Preparation method of core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material induced and synthesized by cobalt ions
The ternary metal MOF derivative of core-shell structure induced by cobalt ion is solved, and the problem of unstable structure and poor conductivity of the potassium ion battery electrode material during charging and discharging is achieved, and the morphology maintenance and conductivity improvement at high temperatures is achieved. It improves cycle stability and rate performance, suitable for large-scale energy storage equipment applications.
Patent Information
- Application Number
- CN202410915613.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The existing potassium ion battery electrode materials are structurally unstable due to the volume expansion of potassium ions during charging and discharging, and most metal organic frame materials decompose during high temperature pyrolysis, resulting in reduced conductivity and poor chemical stability, which is difficult to meet the large-scale The cycle life and rate performance requirements of energy storage requirements.
The ternary metal MOF derivative of core-shell structure induced by cobalt ion is used to form a uniform core-shell structure through cobalt ion induced and epitaxial growth. The external carbon layer and ZnO shell buffer volume expansion, and the in-situ derived porous nitrogen-doped carbon The layer improves conductivity and electrochemically active sites.
It realizes the material's morphology maintained at high temperature, the structural stability and conductivity are improved, and the cycle stability and rate performance of potassium ion batteries are significantly improved, making it suitable for commercial applications of large-scale energy storage equipment.
Smart Images

Figure CN118877869A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of negative electrode materials for potassium ion batteries, and specifically relates to a preparation method of a negative electrode material for potassium ion batteries using a core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction. Background Art
[0002] Energy is inseparable from our lives. As a highly concerned issue in the 21st century, energy affects the development of human society and the global economy. From fossil fuel energy to renewable energy, the energy system is constantly changing in order to achieve green, sustainable and high-quality development. However, as the few renewable energy sources that can be developed and utilized, wind energy, hydropower, tidal energy, solar energy and geothermal energy are mostly restricted to a large extent due to the unpredictability of weather, climate volatility, and unevenness in time and space. Electrochemical energy storage systems, especially rechargeable batteries, as a rapidly developing energy storage device, can store these renewable energy sources that cannot be used up for a while, and maximize their utilization in time and space.
[0003] Potassium has similar physical and chemical properties to lithium, and its reserves in the earth's crust are more abundant (17000ppm), and its cost is more attractive. Potassium-ion batteries developed with it have a higher voltage platform, a suitable embedding potential (about 0.2V), excellent ionic / electronic conductivity and high energy density, and are highly anticipated candidates for future large-scale energy storage devices. However, compared with lithium ions, potassium ions have a larger ionic radius. During the charging and discharging process, the embedding and extraction of potassium ions will cause a greater volume expansion, which also places higher requirements on the structural stability and strength of potassium ion battery electrode materials. Therefore, it is very important to synthesize electrode materials with a specific structure and a certain protective layer that can buffer volume expansion and provide more potassium ion storage sites during the cycle.
[0004] Metal-organic frameworks (MOFs) are a new type of ordered porous materials, which are composed of metal ions or metal clusters and organic ligands bridged by coordination bonds. Due to their unique rich coordinated unsaturated metal active sites, rich and diverse structures and large specific surface area, they are a class of materials that have attracted much attention. However, most of the MOF materials reported so far have very limited direct applications due to their inherent low electrical conductivity and poor chemical stability. High-temperature pyrolysis is currently a good means to improve its conductivity. Unfortunately, due to the instability of MOF materials, decomposition is inevitable during the pyrolysis process, resulting in the destruction of their original structure and morphology, and easily causing the agglomeration of metal / carbon materials, reducing their active sites.
