Waterproof breathable TPU (thermoplastic polyurethane) high-low temperature film and preparation method thereof

By adopting a combined structure of reinforcement layer, waterproof and breathable film layer, TPU foam film layer and mesh hot melt adhesive layer in TPU high and low temperature film, the existing TPU film is solved by solving the waterproof and wear resistance and wear resistance in high-strength use environments in the existing TPU film. The quality of the product can be taken into account, which can achieve higher wear resistance and antibacterial properties and extend the service life of the product.

CN118876538AInactive Publication Date: 2024-11-01SUZHOU YUYAN SPECIAL MATERIAL TECH CO LTD

Patent Information

Application Number
CN202410542128.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing TPU high and low temperature films are difficult to take into account both waterproof and breathable properties and wear resistance in high-strength use environments, and are easily damaged in outdoor sports and other scenarios.

Method used

The structure consists of a reinforcement layer, a waterproof and breathable film layer, a TPU foam film layer, a mesh hot melt adhesive layer and a functional coating. The reinforcement layer is a fiber mesh or glass fiber, and the TPU foam film layer is provided with multiple The air-permeable membrane layer is a microporous film, which improves the overall performance through specific preparation methods.

Benefits of technology

It achieves good waterproof and breathable performance, wear resistance and antibacterial properties, making the product less likely to be damaged during high-intensity exercise, extends its service life, and keeps it clean and tidy in special environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_6
    Figure SMS_6
  • Figure SMS_7
    Figure SMS_7
  • Figure FDA0004821253450000011
    Figure FDA0004821253450000011
Patent Text Reader

Abstract

The invention relates to the technical field of TPU, and particularly discloses a waterproof breathable TPU high-low temperature film and a preparation method thereof.The waterproof breathable TPU high-low temperature film comprises a reinforcing layer, a waterproof breathable film layer, a TPU foaming film layer, a net-shaped hot melt adhesive layer, a release film layer and a functional coating which are sequentially arranged from top to bottom, and the reinforcing layer is at least one of fiber grids, glass fiber cloth and polyester fibers; the protective layer is at least one of a polymer coating, a fluorocarbon resin coating and a siloxane coating, the TPU foaming film layer is provided with a plurality of air passing through holes arranged at intervals, and the air passing through holes penetrate through the upper surface and the lower surface of the TPU foaming film layer; the functional coating can be additionally provided with a coating with a specific function according to different applications, and the waterproof breathable TPU high-low temperature film is simple in structure, convenient to manufacture, good in waterproof and breathable performance, good in wear resistance, corrosion resistance and antibacterial effect and stable in product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of TPU, and more specifically to a waterproof and breathable TPU high and low temperature film and a preparation method thereof. Background Art

[0002] TPU film is an elastic waveguide film, which is composed of a variety of smart materials, usually including polyurethane (PU), polyethylene (PE) and polyvinyl chloride (PVC); TPU film has excellent mechanical properties, wear resistance, acid and alkali resistance and heat resistance, and can withstand higher temperatures and higher pressures; in addition, it also has good aging resistance, chemical corrosion resistance and good elasticity, enabling it to operate under extreme environmental conditions.

[0003] TPU material has a wide temperature range and can maintain stability at higher temperatures, as well as maintain softness and elasticity at low temperatures. It is suitable for use in various climates. Waterproof and breathable TPU high and low temperature membranes are widely used in outdoor equipment, clothing, footwear, medical equipment, building materials and other fields, such as outdoor hiking, raincoats, protective clothing, medical dressings, etc. However, the existing TPU high and low temperature membranes are easily damaged in some high-intensity use environments, such as mountaineering shoes and outdoor sports, and cannot well balance waterproofness, breathability and wear resistance during sports. Summary of the invention

[0004] In order to overcome the above-mentioned defects of the prior art, the present invention provides a waterproof and breathable TPU high and low temperature membrane and a preparation method thereof to solve the problems existing in the above-mentioned background technology.

