vacuum for 48 hours to remove moisture, 0.2 mol of hexamethylene diisocyanate was dissolved in 50 mL of DMF to obtain an isocyanate solution; 0.12 mol of polytetrahydrofuran ether diol (relative molecular weight of 3000) was weighed in a three-necked flask, and the isocyanate solution was added to the three-necked flask under stirring to obtain a mixture; 150 μL of organotin was added to the mixture as a catalyst, and the reaction temperature was controlled to 80° C. for 2 hours to obtain an intermediate product 1; the intermediate product 1 was cooled to 6 0℃, and add 0.22mol of polypropylene glycol 2000 to react for 2h, after the reaction is complete, add 25mL of DMF to dilute the viscosity to obtain intermediate product 2; add 0.1mol of triethylamine to intermediate product 2 and stir evenly to obtain the reactant; then add 0.40mol of bis(4-hydroxyphenyl)chlorophosphate dropwise to the reactant, reflux condensation at 60℃ for 6h, filter, wash the precipitate with deionized water 3 times, collect the organic phase and dry it with anhydrous sodium sulfate, and finally dry it in vacuum to obtain hydroxy polyurethane;

[0095] 0.45 mol of the product prepared in Example 24 was evenly mixed with the hydroxy polyurethane to obtain mixture one; 0.45 mol of terminal carboxyl silicone oil and 0.02 mol of polyvidone were added to obtain mixture two; mixture two was stirred and reacted at 75°C for 15 hours, and a binder was obtained after washing and drying steps; and dried at 60°C for 10 hours to obtain a solidified waterproofing agent.

[0096] Embodiment 39

[0097] The difference from Example 38 is that the amount of bis(4-hydroxyphenyl)chlorophosphate added is 0.42 mol.

[0098] Embodiment 40

[0099] The difference from Example 38 is that the amount of bis(4-hydroxyphenyl)chlorophosphate added is 0.49 mol.

[0100] Embodiment 41

[0101] The difference from Example 38 is that the amount of carboxyl-terminated silicone oil added is 0.60 mol.

[0102] Embodiment 42

[0103] The difference from Example 38 is that the amount of carboxyl-terminated silicone oil added is 0.70 mol.

[0104] Embodiment 43

[0105] The difference from Example 38 is that the amount of carboxyl-terminated silicone oil added is 0.90 mol.

[0106] Comparative Example 5

[0107] The difference from Example 38 is that bis(4-hydroxyphenyl)chlorophosphate is replaced by diphenylchlorophosphate.

[0108] Comparative Example 6

[0109] The difference from Example 38 is that the carboxyl-terminated silicone oil is replaced by PDMS.

[0110] Embodiment 44

[0111] The waterproofing agents prepared in Examples 38-43 and Comparative Examples 5 and 6 were tested for light transmittance and waterproof performance. Since the waterproofing agent is used in bulletproof glass, it needs to have good light transmittance to meet the needs of actual use; the light transmittance of the waterproofing agent was tested using an HCTG-A light transmittance meter. At room temperature, 5 locations on the surface of the cured waterproofing agent were randomly selected for testing, each droplet volume was 3 μL, and the water contact angle obtained from the test was averaged. The test structures for light transmittance and waterproof performance are recorded in Table 6.

[0112] Table 6 Transmittance and waterproof performance test results

[0113] Group Water contact angle Light transmittance Embodiment 38 113° 91.4% Embodiment 39 114° 92.0% Embodiment 40 117° 92.5% Embodiment 41 122° 90.3% Embodiment 42 126° 89.4% Embodiment 43 129° 88.0% Comparative Example 5 115° 84.8% Comparative Example 6 114° 82.1%

[0114] The water contact angle of the water-proofing agent for curing prepared by the present invention is in the range of 113 ° -129 °, and has good hydrophobicity. Among them, in embodiment 38-40, with the increase of bis (4-hydroxyphenyl) chlorophosphate addition, hydrophobicity is slightly improved, and this is because silane has low surface energy, and when the addition of terminal carboxyl silicone oil is fixed, the amount of bis (4-hydroxyphenyl) chlorophosphate increases, and the percentage occupied by benzene ring in the system also increases, so hydrophobicity improves. The result comparison of embodiment 38 and embodiment 41-43 shows that the addition of terminal carboxyl silicone oil gradually improves hydrophobicity; this is because the two ends of the main molecular chain in the obtained polyurethane are connected with bis (4-hydroxyphenyl) chlorophosphate respectively by phosphate bond, and the hydroxyl exposed in the bis (4-hydroxyphenyl) chlorophosphate molecule reacts with the carboxyl of terminal carboxyl silicone oil, and the carboxyl of terminal carboxyl silicone oil can also react with the hydroxyl in the product, and as the amount of terminal carboxyl silicone oil introduced gradually increases, its hydrophobicity is also continuously improved.