[0005] Therefore, researching and developing an electrode material with a stable structure that ensures long cycle life and rate performance to meet the future large-scale energy storage needs is of great significance to promoting the commercialization of potassium-ion batteries. Summary of the invention
[0006] In view of the above technical problems, the present invention aims to provide a method for preparing a potassium ion battery negative electrode material of a core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction. By adopting cobalt ion induction and epitaxial growth, a core-shell structure ternary metal MOF derivative is prepared. The material has uniform morphology and can still maintain its original complete morphology after high-temperature carbonization. The inner core is reduced to ultrafine metal and metal carbide small particles at high temperature and evenly distributed inside the rod; the outer carbon layer and ZnO shell layer play a double-layer confinement role, which can greatly buffer the volume expansion of the material during potassiumization, thereby ensuring the structural stability of the material during repeated cycles; in addition, the in-situ derived porous nitrogen-doped carbon layer acts as a good conductive agent, which can also improve the overall conductivity of the material and provide more electrochemical active sites and potassium ion transmission channels, thereby improving the rate performance of the material. The material prepared by the present invention is used for potassium ion batteries, has excellent electrochemical properties, is simple in preparation method, has a short cycle, and is easy to promote and apply.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is:
[0008] A method for preparing a cobalt ion-induced synthesis of a core-shell structured ternary metal MOF derivative potassium ion battery negative electrode material is carried out in the following order:
[0009] S1, adding cobalt salt, iron salt and organic ligand in an equal molar ratio into an organic solvent N,N-dimethylacetamide, and ultrasonically treating until they are completely dissolved to obtain a black solution, which is recorded as A;
[0010] S2, transfer A to a reactor, perform solvothermal reaction at 150°C for 10 h, centrifuge the product after cooling to room temperature, wash the product with deionized water until the supernatant is transparent and colorless, and vacuum dry at 70°C for 10 h to obtain Co-FeMOF nanorods, which are recorded as B;
[0011] S3, ultrasonically dispersing B in a methanol solution containing PVP, followed by continuous stirring to obtain a PVP-functionalized Co-Fe MOF suspension, denoted as C;
[0012] S4, washing C with methanol at 8000 rpm for 8 min, washing twice, and then ultrasonically dispersing it in a methanol solution again to obtain a dark brown suspension, recorded as D;
[0013] S5. Add cobalt salt, zinc salt and organic ligand to D in an equimolar ratio, and add methanol solution additionally, stir until they are evenly dispersed and then let stand to allow epitaxial growth. After standing for 24 hours, wash twice with methanol, centrifuge and dry, and then carbonize to obtain a ternary metal MOF derivative with a core-shell structure.
[0014] As a limitation of the present invention:
[0015] (i) In step S1, the cobalt salt is cobalt nitrate hexahydrate, the iron salt is ferric chloride hexahydrate, and the organic ligand is 2-aminoterephthalic acid.
[0016] (ii) In step S2, the temperature of the solvent thermal reaction is increased at a rate of 5°C / min to the target temperature.
[0017] In the solvent thermal process of the present invention, iron ions and 2-aminoterephthalic acid undergo a self-polymerization reaction, and the kinetics and thermodynamics of FeMOF growth are regulated by induction of cobalt ions, so that FeMOF is guided to grow in an orderly manner along a specific crystal plane, thereby forming a Co-FeMOF nanorod morphology, which is extremely beneficial for subsequent epitaxial growth and carbonization. The obtained Co-FeMOF nanorods have uniform sizes and a diameter of about 100 nm.
[0018] (III) In step S2, the centrifugal speed is 9000 rpm, the centrifugal time is 10 min, and the number of washing times with deionized water is not less than 9 times.
[0019] (iv) In step S3, the mass ratio of B to PVP is 27:100, and the concentration of the methanol solution of PVP is 0.05 g / mL.
[0020] The mass ratio of B to PVP in the present invention affects the subsequent growth of ZIF-8 on Co-Fe MOF. PVP, as a surfactant and dispersant, has a polymer chain structure and good hydrophilicity and dispersibility. Through stirring treatment, a layer of PVP can be coated on the surface of Co-Fe MOF, thereby weakening the interaction between Co-Fe MOF and ensuring its stable dispersion in methanol. In addition, a large number of oxygen-containing functional groups can be introduced on the surface of Co-Fe MOF through PVP treatment, which can attract metal ions to be adsorbed on its surface.
[0021] (V) In step S5, the cobalt salt is cobalt nitrate hexahydrate, the zinc salt is zinc nitrate hexahydrate, the organic ligand is 2-methylimidazole, and the molar volume ratio of the cobalt salt to D and the methanol solution is 0.4 mmol:9 mL:320 mL.
[0022] In the present invention, during the epitaxial growth of nanorods, the cobalt salt, zinc salt and organic ligand undergo a polymerization reaction with zinc ions and 2-methylimidazole under the induction of cobalt ions, and the ZIF-8 growth kinetics and thermodynamics are regulated to make it epitaxially grow along a specific crystal plane on the surface of Co-Fe MOF. Under this ratio, a ZIF-8 layer with uniform thickness can be coated on the periphery of Co-Fe MOF.