[0005] The present invention provides the following technical solution: a waterproof and breathable TPU high and low temperature film, comprising a reinforcing layer, a waterproof and breathable film layer, a TPU foaming film layer, a mesh hot melt adhesive layer, a release film layer and a functional coating arranged in sequence from top to bottom, the reinforcing layer is at least one of a fiber grid, a glass fiber cloth and a polyester fiber, the protective layer is at least one of a polymer coating, a fluorocarbon resin coating and a siloxane coating, the TPU foaming film layer is provided with a plurality of air holes arranged at intervals, and the air holes penetrate the upper surface and the lower surface of the TPU foaming film layer; the functional coating can be added with a coating with specific functions according to different applications;

[0006] In a preferred embodiment, the ratio of the polyester fiber to the resin in the reinforcement layer is between 20:80 and 40:60. The reinforcement layer is added to the membrane structure to improve the overall strength and wear resistance.

[0007] In a preferred embodiment, the waterproof breathable membrane layer is a microporous film waterproof breathable membrane layer.

[0008] In a preferred embodiment, the release film layer is a polytetrafluoroethylene (PTFE) release film or a polyethylene (PE) release film.

[0009] In a preferred embodiment, the method for preparing the waterproof breathable membrane layer comprises the following steps:

[0010] S1. Add polyurethane particles, polyethylene particles, polypropylene particles, polytetrafluoroethylene and additives to mixed solution A and stir for 12-15 hours to obtain an electrospinning solution; the mixed solution A is a mixed solution of organic solvent, water and functional additives, the organic solvent is a mixed solution of methanol, acetone and dimethyl sulfoxide, the total mass of the mixed solvent is: mtotal (100%) = mmethanol + macetone + mdimethyl sulfoxide, the functional additives are antioxidants, ultraviolet absorbers, fillers and antibacterial agents, and the mixing mass ratio of the functional additives is: Among them, Z 总 =Z1+Z2+...+M n is the total mass of all additives, mass ratio i represents the mass ratio of the ith additive, and the mixed mass ratios are all optimal mass ratios;

[0011] S2, subjecting the electrospinning solution to anti-static spinning treatment to obtain a preliminary membrane product;

[0012] S3, pre-treating the membrane product and coating a layer of pre-treatment agent after surface activation, placing the pre-treated membrane product in a treatment chamber and blowing nitrogen gas into it, and performing plasma surface activation on the membrane product using a plasma device;

[0013] S4, soaking the treated membrane in mixture B for 20-24 hours, wherein mixture B is a mixture of dodecafluoroheptylpropyltrimethoxysilane and methanol;

[0014] S5. After the immersion, the primary membrane is taken out and dried in a microwave oven at 50° C.-70° C. for 15-18 hours to obtain a waterproof and breathable membrane layer.

[0015] In a preferred embodiment, in step S1, the concentration of the organic solvent in the mixed solution A is 5%-15%.

[0016] In a preferred embodiment, in the step S4, the concentration of dodecafluoroheptylpropyltrimethoxysilane in the mixture B is 1-2.5 wt %.

[0017] In a preferred embodiment, the pretreatment in step 3 and the treatment parameters of the plasma equipment for the waterproof and breathable membrane layer are optimal parameters, such as a treatment power of 75-130w, a pressure of 15-50Pa, and a treatment time of 85-160s;

[0018] The TPU foam film layer is made of TPU foam material, and the TPU foam material includes the following raw materials in parts by weight: polyurethane is the main part with a weight of 50%-70%, foaming agent is 7%-35%, reinforcing agent is 5%-25%, stabilizer and auxiliary agent are 0.1%-5%, and colorant and filler are 0%-10%.

[0019] In a preferred embodiment, the preparation method of the TPU foam material is: after mixing various raw materials in an optimal ratio, using an air foaming machine to foam, the foaming ratio is 1:1.8-2.4, to obtain the TPU foam material, and the foaming method of the TPU foam material adopts the foaming steps in the prior art.

[0020] Another aspect of the present application provides a method for preparing a waterproof and breathable TPU high and low temperature film, comprising the following steps:

[0021] S21, taking the release film, spraying and treating the surface of the release film with a functional coating, and then compounding a mesh hot melt adhesive layer on the surface of the release film, adding a reinforcing layer to the surface of the waterproof and breathable membrane layer to form an enhanced waterproof and breathable membrane layer, and coating the surface of the enhanced waterproof and breathable membrane layer with a uniform TUP foaming material to form a TPU foaming membrane layer on the surface of the enhanced waterproof and breathable membrane layer;

[0022] S22, laminating the assembled mesh hot melt adhesive layer and the combined TPU foam film layer to form a waterproof and breathable TPU high and low temperature film; the laminating method of the mesh hot melt adhesive layer and the TPU foam film layer is a composite method in the prior art.