[0115] The light transmittance of the cured waterproofing agent is in the range of 82.1%-92.5%. In Examples 38-40, the amount of bis(4-hydroxyphenyl) chlorophosphate added increases, and the light transmittance gradually increases. This is because the amount of terminal carboxyl silicone oil is constant, more bis(4-hydroxyphenyl) chlorophosphate is covalently bonded to the terminal carboxyl silicone oil, and the structure of the waterproofing agent is more uniform; in Examples 41-43, the amount of terminal carboxyl silicone oil added gradually increases, and the light transmittance is between 88.0%-90.3%; the cured waterproofing agent obtained in Comparative Example 5 has a reduced light transmittance due to the replacement of bis(4-hydroxyphenyl) chlorophosphate with diphenyl chlorophosphate, and there is no functional group in diphenyl chlorophosphate that can be covalently bonded to the terminal carboxyl silicone oil, so the uniformity of the system decreases and the light transmittance decreases; the light transmittance of Comparative Example 6 is reduced after being replaced with PDMS, and the compatibility between PDMS and the three systems of polyurethane and product is reduced, so the light transmittance is the lowest, which is 82.1%. In general, the cured waterproofing agent prepared by the present invention has good light transmittance and is applied to the interlayer of bullet-proof glass. It can not only ensure the transparent effect, but also has waterproof properties, preventing water from entering the interlayer, and avoiding water from affecting the polyurethane layer, PVB film and polycarbonate layer, thereby affecting the overall bulletproof effect of the bullet-proof glass.

[0116] Embodiment 45

[0117] The semi-tempered glass is cut and trimmed, and then soaked in anhydrous ethanol at room temperature for 2 hours, cleaned and dried to obtain surface-treated semi-tempered glass; the surface-treated semi-tempered glass, PVB film and surface-treated semi-tempered glass are pushed into a dustproof room in the order of stacking and combining to obtain laminated glass, and the humidity of the dustproof room is maintained at 30%-50%, and the temperature is 18°C-25°C; the laminated glass is placed on a flat press and pre-pressed at 95°C to obtain a bulletproof glass precursor 1; the polycarbonate plate, the polyurethane layer and the polycarbonate plate are stacked in sequence, and the bulletproof glass precursor 2 is obtained after pre-pressing; brackets are placed at the four corners of the bulletproof glass precursor 1, and the height of the brackets is 100°C. The thickness is 2mm, and a bullet-proof glass precursor 2 is placed on the bracket for lamination to obtain a bullet-proof glass intermediate; a space gap is formed in the bullet-proof glass intermediate due to the action of the bracket; the bullet-proof glass intermediate is placed vertically, and after lamination, the entire body is wrapped with a rubber strip, and then the adhesive prepared according to the method of Example 43 is injected into the space gap, the bracket is removed, vacuum is applied to remove the air in the space gap, and the adhesive is cured at 60°C, and sealed to obtain a laminated bullet-proof glass intermediate; the laminated bullet-proof glass intermediate is placed in an autoclave, the initial temperature is set to 50°C, the temperature is raised to 130°C after 3 hours, and the temperature is lowered to 60°C after 2.5 hours of heat preservation to obtain a laminated bullet-proof glass.

[0118] The thickness of the surface treated semi-tempered glass is 5mm, the thickness of the PVB film is 0.73mm, the thickness of the polycarbonate plate is 2.2mm, and the thickness of the polyurethane layer is 0.62mm.

[0119] Different from Example 45, the following preparation conditions are changed, as shown in Table 7.

[0120] Table 7 Changes in conditions during the preparation of laminated bulletproof glass

[0121]

[0122]

[0123] Comparative Example 9

[0124] Different from Example 51, the bullet-proof glass precursor one and the bullet-proof glass precursor two are directly stacked, pre-pressed and finally placed in an autoclave to obtain a laminated bullet-proof glass; that is, no space gap is formed between the bullet-proof glass precursor one and the bullet-proof glass precursor two, and no corresponding adhesive is injected.