[0023] (VI) In step S5, the centrifugal speed is 7000 rpm and the time is 7 min.
[0024] (VII) In step S5, the carbonization treatment is carried out under the protection of a nitrogen atmosphere according to the following procedure:
[0025] The first stage: heating from room temperature to 200℃, keeping warm for 2h;
[0026] The second stage: heating from 200℃ to 700℃, keeping warm for 2h;
[0027] The third stage: cooling to room temperature in the furnace.
[0028] (VIII) In step S5, the heating rate of the first stage and the second stage is 2°C / min.
[0029] The high-temperature carbonization process is to further enhance the stability and conductivity of the material, which is critical for the formation of core-shell structure ternary metal MOF derivatives. The first stage is a low-temperature heat treatment at 200 ° C. Through low-temperature heat treatment, the residual organic ligands, solvents and some volatile substances in the material can be removed, and these organic substances can be volatilized, thereby removing their interference with subsequent high-temperature treatment. At the same time, during the low-temperature treatment process, some structural components in the material will also undergo certain chemical changes and structural adjustments. Through low-temperature treatment, heat is gradually introduced to avoid the thermal stress problem caused by a one-time large-scale temperature increase, thereby reducing the thermal damage and structural damage to the material by high temperature, and enhancing its stability at high temperature. This step helps to maintain the structure and stability of the material during the subsequent 700 ° C high-temperature treatment process. In the second stage, the temperature is raised from 200 ° C to 700 ° C, thereby achieving the final high-temperature treatment to further enhance the thermal stability of the material, improve its conductivity, optimize the performance of the final material, and finally form a core-shell structure ternary metal MOF derivative.
[0030] The present invention has another limitation, that the core-shell structured ternary metal MOF derivative has a shuttle-like morphology, and this morphology can be prepared in a controlled manner.
[0031] The above technical solution of the present invention is taken as a whole, and each step is closely related and influences each other, which jointly determine the morphological characteristics and performance of the product.
[0032] The above technical solution has the following advantages or beneficial effects:
[0033] 1. The present invention adopts a cobalt ion induction method. In an organic solvent N,N-dimethylacetamide, through a solvothermal reaction, cobalt ions are used to directionally induce the reaction between iron ions and an organic ligand 2-aminoterephthalic acid to form a bimetallic Co-FeMOF having a specific shuttle-like morphology. This cobalt ion induction method ensures the uniformity of its synthetic morphology and size, and can be prepared in batches.
[0034] 2. Based on the one-step cobalt ion-induced synthesis of bimetallic Co-Fe MOF, the present invention introduces cobalt salt and zinc salt again, and utilizes the inductive effect of cobalt ions to guide zinc ions and organic ligand 2-methylimidazole to grow directional in methanol solution and grow uniformly on the surface of Co-Fe MOF. Due to the presence of cobalt ions, ZIF-8 tends to be generated along a specific crystal plane to obtain a thin layer of hexagonal crystals, thereby forming a good protective layer coated on the outer surface of Co-Fe MOF. This cobalt ion-induced epitaxial growth method further ensures the uniformity of the morphology and size of the synthesized ternary metal MOF, and optimizes the electronic structure and stability of the material through the two-step introduction of cobalt.
[0035] 3. The core-shell structure ternary metal MOF derivative prepared by the present invention has uniform morphology and can still maintain its original complete morphology after high-temperature carbonization. The inner core is reduced to ultrafine metal and metal carbide particles at high temperature and evenly distributed inside the rod; the outer carbon layer and ZnO shell layer play a double-layer confinement role, which can greatly buffer the volume expansion of the material during potassiumization, thereby ensuring the structural stability of the material during repeated cycles; at the same time, the in-situ derived porous nitrogen-doped carbon layer acts as a good conductive agent, which can also improve the overall conductivity of the material and provide more electrochemical active sites and potassium ion transmission channels, thereby improving the rate performance of the material.
[0036] 4. The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction of the present invention has long cycle stability and high rate performance, and is used as anode material of potassium ion battery. Its electrochemical performance is significantly improved, and the preparation process is easy to control, which is suitable for industrial promotion.