[0023] The waterproof and breathable TPU high and low temperature membrane of the present invention has a simple structure, is easy to manufacture, has good waterproof and breathable performance, good wear resistance, good corrosion resistance, good antibacterial effect, good mechanical properties, is simple and convenient to use, has strong practicality, is simple to manufacture, has stable product quality, and is easy to control.

[0024] Technical effects and advantages of the present invention:

[0025] The present invention provides a reinforcing layer, a waterproof and breathable membrane layer, a TPU foaming membrane layer, a mesh hot melt adhesive layer, a release membrane layer and a functional coating, which are sequentially arranged from top to bottom, so that the waterproof and breathable TPU high and low temperature membrane has good waterproof and breathable functions, increases its wear resistance and antibacterial properties, and increases the service life of the waterproof and breathable TPU high and low temperature membrane when used on fabric materials, upper materials or other products. The good waterproof and breathable properties ensure good breathability while ensuring waterproofness, and the increased wear resistance prevents damage during high-intensity exercise, thereby increasing its service life. The increased antibacterial properties have good antibacterial properties in special environments, and will not breed a large number of bacteria after long-term use, thereby maintaining a clean and tidy use environment. DETAILED DESCRIPTION

[0026] The technical solution in the present invention is described clearly and completely below. In addition, the forms of the various structures described in the following embodiments are merely illustrative. The waterproof and breathable TPU high and low temperature membrane and the preparation method thereof involved in the present invention are not limited to the various structures described in the following embodiments. All other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.

[0027] In an embodiment of the present invention, the present invention provides a waterproof and breathable TPU high and low temperature membrane, comprising a reinforcement layer, a waterproof and breathable membrane layer, a TPU foam film layer, a mesh hot melt adhesive layer, a release film layer and a functional coating arranged in sequence from top to bottom, the reinforcement layer is at least one of a fiber grid, a glass fiber cloth and a polyester fiber, the protective layer is at least one of a polymer coating, a fluorocarbon resin coating and a silicone coating, the TPU foam film layer is provided with a plurality of spaced-apart air holes, and the air holes penetrate the upper and lower surfaces of the TPU foam film layer; the functional coating can be increased with a coating having specific functions depending on the application.

[0028] What needs to be specifically explained in this embodiment is that: the reinforcement layer added to the membrane structure can improve the overall strength and wear resistance. The reinforcement layer has a ratio of polyester fiber to resin between 20:80 and 40:60. The ratio is determined according to the product use requirements. The polyester fiber accounts for 20% and the resin accounts for 80%, which has better curing effect and wear resistance. The polyester fiber accounts for 30% and the resin accounts for 70%, which provides better softness while maintaining a certain strength. The polyester fiber accounts for 40% and the resin accounts for 60%, which has better strength and rigidity and is suitable for higher strength situations. The waterproof and breathable membrane layer is a microporous film waterproof and breathable membrane layer, and the release membrane layer is a polytetrafluoroethylene (PTFE) release membrane or a polyethylene (PE) release membrane. The functional coating can be added with a coating with specific functions according to different applications. For example, the antibacterial / antimicrobial coating can be used in medical supplies and outdoor equipment, the anti-ultraviolet coating can be used in outdoor products, the anti-fouling layer can be used in an environment that needs to be kept clean for a long time, and the wear-resistant coating can be used in application scenarios that require frequent contact or friction.

[0029] In one embodiment of the present invention, the method for preparing the waterproof breathable membrane layer comprises the following steps:

[0030] S1. Add polyurethane particles, polyethylene particles, polypropylene particles, polytetrafluoroethylene and additives to mixed solution A and stir for 12-15 hours to obtain an electrospinning solution; the mixed solution A is a mixed solution of organic solvent, water and functional additives, the organic solvent is a mixed solution of methanol, acetone and dimethyl sulfoxide, the total mass of the mixed solvent is: mtotal (100%) = mmethanol + macetone + mdimethyl sulfoxide, the functional additives are antioxidants, ultraviolet absorbers, fillers and antibacterial agents, and the mixing mass ratio of the functional additives is: Among them, Z 总 =Z1+Z2+...+M n is the total mass of all additives, mass ratio i represents the mass ratio of the ith additive, and the mixed mass ratios are all optimal mass ratios;

[0031] S2, subjecting the electrospinning solution to anti-static spinning treatment to obtain a preliminary membrane product;

[0032] S3, pre-treating the membrane product and coating a layer of pre-treatment agent after surface activation, placing the pre-treated membrane product in a treatment chamber and blowing nitrogen gas into it, and performing plasma surface activation on the membrane product using a plasma device;

[0033] S4, soaking the treated membrane in mixture B for 20-24 hours, wherein mixture B is a mixture of dodecafluoroheptylpropyltrimethoxysilane and methanol;

[0034] S5. After the immersion, the primary membrane is taken out and dried in a microwave oven at 50° C.-70° C. for 15-18 hours to obtain a waterproof and breathable membrane layer.