[0125] Embodiment 55

[0126] The laminated bulletproof glass prepared in Examples 45-54 and Comparative Examples 7-9 was tested for heat resistance, impact resistance and light transmittance. The laminated bulletproof glass obtained in Examples 51-54 was tested for peeling performance. The peeling performance test was to apply a 45° load (load rate of 5 mm / min) to the sample until the glass and the colloid peeled off, and the strength of the applied force during the peeling was recorded. The sample of the example was tested using standard equipment ER-5046-5. The test results are shown in the figure. Figure 2 As shown; the heat resistance is characterized by thermogravimetric analysis. The polymer is tested and analyzed in a nitrogen atmosphere using a Beijing Hengjiu HCT-1 thermogravimetric analyzer (TGA). The heating rate is 10°C / min and the heating range is 50-780°C. The test results are shown in Figure 1 As shown; the impact resistance is consistent with the test method of Example 37; the light transmittance test method is consistent with the method of Example 44; the test results are shown in Table 8.

[0127] Table 8 Test results of heat resistance, impact resistance and light transmittance of laminated bulletproof glass

[0128]

[0129]

[0130] Figure 1 The test results show that the T 95% The value shows a gradual trend. As the thickness of the polyurethane layer increases, the number of heat-resistant groups in the polyurethane gradually increases, so the heat-resistant effect gradually increases, T 95% The maximum value of is 526℃, as shown in Example 49; however, in Example 49, when the thickness of the polyurethane layer is 2.15mm, the glass turns yellow significantly; the laminated tempered glass prepared by the present invention has excellent heat resistance. As shown in Table 8, when the results of Example 48 are compared with those of Examples 50 and 51, the heat resistance is gradually improved due to the increase in the thickness of the PVB film, T 95% The temperature of the laminated bulletproof glass is 514-519°C. In Examples 52-54, changing the type of surface treatment agent for the semi-tempered glass has no significant effect on the heat resistance of the laminated bulletproof glass. 95% The value is reduced, which may be due to the lack of protection of the semi-tempered glass with surface treatment in the middle layer, and the heat resistance is reduced; the laminated bullet-proof glass obtained in Comparative Example 8 has good heat resistance, and Comparative Example 9 does not add adhesive, and the heat resistance effect is greatly reduced. The Si-O-Si, benzene ring and phosphate group in the adhesive provide good heat resistance for the laminated bullet-proof glass.

[0131] Figure 2The test results of the laminated bulletproof glass of Examples 51-54 are shown, and the peel strength is between 386-435MPa. The peel strength of the laminated bulletproof glass obtained by laminating the semi-tempered glass treated with anhydrous ethanol and the PVB film is the largest, as shown in Example 41; while the peel strength of the finished product obtained by the semi-tempered glass treated with 5% sodium hydroxide, 3% sulfuric acid and toluene decreases in sequence; Example 54 reduces the adhesion performance of the semi-tempered glass, so the peel strength is the lowest.

[0132] The impact strength test results show that the impact strength of the laminated bullet-proof glass prepared by the present invention is between 1671 and 2112 J / cm 2 In the range of Examples 45-49, when the thickness of other components remains unchanged, the impact strength increases with the increase of the thickness of the polyurethane layer. This is because the number of unsaturated double bonds increases, the elasticity of the system increases, and thus the impact resistance is enhanced; the results of Examples 48 and Examples 50 and 51 show that the increase of the thickness of the PVB film also increases the impact strength; the impact strength of the laminated bullet-proof glass obtained in Examples 52-54 is between 2101-2110 J / cm 2 range; Comparative Examples 7 and 8 both reduce the number of layers of the laminated bulletproof glass to 5 layers, and increase the thickness of the surface-treated semi-tempered glass and the polycarbonate plate accordingly, but the impact strength is lower than that of the embodiments. The surface-treated semi-tempered glass cooperates with the PVB film, the polycarbonate plate and the polyurethane layer to jointly improve the impact strength of the laminated bulletproof glass. The light transmittance of the laminated bulletproof glass obtained in Examples 45-54 and Comparative Examples 7 and 8 is in the range of 81.9%-85.1%, and the light transmittance is good. In summary, the laminated bulletproof glass prepared by the present invention has good transparency, heat resistance and good impact resistance.