[0037] The invention is suitable for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material.
[0038] The technical solution of the present invention will be further described in detail below in conjunction with the embodiments of the present invention and the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1This is a scanning electron microscope image of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention;
[0040] Figure 2 It is a transmission electron microscope image and a particle size distribution diagram of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention;
[0041] Figure 3 This is an energy spectrum picture of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction with a multi-level layered structure prepared in Example 1 of the present invention;
[0042] Figure 4 This is a high-resolution image of the cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative prepared in Example 1 of the present invention;
[0043] Figure 5 is the XRD pattern of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention;
[0044] Figure 6 This is a Raman graph of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention;
[0045] Figure 7 This is an XPS graph of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention;
[0046] Figure 8 This is an impedance diagram of a potassium ion battery made of a core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention;
[0047] Fig. 9 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 0.5mV·s -1 CV curves measured at a scan rate of ;
[0048] Fig.10 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 0.1A·g -1 The charge and discharge diagram measured under the current of;
[0049] Fig.11 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 0.1A·g -1 Performance diagram of 130 cycles at a current density of;
[0050] Fig.12 This is a rate performance diagram of a potassium ion battery made of a core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention at different current densities;
[0051] Fig.13 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 1.0A·g -1 Performance diagram of 2000 cycles at a current density of;
[0052] Fig.14 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 1.0A·g -1 Scanning electron microscope image of 2000 cycles at a current density of ;
[0053] Fig.15 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 0.5mV·s -1 CV curves measured at different temperatures at a scan rate of ;
[0054] Fig.16 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 45°C, 0.1A·g -1 Performance diagram of 100 cycles at a current density of;
[0055] Fig.17 This is a rate performance diagram of a potassium ion battery made of a core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention at 45° C. and different current densities;
[0056] Fig.18 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in Example 1 of the present invention is used as a potassium ion battery at 45°C, 1.0A·g -1 Performance diagram of 300 cycles at a current density of . DETAILED DESCRIPTION
[0057] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.
[0058] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.
[0059] Example 1 A method for preparing a cobalt ion-induced synthesis of a core-shell structured ternary metal MOF derivative potassium ion battery negative electrode material
[0060] S1, adding 3 mmol of cobalt nitrate hexahydrate, 3 mmol of ferric chloride hexahydrate and 3 mmol of 2-aminoterephthalic acid to 60 mL of organic solvent N,N-dimethylacetamide, and ultrasonically treating them at an ultrasonic power of 360 W for 90 min until they are completely dissolved to obtain a black solution, which is recorded as A;
[0061] S2, transfer A to a 100 mL polytetrafluoroethylene stainless steel autoclave, heat from room temperature to 150°C at a heating rate of 5°C / min, and react for 10 hours. After cooling to room temperature, centrifuge and wash with deionized water for no less than 9 times at a centrifugal speed of 9000 rpm for 10 minutes until the supernatant is transparent and colorless, and then vacuum dry at 70°C for 10 hours to obtain bimetallic Co-Fe MOF nanorods, which are recorded as B;
[0062] S3, adding 405 mg of B to 30 mL of methanol solution containing 1.5 g of PVP, ultrasonically treating for 20 min at a power of 360 W, and then stirring for 12 h to obtain a Co-Fe MOF suspension functionalized with PVP, recorded as C;
[0063] S4, C was ultrasonically washed with methanol, centrifuged at 8000 rpm for 8 min each time, washed twice with methanol, and then the sample was ultrasonically dispersed in 45 mL of methanol solution again, with an ultrasonic power of 360 W and an ultrasonic time of 2 h to obtain a dark brown PVP functionalized Co-Fe MOF suspension, recorded as D;
[0064] S5. Add 0.4mmol cobalt nitrate hexahydrate, 0.4mmol zinc nitrate hexahydrate and 0.4mmol 2-methylimidazole to 9mL D, then add 320mL methanol solution, stir for 2h, mix well and let it stand, grow for 24h at room temperature; then centrifuge and wash twice with methanol, the centrifugal speed is 7000rpm, the time is 7min; after the sample is dried, it is carbonized under nitrogen atmosphere protection, and the temperature is increased according to a two-stage program, first from room temperature to 200℃ at a heating rate of 2℃ / min, and kept warm for 2h, then continue to heat from 200℃ to 700℃ at a heating rate of 2℃ / min, and keep warm for 2h. After completion, cool to room temperature with the furnace to obtain the sample Co-SNCS-t.