[0035] In one embodiment of the present invention, in step S1, the concentration of the organic solvent in the mixed solution A is 5%-15%.

[0036] In one embodiment of the present invention, in step S4, the concentration of dodecafluoroheptylpropyltrimethoxysilane in the mixture B is 1-2.5 wt %.

[0037] In one embodiment of the present invention, the pretreatment in step 3 and the processing parameters of the plasma equipment for the waterproof and breathable membrane layer are optimal parameters, such as a processing power of 75-130w, a pressure of 15-50Pa, and a processing time of 85-160s.

[0038] The TPU foam film layer is made of TPU foam material, and the TPU foam material includes the following raw materials in parts by weight: polyurethane is the main part with a weight of 50%-70%, foaming agent is 7%-35%, reinforcing agent is 5%-25%, stabilizer and auxiliary agent are 0.1%-5%, and colorant and filler are 0%-10%.

[0039] The preparation method of the TPU foam material is as follows: various raw materials are mixed in an optimal ratio, and then foamed using an air foaming machine with a foaming ratio of 1:1.8-2.4 to obtain the TPU foam material. The foaming method of the TPU foam material adopts the foaming steps in the prior art.

[0040] The present invention also provides a method for preparing the waterproof and breathable TPU high and low temperature film, comprising the following steps:

[0041] S21, taking the release film, spraying and treating the surface of the release film with a functional coating, and then compounding a mesh hot melt adhesive layer on the surface of the release film, adding a reinforcing layer to the surface of the waterproof and breathable membrane layer to form an enhanced waterproof and breathable membrane layer, and coating the surface of the enhanced waterproof and breathable membrane layer with a uniform TUP foaming material to form a TPU foaming membrane layer on the surface of the enhanced waterproof and breathable membrane layer;

[0042] S22, laminating the assembled mesh hot melt adhesive layer and the combined TPU foam film layer to form a waterproof and breathable TPU high and low temperature film; the laminating method of the mesh hot melt adhesive layer and the TPU foam film layer is a composite method in the prior art.

[0043] Example 1

[0044] In this embodiment, the waterproof and breathable TPU high and low temperature membrane includes a reinforcement layer, a waterproof and breathable membrane layer, a TPU foam membrane layer, a mesh hot melt adhesive layer, a release membrane layer and a functional coating arranged in sequence from top to bottom, the reinforcement layer is at least one of a fiber grid, a glass fiber cloth and a polyester fiber, the protective layer is at least one of a polymer coating, a fluorocarbon resin coating and a silicone coating, the TPU foam membrane layer is provided with a plurality of air holes arranged at intervals, and the air holes penetrate the upper surface and the lower surface of the TPU foam membrane layer; the functional coating can be increased with a coating with specific functions according to different applications, the waterproof and breathable membrane layer is a microporous film waterproof and breathable membrane layer, and the release membrane layer is a polytetrafluoroethylene (PTFE) release membrane.

[0045] Example 2

[0046] In this embodiment, the waterproof and breathable TPU high and low temperature membrane includes a reinforcement layer, a waterproof and breathable membrane layer, a TPU foamed membrane layer, a mesh hot melt adhesive layer, a release film layer and a functional coating arranged in sequence from top to bottom, the reinforcement layer is at least one of a fiber grid, a glass fiber cloth and a polyester fiber, the protective layer is at least one of a polymer coating, a fluorocarbon resin coating and a silicone coating, the TPU foamed membrane layer is provided with a plurality of air holes arranged at intervals, and the air holes penetrate the upper surface and the lower surface of the TPU foamed membrane layer; the functional coating can be increased with a coating with specific functions according to different applications, the waterproof and breathable membrane layer is a microporous film waterproof and breathable membrane layer, and the release film layer is a polyethylene (PE) release film.