[0133] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing laminated bulletproof glass, characterized in that: The following steps are involved: Using a surface treatment agent to soak and dry the semi-tempered glass to obtain the surface-treated semi-tempered glass; in the order of the surface-treated semi-tempered glass, the PVB film and the surface-treated semi-tempered glass, push them into a dustproof room for lamination and bonding to obtain laminated glass; the laminated glass is pre-pressed to obtain a bullet-proof glass precursor 1; in the order of the polycarbonate plate, the polyurethane layer and the polycarbonate plate, the laminates are pre-pressed to obtain a bullet-proof glass precursor 2; brackets are placed at the four corners of the bullet-proof glass precursor 1, and the bullet-proof glass precursor 2 is placed above the bracket to obtain a bullet-proof glass intermediate; the layer where the bracket is located forms a space gap; the bullet-proof glass intermediate is placed vertically on the ground, wrapped with a rubber strip, an adhesive is injected into the space gap, vacuumed, cured and sealed to obtain a laminated bullet-proof glass intermediate; the laminated bullet-proof glass intermediate is placed in an autoclave, heated, kept and cooled to obtain a laminated bullet-proof glass; The thickness of the surface treated semi-tempered glass is 0-12 mm, the thickness of the PVB film is 0.73-1.70 mm, the thickness of the polycarbonate plate is 0-2.4 mm, and the thickness of the polyurethane layer is 0.86-2.15 mm; The polyurethane layer contains polyether polyol, isocyanate, polytetramethylene ether glycol, diol and 0-0.28 mol chlorophosphate; The PVB film contains a solid catalyst, an emulsifier, PVB, n-butyraldehyde, an organic acid, a plasticizer and a viscosity regulator; The adhesive contains 0.42-0.49 mol of bis(4-hydroxyphenyl)chlorophosphate and 0.6-0.9 mol of silicone oil.

2. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The preparation method of the polyurethane layer is as follows: drying the polyether polyol under vacuum conditions for 48 hours to remove moisture, dissolving 0.2 mol of the isocyanate in 50 mL of DMF to obtain an isocyanate solution; weighing 0.12 mol of the polytetrahydrofuran ether diol in a three-necked flask, adding the isocyanate solution to the three-necked flask under stirring to obtain a mixture; adding 150 μL of an organic tin catalyst to the mixture, controlling the reaction temperature to 80° C. for 2 hours to obtain an intermediate product 1; cooling the intermediate product 1 to 60° C., adding 0. 22 mol of the diol is reacted for 2 hours. After the reaction is complete, 25 mL of DMF is added for viscosity dilution to obtain intermediate product 2; 0.1 mol of triethylamine is added to the intermediate product 2 and stirred evenly to obtain the reactant; then 0.18-0.28 mol of the chlorophosphate is added dropwise to the reactant, refluxed and condensed at 60° C. for 6 hours, filtered, the precipitate is washed with deionized water 3 times, the organic phase is collected and dried with anhydrous sodium sulfate, and finally vacuum dried to obtain polyurethane; the polyurethane is put into an extruder and extruded to obtain the polyurethane layer.

3. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The isocyanate is any one of 4,4-diisocyanate dicyclohexylmethane, 1-isocyanate-4-[(4-isocyanate cyclohexyl)methyl]-2-methylcyclohexane, 3,12-diisocyanato-2,13-dimethyltetradecane, hexamethylene diisocyanate and isophorone diisocyanate.

4. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The diol is any one of polypropylene glycol 2000, polypropylene glycol 400, cis-1,2-dihydroxymethylethylene, 1,4-butanediol and cis,cis-2,4-hexadiene-1,6-diol.

5. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The chlorophosphate ester is any one of diphenyl chlorophosphate, phenyl phosphoryl chloride and phosphoryl chloride, di-1-naphthyl ester (9Cl).

6. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The preparation method of the PVB film is as follows: the washed and dried peanut shells are crushed with a crusher and passed through a 60-mesh sieve to obtain shell powder; 70 parts of the shell powder, 0-40 parts of carbon nanotubes and 5 parts of TNWDIS are mixed evenly in deionized water to obtain carbon liquid; the carbon liquid is placed in a tube furnace for carbonization at 500° C. for 3 hours to obtain carbon powder; the carbon powder is placed in concentrated sulfuric acid for 17 hours for sulfonation to obtain a powder to be washed, and the soaking temperature is 135-175° C.; the powder to be washed is washed to neutrality and dried to obtain the solid catalyst; Accurately weigh 5.0 parts of polyvinyl alcohol into a four-necked flask, add 100 mL of 90% ethanol aqueous solution, and add 0.01 parts of the emulsifier and 0-0.8 parts of the PVB, and obtain a uniform solution under stirring at 90° C.; after the uniform solution is cooled to 30° C., 0.65-1.50 parts of the solid catalyst and 11.0-14.0 parts of the n-butyraldehyde are added to obtain a reaction liquid; the reaction liquid is heated to 60-100° C. and reacted for 15 hours to obtain a product; 0-44.9 parts of the organic acid are added to the product, and the reaction is continued for 1 hour to obtain a PVB resin; The plasticizer and the PVB resin are uniformly mixed in a mass ratio of 1:4, and 4 wt % of the viscosity modifier is added and mixed to obtain a mixed material; the mixed material is put into an extruder and extruded to obtain the PVB film; the inlet temperature of the extruder is 50° C. and the outlet temperature is 170° C.

7. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The emulsifier is any one of sodium dioctyl sulfosuccinate and sodium dibutylnaphthalene sulfonate; the organic acid is any one of 2-methylcyclopropanecarboxylic acid, 3-oxocyclobutanecarboxylic acid, cyclohexanecarboxylic acid, rosin acid, 1-adamantaneacetic acid and chenodeoxycholic acid; the plasticizer is any one of triethyl acetyl citrate, tributyl acetyl citrate and epoxy soybean oil; the viscosity modifier is any one of povidone, methyl cellulose and polyvinyl alcohol.

8. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The preparation method of the adhesive is as follows: adding 0.40-0.49 mol of the bis(4-hydroxyphenyl) chlorophosphate to the reactant to obtain hydroxy polyurethane; uniformly mixing the hydroxy polyurethane with the product to obtain a mixture one; adding 0.6-0.9 mol of the silicone oil and 0.02 mol of polyvidone to the mixture one to obtain a mixture two; stirring the mixture two at 75° C. for 15 hours, and washing and drying to obtain the adhesive; The raw materials of the reactants include: the polyether polyol, 0.2 mol hexamethylene diisocyanate, 0.12 mol polytetramethylene ether diol, and 0.22 mol polypropylene glycol 2000; The product comprises: 1.50 parts of the solid catalyst, sodium diisooctyl sulfosuccinate and 14 parts of n-butyraldehyde obtained by soaking 25 parts of carbon nanotubes as raw materials at 155°C; The adhesive is dried to obtain a cured waterproofing agent.

9. The process for preparing a laminated bulletproof glass according to claim 1, characterized in that: The silicone oil is any one of carboxyl-terminated silicone oil and polydimethylsiloxane; the surface treatment agent is any one of anhydrous ethanol, 3% sulfuric acid, 5% sodium hydroxide and toluene.

10. A laminated bulletproof glass, characterized by: The laminated bulletproof glass is composed of the surface treated semi-tempered glass, the PVB film, the polycarbonate board, the adhesive and the polyurethane layer; the structure of the laminated bulletproof glass is the surface treated semi-tempered glass, the PVB film, the surface treated semi-tempered glass, the adhesive, the polycarbonate board, the polyurethane layer and the polycarbonate board from top to bottom; the laminated bulletproof glass is prepared by the preparation process according to any one of claims 1 to 9; the elastic modulus of the polyurethane is 38-163MPa, and the LOI value is 19.5%-36.5%; the acetal degree of the PVB resin is 72.9%-83.1%; the impact strength of the PVB film is 481.1-546.8J / cm 2 The water contact angle of the cured waterproofing agent is 113°-129°, and the light transmittance is 82.1%-92.5%; the laminated bulletproof glass T 95% The temperature is 395-519℃, and the impact strength is 1671-2112J / cm 2 , the light transmittance is 81.9%-85.1%.

Citation Information

Patent Citations

  • Light-weight bullet-proof glass and preparation method thereof

    CN104369476A

  • Polyvinyl butyral rubber sheet and preparation method thereof

    CN106752995A

  • Impact-resistant high-strength bulletproof glass and preparation method thereof

    CN111452457A