[0065] A series of performance tests were conducted on the product prepared in this example to determine the process of assembling it as a negative electrode material into a potassium ion battery as follows: a negative electrode shell, a metal potassium sheet, a diaphragm, an electrolyte, an electrode sheet, a gasket, a spring and a positive electrode shell. The specific results of the test are as follows:
[0066] Figure 1 This is a scanning image of the cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative prepared in an embodiment of the present invention. It can be clearly seen from the figure that after high-temperature carbonization, the Co-SNCS-t material basically maintains a shuttle-shaped rod morphology, and the rod diameter is about 110nm.
[0067] Figure 2 This is a transmission and particle size distribution diagram of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention. It can be seen from the figure that the Co-SNCS-t material presents a core-shell structure, and some small black particles are evenly distributed inside the rod, and the particle size is about 6.03nm.
[0068] Figure 3 This is the energy spectrum of the cobalt ion-induced synthesized core-shell ternary metal MOF derivative prepared in the embodiment of the present invention. From the figure, it can be seen that the six elements C, N, Fe, Co, Zn and O are evenly distributed in the whole material, proving the presence of C, N, Fe, Co, Zn and O elements in Co-SNCS-t.
[0069] Figure 4 This is a high-resolution image of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention. From the image, it can be seen that the small black particles inside the Co-SNCS-t material correspond to the crystal planes of Fe3C and Fe. Among them, the crystal plane spacing is Corresponding to the (011) crystal plane of Fe element, the interplanar spacing is and They correspond to the (031) and (211) crystal planes of Fe3C, respectively. In addition, there are many obvious defects inside the material, and the carbon in the outer shell is mostly in an amorphous form, which shows that after high-temperature carbonization, the core inside the ternary metal MOF is mainly transformed into Fe and Fe3C, and the corresponding organic ligand is mainly transformed into an amorphous carbon layer. The small particles inside are tightly wrapped by the outer amorphous carbon layer, which can ensure the stability of the material structure and provide more active sites and potassium ion transmission channels at the same time.
[0070] Figure 5This is the XRD diagram of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention. It can be seen from the figure that the main peaks of the Co-SNCS-t material correspond to the characteristic peaks of PDF#96-901-3415 of Fe element, PDF35-0772 of Fe3C and PDF#98-006-5119 of ZnO, indicating that the main components of the material are Fe, Fe3C and ZnO; at the same time, there is a large steamed bun peak between 20-30°, indicating the presence of amorphous carbon, which corresponds to the results of high resolution and energy spectrum.
[0071] Figure 6 This is the Raman graph of the core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention. There are obvious D peaks and G peaks in the graph, which can further prove the existence of amorphous carbon, and A D / A G The value is 3.76, indicating that there are a large number of defect sites in the material, which is conducive to the storage of potassium ions.
[0072] Figure 7 The XPS of the core-shell ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention. The presence of C, N, Fe, Co, Zn and O in the XPS total spectrum further proves the synthesis of Co-SNCS-t material. The CN bond in the fine spectrum of C mainly comes from the organic ligand. The fine spectrum analysis of N and Fe can also indicate the presence of Fe element and Fe3C phase in the material. The fine spectrum analysis of Co shows that Co is Co 2+ and Co 3+ Mixed, the ratio is about 1:1, and the detailed spectrum analysis of Zn and O can prove that ZIF-8 is mainly transformed into ZnO after high-temperature carbonization. The atomic contents of C, O, N, Fe, Co and Zn are 79.52%, 10.98%, 6.42%, 1.38%, 0.57% and 1.13%, respectively.
[0073] Figure 8 The impedance diagram of the core-shell ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention measured in a potassium ion battery. It can be seen from the figure that the charge transfer resistance R of the Co-SNCS-t material ct It is 1697 ohms, showing good conductivity.
[0074] Fig. 9 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery with a voltage of 0.5 mV s -1The CV curves were measured at a scan rate of . It can be seen from the figure that the curves have good overlap in the last two cycles, indicating that the Co-SNCS-t material has good cycle stability.