[0047] Example 3

[0048] In this embodiment, the method for preparing the waterproof breathable membrane layer comprises the following steps:

[0049] Polyurethane particles, polyethylene particles, polypropylene particles, polytetrafluoroethylene and additives are added to a mixed solution A and stirred for 12 hours to obtain an electrospinning solution; the mixed solution A is a mixed solution of organic solvent, water and functional additives, the organic solvent is a mixed solution of methanol, acetone and dimethyl sulfoxide, the total mass of the mixed solvent is: mtotal (100%) = mmethanol + macetone + mdimethyl sulfoxide, the functional additives are antioxidants, ultraviolet absorbers, fillers and antibacterial agents, and the mixing mass ratio of the functional additives is: Among them, Z 总 =Z1+Z2+...+M n is the total mass of all additives, mass ratio i represents the mass ratio of the ith additive, and the mixed mass ratios are all optimal mass ratios;

[0050] S2, subjecting the electrospinning solution to anti-static spinning treatment to obtain a preliminary membrane product;

[0051] S3, pre-treating the membrane product and coating a layer of pre-treatment agent after surface activation, placing the pre-treated membrane product in a treatment chamber and blowing nitrogen gas into it, and performing plasma surface activation on the membrane product using a plasma device;

[0052] S4, soaking the treated film in mixture B for 20 hours, wherein mixture B is a mixture of dodecafluoroheptylpropyltrimethoxysilane and methanol;

[0053] S5. After the immersion, the primary membrane is taken out and dried in a microwave oven at 50° C. for 18 hours to obtain a waterproof and breathable membrane layer.

[0054] Furthermore, in step S1, the concentration of the organic solvent in the mixed solution A is 8%.

[0055] Further, in step S4, the concentration of dodecafluoroheptylpropyltrimethoxysilane in the mixture B is 1.5 wt %.

[0056] Furthermore, the pretreatment in step 3 and the treatment parameters of the plasma equipment for the waterproof and breathable membrane layer are optimal parameters, such as a treatment power of 75w, a pressure of 35Pa, and a treatment time of 150s.

[0057] The TPU foam film layer is made of TPU foam material, and the TPU foam material includes the following raw materials in parts by weight: polyurethane as the main part is 50% by weight, foaming agent is 30% by weight, reinforcing agent is 10% by weight, stabilizer and auxiliary agent is 3% by weight, and colorant and filler are 7% by weight.

[0058] The preparation method of the TPU foam material is as follows: various raw materials are mixed in an optimal ratio, and then foamed using an air foaming machine at a foaming ratio of 1:2 to obtain the TPU foam material. The foaming method of the TPU foam material adopts the foaming steps in the prior art.

[0059] The method for preparing the waterproof and breathable TPU high and low temperature membrane in this example includes the following steps:

[0060] S21, taking the release film, spraying and treating the surface of the release film with a functional coating, and then compounding a mesh hot melt adhesive layer on the surface of the release film, adding a reinforcing layer to the surface of the waterproof and breathable membrane layer to form an enhanced waterproof and breathable membrane layer, and coating the surface of the enhanced waterproof and breathable membrane layer with a uniform TUP foaming material to form a TPU foaming membrane layer on the surface of the enhanced waterproof and breathable membrane layer;

[0061] S22, laminating the assembled mesh hot melt adhesive layer and the combined TPU foam film layer to form a waterproof and breathable TPU high and low temperature film; the laminating method of the mesh hot melt adhesive layer and the TPU foam film layer is a composite method in the prior art.

[0062] The rest of this example is the same as that of Example 1 and will not be described in detail here.

[0063] Example 4

[0064] In this embodiment, the method for preparing the waterproof breathable membrane layer comprises the following steps:

[0065] S1. Add polyurethane particles, polyethylene particles, polypropylene particles, polytetrafluoroethylene and additives to mixed solution A and stir for 12 hours to obtain an electrospinning solution; the mixed solution A is a mixed solution of organic solvent, water and functional additives, the organic solvent is a mixed solution of methanol, acetone and dimethyl sulfoxide, the total mass of the mixed solvent is: mtotal (100%) = mmethanol + macetone + mdimethyl sulfoxide, the functional additives are antioxidants, ultraviolet absorbers, fillers and antibacterial agents, and the mixing mass ratio of the functional additives is: Among them, Z 总 =Z1+Z2+...+M n is the total mass of all additives, mass ratio i represents the mass ratio of the ith additive; the mixed mass ratios are all optimal mass ratios;

[0066] S2, subjecting the electrospinning solution to anti-static spinning treatment to obtain a preliminary membrane product;

[0067] S3, pre-treating the membrane product and coating a layer of pre-treatment agent after surface activation, placing the pre-treated membrane product in a treatment chamber and blowing nitrogen gas into it, and performing plasma surface activation on the membrane product using a plasma device;

[0068] S4, soaking the treated film in mixture B for 22 hours, wherein mixture B is a mixture of dodecafluoroheptylpropyltrimethoxysilane and methanol;

[0069] S5. After the immersion, the primary membrane is taken out and dried in a microwave oven at 60° C. for 17 hours to obtain a waterproof and breathable membrane layer.

[0070] Furthermore, in step S1, the concentration of the organic solvent in the mixed solution A is 13%.

[0071] Further, in step S4, the concentration of dodecafluoroheptylpropyltrimethoxysilane in the mixture B is 2 wt %.

[0072] Furthermore, the pretreatment in step 3 and the treatment parameters of the plasma equipment for the waterproof and breathable membrane layer are optimal parameters, such as a treatment power of 100W, a pressure of 43Pa, and a treatment time of 130s.

[0073] The TPU foam film layer is made of TPU foam material, and the TPU foam material includes the following raw materials in parts by weight: polyurethane as the main part is 60% by weight, foaming agent is 20% by weight, reinforcing agent is 20% by weight, stabilizer and auxiliary agent is 4% by weight, and colorant and filler are 6% by weight.

[0074] The preparation method of the TPU foam material is as follows: various raw materials are mixed in an optimal ratio, and then foamed using an air foaming machine at a foaming ratio of 1:2.2 to obtain the TPU foam material. The foaming method of the TPU foam material adopts the foaming steps in the prior art.

[0075] The method for preparing the waterproof and breathable TPU high and low temperature membrane in this example includes the following steps:

[0076] S21, taking the release film, spraying and treating the surface of the release film with a functional coating, and then compounding a mesh hot melt adhesive layer on the surface of the release film, adding a reinforcing layer to the surface of the waterproof and breathable membrane layer to form an enhanced waterproof and breathable membrane layer, and coating the surface of the enhanced waterproof and breathable membrane layer with a uniform TUP foaming material to form a TPU foaming membrane layer on the surface of the enhanced waterproof and breathable membrane layer;

[0077] S22, laminating the assembled mesh hot melt adhesive layer and the combined TPU foam film layer to form a waterproof and breathable TPU high and low temperature film; the laminating method of the mesh hot melt adhesive layer and the TPU foam film layer is a composite method in the prior art.

[0078] The rest of this example is the same as that of Example 1 and will not be described in detail here.

[0079] Example 5

[0080] In this embodiment, the method for preparing the waterproof breathable membrane layer comprises the following steps:

[0081] S1. Add polyurethane particles, polyethylene particles, polypropylene particles, polytetrafluoroethylene and additives to mixed solution A and stir for 12-15 hours to obtain an electrospinning solution; the mixed solution A is a mixed solution of organic solvent, water and functional additives, the organic solvent is a mixed solution of methanol, acetone and dimethyl sulfoxide, the total mass of the mixed solvent is: mtotal (100%) = mmethanol + macetone + mdimethyl sulfoxide, the functional additives are antioxidants, ultraviolet absorbers, fillers and antibacterial agents, and the mixing mass ratio of the functional additives is: Among them, Z 总 =Z1+Z2+...+M n is the total mass of all additives, mass ratio i represents the mass ratio of the ith additive, and the mixed mass ratios are all optimal mass ratios;

[0082] S2, subjecting the electrospinning solution to anti-static spinning treatment to obtain a preliminary membrane product;

[0083] S3, pre-treating the membrane product and coating a layer of pre-treatment agent after surface activation, placing the pre-treated membrane product in a treatment chamber and blowing nitrogen gas into it, and performing plasma surface activation on the membrane product using a plasma device;

[0084] S4, soaking the treated film in mixture B for 24 hours, wherein mixture B is a mixture of dodecafluoroheptylpropyltrimethoxysilane and methanol;

[0085] S5. After the immersion, the primary membrane is taken out and dried in a microwave oven at 70° C. for 15 hours to obtain a waterproof and breathable membrane layer.