[0075] Fig.10 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. · g -1 The charge-discharge diagram measured at a current of , from which we can know that the first cycle discharge capacity of Co-SNCS-t material is 398.3mA hg -1 , the first coulombic efficiency is 52.5%.
[0076] Fig.11 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. · g -1 Performance diagram after 130 cycles at a current density of . From the figure, it can be seen that the capacity of Co-SNCS-t material remains at 186.4 mA h g after 130 cycles -1 .
[0077] Fig.12 The cobalt ion-induced synthesized core-shell ternary metal MOF derivative prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. The rate performance diagram is measured. It can be seen from the figure that even at 5A · g -1 At a current density of 69.5 mA h g -1 mass specific capacity.
[0078] Fig.13 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. · g -1 The performance diagram after 2000 cycles at a high current density is shown in the figure. It can be seen from the figure that the capacity of Co-SNCS-t material can still be maintained at 86.1 mA hg after 2000 cycles. -1 , the capacity retention rate is 93.4%.
[0079] Fig.14 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. · g -1The scanning and energy spectrum diagram after 2000 cycles at a high current density. From the figure, we can see that the structure of the Co-SNCS-t material remains intact after 2000 cycles, and the rod structure is not destroyed. It’s just that the surface of the rod has become smoother due to the attachment of a layer of binder and electrolyte layer, and the diameter of the entire rod has not changed significantly. Compared with the initial 110nm, the rod diameter only increases by 5nm after 2000 cycles, which is basically negligible. This more intuitively proves that the Co-SNCS-t material has a good structural stability, which provides a guarantee for its excellent cycle stability.
[0080] Fig.15 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery with a voltage of 0.5 mV s -1 The CV curves at different temperatures measured at a scan rate of . It can be seen from the figure that with the increase of temperature, the corresponding CV curve area only increases slightly, which further indicates that the Co-SNCS-t material also has good cycle stability at high temperatures.
[0081] Fig.16 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. · g -1 The performance diagram after 100 cycles at a current density of 1.58 Å. From the figure, it can be seen that the capacity of Co-SNCS-t material can still be maintained at 193.58 mA hg after 100 cycles. -1 .
[0082] Fig.17 The cobalt ion induced synthesized core-shell structure ternary metal MOF derivative prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. The rate performance diagram is measured. It can be seen from the figure that at 45°C, due to the faster ion transmission rate, at 5A · g -1 Co-SNCS-t material can have a current density of up to 99.8 mA hg -1 mass specific capacity.
[0083] Fig.18 The core-shell structure ternary metal MOF derivative synthesized by cobalt ion induction prepared in the embodiment of the present invention is used as the negative electrode material and assembled into a potassium ion battery. · g -1 The performance diagram after 300 cycles at a current density of 1.38 Å. From the figure, it can be seen that the capacity of Co-SNCS-t material can still be maintained at 168.3 mA h g after 300 cycles.-1 , which further demonstrates that the material has an excellent cycle stability and can be used in high temperature environments.
[0084] Comparative Example 1
[0085] (1) Cobalt nitrate hexahydrate, ferric chloride hexahydrate and 2-aminoterephthalic acid were added in an equal molar ratio, i.e., 3 mmol of each, to 60 mL of an organic solvent, N,N-dimethylacetamide, and subjected to ultrasonic treatment at a power of 360 W for 90 min until they were completely dissolved to obtain a black solution;
[0086] (2) The prepared black solution was transferred to a 100 mL polytetrafluoroethylene stainless steel autoclave, heated from room temperature to 150°C at a heating rate of 5°C / min, and reacted for 10 h. After cooling to room temperature, it was washed with deionized water for no less than 9 times, and the centrifugal speed was 9000 rpm for 10 min until the supernatant was transparent and colorless, and then vacuum dried at 70°C for 10 h to obtain bimetallic Co-Fe MOF nanorods;
[0087] (3) After the sample is dried, it is carbonized under nitrogen atmosphere protection, and the temperature is programmed to rise from room temperature to 200 °C, kept at this temperature for 2 h, and then continued to rise to 700 °C, kept at this temperature for 2 h, and then raised to the target temperature at a heating rate of 2 °C / min to obtain the sample Co-SNs.