[0086] In one embodiment of the present invention, in step S1, the concentration of the organic solvent in the mixed solution A is 15%.

[0087] In one embodiment of the present invention, in step S4, the concentration of dodecafluoroheptylpropyltrimethoxysilane in the mixture B is 2.5 wt%.

[0088] In one embodiment of the present invention, the pretreatment in step 3 and the treatment parameters of the plasma equipment on the waterproof and breathable membrane layer are optimal parameters, such as a treatment power of 130w, a pressure of 50Pa, and a treatment time of 100s.

[0089] The TPU foam film layer is made of TPU foam material, and the TPU foam material includes the following raw materials in parts by weight: polyurethane as the main part is 70% by weight, foaming agent is 20% by weight, reinforcing agent is 20% by weight, stabilizer and auxiliary agent is 5% by weight, and colorant and filler are 5% by weight.

[0090] The preparation method of the TPU foam material is as follows: various raw materials are mixed in an optimal ratio, and then foamed using an air foaming machine with a foaming ratio of 1:1.8 to obtain the TPU foam material. The foaming method of the TPU foam material adopts the foaming steps in the prior art.

[0091] The present invention also provides a method for preparing the waterproof and breathable TPU high and low temperature film, comprising the following steps:

[0092] S21, taking the release film, spraying and treating the surface of the release film with a functional coating, and then compounding a mesh hot melt adhesive layer on the surface of the release film, adding a reinforcing layer to the surface of the waterproof and breathable membrane layer to form an enhanced waterproof and breathable membrane layer, and coating the surface of the enhanced waterproof and breathable membrane layer with a uniform TUP foaming material to form a TPU foaming membrane layer on the surface of the enhanced waterproof and breathable membrane layer;

[0093] S22, laminating the assembled mesh hot melt adhesive layer and the combined TPU foam film layer to form a waterproof and breathable TPU high and low temperature film; the laminating method of the mesh hot melt adhesive layer and the TPU foam film layer is a composite method in the prior art.

[0094]

[0095]

[0096] Among them, the water resistance is measured by GB / T 4744-2013, the air permeability is measured by GB / T 5453-1997, the moisture permeability is measured by GB / T 12704.1-2009, and the tensile strength is measured by a tensile testing machine using a biaxial stretching method, with a stretching rate of 0.4 cm / min and a measuring range of 12 cm.

[0097] The waterproof and breathable TPU high and low temperature membrane of the present invention has a simple structure, is easy to manufacture, has good waterproof and breathable performance, good wear resistance, good corrosion resistance, good antibacterial effect, good mechanical properties, is simple and convenient to use, has strong practicality, is simple to manufacture, has stable product quality, and is easy to control.

[0098] Finally: The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. Waterproof and breathable TPU high and low temperature membrane, characterized by: It includes a reinforcement layer, a waterproof and breathable film layer, a TPU foam film layer, a mesh hot melt adhesive layer, a release film layer and a functional coating which are arranged in sequence from top to bottom. The reinforcement layer is at least one of a fiber mesh, a glass fiber cloth and a polyester fiber. The protective layer is at least one of a polymer coating, a fluorocarbon resin coating and a silicone coating. The TPU foam film layer is provided with a plurality of air holes arranged at intervals, and the air holes penetrate the upper surface and the lower surface of the TPU foam film layer. The functional coating can be increased with a coating having specific functions according to different applications.

2. The waterproof and breathable TPU high and low temperature membrane according to claim 1, characterized in that: The ratio of the polyester fiber to the resin in the reinforcement layer is between 20:80 and 40:

60. The reinforcement layer is added to the membrane structure to improve the overall strength and wear resistance.

3. The waterproof and breathable TPU high and low temperature membrane according to claim 1, characterized in that: The waterproof and breathable membrane layer is a microporous film waterproof and breathable membrane layer.

4. The waterproof and breathable TPU high and low temperature membrane according to claim 1, characterized in that: The release film layer is a polytetrafluoroethylene (PTFE) release film or a polyethylene (PE) release film.