[0088] Comparative Example 2
[0089] (1) Cobalt nitrate hexahydrate, ferric chloride hexahydrate and 2-aminoterephthalic acid were added in an equal molar ratio, i.e., 3 mmol of each, to 60 mL of an organic solvent, N,N-dimethylacetamide, and subjected to ultrasonic treatment at a power of 360 W for 90 min until they were completely dissolved to obtain a black solution;
[0090] (2) The prepared black solution was transferred to a 100 mL polytetrafluoroethylene stainless steel autoclave, heated from room temperature to 150°C at a heating rate of 5°C / min, and reacted for 10 h. After cooling to room temperature, it was washed with deionized water for no less than 9 times, and the centrifugal speed was 9000 rpm for 10 min until the supernatant was transparent and colorless, and then vacuum dried at 70°C for 10 h to obtain bimetallic Co-Fe MOF nanorods;
[0091] (3) 405 mg of Co-Fe MOF nanorods were added to 30 mL of methanol solution containing 1.5 g of PVP, and ultrasonically treated for 20 min at a power of 360 W, followed by stirring for 12 h to obtain a PVP-functionalized Co-Fe MOF suspension;
[0092] (4) Washing with methanol, centrifuging at 8000 rpm for 8 min each time, washing with methanol twice, and then ultrasonically dispersing the sample in 45 mL of methanol solution again, with an ultrasonic power of 360 W and an ultrasonic time of 2 h to obtain a dark brown PVP functionalized Co-Fe MOF suspension;
[0093] (5) Zinc nitrate hexahydrate and 2-methylimidazole were added to 9 mL of dark brown PVP functionalized Co-Fe MOF suspension in an equal molar ratio, i.e., 0.4 mmol each, and then 320 mL of methanol solution was added. After stirring for 2 h to mix evenly, the mixture was allowed to stand for 24 h at room temperature. The mixture was then washed twice by centrifugation with methanol at a speed of 7000 rpm for 7 min. After the sample was dried, it was carbonized under nitrogen atmosphere protection, and the temperature was programmed to rise from room temperature to 200 ° C for 2 h, then continued to rise to 700 ° C for 2 h, and then continued to rise to the target temperature at a heating rate of 2 ° C / min to obtain the sample Co-SNCS-p.
[0094] Comparative Example 3
[0095] (1) Cobalt nitrate hexahydrate, ferric chloride hexahydrate and 2-aminoterephthalic acid were added in an equal molar ratio, i.e., 3 mmol of each, to 60 mL of an organic solvent, N,N-dimethylacetamide, and subjected to ultrasonic treatment at a power of 360 W for 90 min until they were completely dissolved to obtain a black solution;
[0096] (2) The prepared black solution was transferred to a 100 mL polytetrafluoroethylene stainless steel autoclave, heated from room temperature to 150°C at a heating rate of 5°C / min, and reacted for 10 h. After cooling to room temperature, it was washed with deionized water for no less than 9 times, and the centrifugal speed was 9000 rpm for 10 min until the supernatant was transparent and colorless, and then vacuum dried at 70°C for 10 h to obtain bimetallic Co-Fe MOF nanorods;
[0097] (3) 405 mg of Co-Fe MOF nanorods were added to 30 mL of methanol solution containing 1.5 g of PVP, and ultrasonically treated for 20 min at a power of 360 W, followed by stirring for 12 h to obtain a PVP-functionalized Co-Fe MOF suspension;
[0098] (4) Washing with methanol, centrifuging at 8000 rpm for 8 min each time, washing with methanol twice, and then ultrasonically dispersing the sample in 45 mL of methanol solution again, with an ultrasonic power of 360 W and an ultrasonic time of 2 h to obtain a dark brown PVP functionalized Co-Fe MOF suspension;
[0099] (5) Zinc nitrate hexahydrate and 2-methylimidazole were added to 9 mL of dark brown PVP functionalized Co-Fe MOF suspension in an equal molar ratio, i.e., 0.8 mmol each, and then 320 mL of methanol solution was added. After stirring for 2 h to mix evenly, the mixture was allowed to stand for 24 h at room temperature. The mixture was then washed twice by centrifugation with methanol at a speed of 7000 rpm for 7 min. After the sample was dried, it was carbonized under nitrogen atmosphere protection, and the temperature was programmed to rise from room temperature to 200 ° C for 2 h, then continued to rise to 700 ° C for 2 h, and then continued to rise to the target temperature at a heating rate of 2 ° C / min to obtain the sample Co-SNCS-T.