5. The waterproof and breathable TPU high and low temperature membrane according to claim 1, characterized in that: The method for preparing the waterproof breathable membrane layer comprises the following steps: S1. Add polyurethane particles, polyethylene particles, polypropylene particles, polytetrafluoroethylene and additives to mixed solution A and stir for 12-15 hours to obtain an electrospinning solution; the mixed solution A is a mixed solution of organic solvent, water and functional additives, the organic solvent is a mixed solution of methanol, acetone and dimethyl sulfoxide, the total mass of the mixed solvent is: mtotal (100%) = mmethanol + macetone + mdimethyl sulfoxide, the functional additives are antioxidants, ultraviolet absorbers, fillers and antibacterial agents, and the mixing mass ratio of the functional additives is: mass ratio Among them, Z 总 =Z1+Z2+...+M n is the total mass of all additives, mass ratio i represents the mass ratio of the ith additive, and the mixed mass ratios are all optimal mass ratios; S2, subjecting the electrospinning solution to anti-static spinning treatment to obtain a preliminary membrane product; S3, pre-treating the membrane product and coating a layer of pre-treatment agent after surface activation, placing the pre-treated membrane product in a treatment chamber and blowing nitrogen gas into it, and performing plasma surface activation on the membrane product using a plasma device; S4, soaking the treated membrane in mixture B for 20-24 hours, wherein mixture B is a mixture of dodecafluoroheptylpropyltrimethoxysilane and methanol; S5. After the immersion, the primary membrane is taken out and dried in a microwave oven at 50° C.-70° C. for 15-18 hours to obtain a waterproof and breathable membrane layer.

6. The waterproof and breathable TPU high and low temperature membrane according to claim 5, characterized in that: In the step S1, the concentration of the organic solvent in the mixed solution A is 5%-15%.

7. The waterproof and breathable TPU high and low temperature membrane according to claim 5, characterized in that: In the step S4, the concentration of dodecafluoroheptylpropyltrimethoxysilane in the mixture B is 1-2.5 wt %.

8. The waterproof and breathable TPU high and low temperature membrane according to claim 5, characterized in that: The pretreatment and plasma equipment processing parameters for the waterproof and breathable membrane layer in step 3 are optimal parameters, such as a processing power of 75-130w, a pressure of 15-50Pa, and a processing time of 85-160s; The TPU foam film layer is made of TPU foam material, and the TPU foam material includes the following raw materials in parts by weight: polyurethane is the main part with a weight of 50%-70%, foaming agent is 7%-35%, reinforcing agent is 5%-25%, stabilizer and auxiliary agent are 0.1%-5%, and colorant and filler are 0%-10%.

9. The waterproof and breathable TPU high and low temperature membrane according to claim 8, characterized in that: The preparation method of the TPU foam material is as follows: various raw materials are mixed in an optimal ratio, and then foamed using an air foaming machine with a foaming ratio of 1:1.8-2.4 to obtain the TPU foam material. The foaming method of the TPU foam material adopts the foaming steps in the prior art.

10. A method for preparing a waterproof and breathable TPU high and low temperature membrane, using the waterproof and breathable TPU high and low temperature membrane as claimed in any one of claims 1 to 9, characterized in that: The following steps are involved: S21, taking the release film, spraying and treating the surface of the release film with a functional coating, and then compounding a mesh hot melt adhesive layer on the surface of the release film, adding a reinforcing layer to the surface of the waterproof and breathable membrane layer to form an enhanced waterproof and breathable membrane layer, and coating the surface of the enhanced waterproof and breathable membrane layer with a uniform TUP foaming material to form a TPU foaming membrane layer on the surface of the enhanced waterproof and breathable membrane layer; S22, laminating the assembled mesh hot melt adhesive layer and the combined TPU foam film layer to form a waterproof and breathable TPU high and low temperature film; the laminating method of the mesh hot melt adhesive layer and the TPU foam film layer is a composite method in the prior art.

Citation Information

Patent Citations

  • Moisture permeable waterproof composite film and moisture permeable waterproof fabric having moisture permeable waterproof composite film

    CN103660464A

  • Single-layer roof waterproof coiled material and preparation method therefor

    CN108136748A

  • High-strength and single-layer roof waterproof coiled material and preparation method thereof

    CN109049898A

  • Simulated leather texture polyurethane leather for automobile and preparation method of simulated leather texture polyurethane leather

    CN109530190A

  • Device and method for preparing waterproof and moisture-permeable TPU (Thermoplastic Polyurethane) composite film

    CN115284719A

Cited By

  • High-temperature and low-temperature film with high surface wear resistance and preparation method thereof

    CN121798947A

  • A surface high wear-resistant high-low temperature film and a preparation method thereof