[0100] Performance Testing
[0101] The products prepared in Example 1 of the present invention and Comparative Examples 1-3 were assembled into potassium ion batteries, and a series of electrochemical performance tests were performed, as shown in the table below.
[0102]
[0103]
[0104] In summary, the core-shell structured ternary metal MOF derivative of the present invention has long cycle stability and high rate performance, and is used for the negative electrode material of potassium ion batteries, and its electrochemical performance is significantly improved, and has good application prospects.
[0105] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a cobalt ion-induced synthesis of a core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material, characterized in that: Follow the steps below in order: S1, adding cobalt salt, iron salt and organic ligand in an equal molar ratio into an organic solvent N,N-dimethylacetamide, and ultrasonically treating until they are completely dissolved to obtain a black solution, which is recorded as A; S2, transfer A to a reactor, perform solvothermal reaction at 150°C for 10 h, centrifuge the product after cooling to room temperature, wash the product with deionized water until the supernatant is transparent and colorless, and vacuum dry at 70°C for 10 h to obtain Co-Fe MOF nanorods, which are recorded as B; S3, ultrasonically dispersing B in a methanol solution containing PVP, followed by continuous stirring to obtain a PVP-functionalized Co-FeMOF suspension, denoted as C; S4, washing C with methanol at 8000 rpm for 8 min, washing twice, and then ultrasonically dispersing it in a methanol solution again to obtain a dark brown suspension, recorded as D; S5. Add cobalt salt, zinc salt and organic ligand to D in an equimolar ratio, and add methanol solution additionally, stir until they are evenly dispersed and then let stand to allow epitaxial growth. After standing for 24 hours, wash twice with methanol, centrifuge and dry, and then carbonize to obtain a ternary metal MOF derivative with a core-shell structure.
2. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S1, the cobalt salt is cobalt nitrate hexahydrate, the iron salt is ferric chloride hexahydrate, and the organic ligand is 2-aminoterephthalic acid.
3. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S2, the temperature of the solvent thermal reaction is increased at a rate of 5°C / min to the target temperature.
4. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S2, the centrifugal speed is 9000 rpm, the centrifugal time is 10 min, and the number of washing times with deionized water is not less than 9 times.
5. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S3, the mass ratio of B to PVP is 27:100, and the concentration of the methanol solution of PVP is 0.05 g / mL.
6. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S5, the cobalt salt is cobalt nitrate hexahydrate, the zinc salt is zinc nitrate hexahydrate, the organic ligand is 2-methylimidazole, and the molar volume ratio of the cobalt salt to D and the methanol solution is 0.4 mmol:9 mL:320 mL.
7. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S5, the centrifugal speed is 7000 rpm and the time is 7 min.
8. The method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 1, characterized in that: In step S5, the carbonization treatment is carried out under the protection of a nitrogen atmosphere according to the following procedure: The first stage: heating from room temperature to 200℃, keeping warm for 2h; The second stage: heating from 200℃ to 700℃, keeping warm for 2h; The third stage: cooling to room temperature in the furnace.
9. The method for preparing a cobalt ion-induced synthesis core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to claim 8, characterized in that: In step S5, the heating rate of the first stage and the second stage is 2°C / min.
10. A method for preparing a cobalt ion-induced synthesized core-shell structure ternary metal MOF derivative potassium ion battery negative electrode material according to any one of claims 1 to 9, characterized in that: The core-shell structured ternary metal MOF derivative has a shuttle-like morphology.
Citation Information
Patent Citations
Potassium ion battery negative electrode material metal alloy and preparation method thereof
CN112002886A
Cobalt-manganese bimetal MOFs (Metal-Organic Frameworks) derivative material as well as preparation method and application thereof
CN114335472A
Monatomic catalyst based on functionalized MOF (Metal Organic Framework) as well as preparation method and application of monatomic catalyst
CN116130686A
Ferrocobalt MOF-derived nanocube material as well as preparation method and application thereof
CN117512659A
Negative electrode active material, negative electrode material, alkaline ion battery including negative electrode material, and manufacturing method of negative electrode active material
JP2022123563A