Boron-doped porous carbon material and preparation method thereof, silicon-carbon negative electrode material and lithium ion battery

Through the preparation method of boron-doped porous carbon materials, the problems of small strength and uncontrollable pore size of porous silicon carbon negative electrode materials are solved, the electrochemical performance and stability of lithium-ion batteries are improved, and the silicon with high strength and adjustable pore size is realized Carbon negative electrode material improves the circulation performance of lithium-ion batteries.

CN118877872APending Publication Date: 2024-11-01SHAANXI EPUNO NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411051207.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The carbon negative electrode material of existing porous silicon carbon negative electrode materials has small strength and uncontrollable pore size, which leads to the particles of lithium-ion batteries being easily broken when they are embedded in lithium, affecting battery performance, and the uneven increase of silicon materials affects electrochemical performance.

Method used

Using the preparation method of boron-doped porous carbon material, by mixing, crushing, carbonizing and fusion treatment of carbon source, boron source and pore-forming agent, a boron-doped porous carbon material with high strength and adjustable pore size is formed as silicon carbon The carrier of the negative electrode material and nanosilicon particles are located in their holes, improving the stability and electrochemical properties of the material.

Benefits of technology

Improve the mechanical strength and electrochemical performance of silicon carbon negative electrode materials, weaken the diffusion energy barrier of lithium ion, enhance the stability and electrochemical performance of the material, avoid the particle breakage caused by silicon expansion, and improve the circulation of lithium ion batteries. stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877872A_ABST
    Figure CN118877872A_ABST
Patent Text Reader

Abstract

The invention provides a boron-doped porous carbon material and a preparation method thereof, a silicon-carbon negative electrode material and a lithium ion battery, and relates to the field of carbon materials. The preparation method comprises the following steps: mixing a carbon source, a boron source and a pore-forming agent to obtain a mixed material A; crushing the mixed material A to obtain a crushed material B; and carrying out carbonization treatment and fusion treatment on the crushed material B to obtain the boron-doped porous carbon negative electrode material. According to the preparation method, a boron-doped soft and hard carbon composite material is formed through carbonization treatment, and then a lamellar structure is twisted, disordered and unstable layered carbon material through fusion treatment, so that the structure of the layered carbon material is tighter.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of carbon materials, and in particular to a boron-doped porous carbon material and a preparation method thereof, a silicon-carbon negative electrode material and a lithium-ion battery. Background Art

[0002] In recent years, people have an increasing demand for long-range and lightweight 3C electronic products and electric vehicles, which has put forward higher requirements on the performance of lithium-ion batteries, especially electrode materials. Silicon materials have become the focus and hot spot of current electrode material research and development due to their ultra-high theoretical specific capacity, wide sources and low cost. However, as a new generation of commercial negative electrode materials, silicon / carbon negative electrode materials still have many problems.

[0003] Si anodes usually undergo significant volume changes during electrochemical cycles, leading to particle crushing, loss of electrical contact, and rupture of the solid electrolyte interphase (SEI), which in turn leads to rapid deterioration of storage performance. People have explored various strategies to alleviate these limitations. Among them, silicon-carbon negative electrode materials grown by vapor deposition have shown good application prospects in the market, but the choice of carbon materials that carry the deposited silicon has a very important impact on its overall performance. Porous silicon-carbon negative electrode materials use porous carbon as a carrier to deposit the silicon source into the pores of porous carbon under a certain temperature and pressure to form silicon-carbon negative electrode materials. The pores of porous carbon are mainly micropores, and the deposited silicon is separated by the micropores of porous carbon. There are no large particles of silicon, and the expansion stress is small. At the same time, the porous structure of porous carbon provides space for the expansion of silicon. Porous carbon is the core material of porous silicon-carbon negative electrode materials. The morphology and pore structure of porous carbon have a significant impact on the silicon source deposition conditions and the performance of porous silicon-carbon negative electrode materials. At present, most of the raw porous carbons used in porous silicon-carbon negative electrode materials have various problems such as low strength and uncontrollable pore size. The carbon negative electrode materials with low strength are easily broken by the force when they are expanded by lithium insertion, which affects the battery performance. Even when preparing the electrode roll, the particles overlap with each other and are easily crushed by shear force, resulting in a decrease in the first efficiency. At the same time, the problem of uncontrollable pore size will also lead to the uneven growth of silicon materials during the deposition process, affecting the electrochemical properties of the final material.

[0004] Therefore, how to prepare porous carbon materials with excellent electrochemical properties is a problem that needs to be solved urgently. Summary of the invention

[0005] The purpose of the present application is to provide a boron-doped porous carbon material and a preparation method thereof, a silicon-carbon negative electrode material and a lithium-ion battery to solve the above-mentioned problems.

[0006] To achieve the above objectives, the present application provides a first aspect of a method for preparing a boron-doped porous carbon material, comprising:

[0007] Mixing a carbon source, a boron source and a pore-forming agent to obtain a mixture A;

[0008] The mixed material A is crushed to obtain a crushed material B;

[0009] Carbonizing the crushed material B to obtain a carbonized material C;

[0010] The carbonized material is fused to obtain a boron-doped porous carbon negative electrode material.

[0011] Optionally, the carbon source includes one or more of asphalt, resin, glucose and sucrose.

[0012] Optionally, the method for preparing the boron-doped porous carbon material satisfies at least one of the following conditions:

[0013] A. the boron source comprises boric acid;

[0014] B. The pore-forming agent includes one or more of sodium chloride, potassium chloride, sodium carbonate and potassium carbonate.

[0015] Optionally, the method for preparing the boron-doped porous carbon material satisfies at least one of the following conditions:

[0016] A. The mass ratio of the carbon source to the pore-forming agent is (6-9): (1-4);

[0017] B. The mass ratio of the carbon source to the boron source is (7-9):1.

[0018] Optionally, the method for preparing the boron-doped porous carbon material satisfies at least one of the following conditions:

[0019] A. the carbonization treatment includes a first carbonization treatment and a second carbonization treatment;

[0020] The temperature of the first carbonization treatment is 350°C-650°C, and the time is 1h-3h;

[0021] The temperature of the second carbonization treatment is 900°C-1300°C, and the time is 1h-3h;

[0022] B. The heating rate of the carbonization treatment is 1°C / min-5°C / min.

[0023] Optionally, the rotation speed of the fusion process is 1500r / min-2500r / min, and the fusion time is 5min-20min.

[0024] Optionally, washing and screening are performed after the fusion treatment to obtain the boron-doped porous carbon material;

[0025] The sieve aperture of the sieving is 100 mesh to 1000 mesh.

[0026] A second aspect of the present application provides a boron-doped porous carbon material, which is prepared by the method for preparing the boron-doped porous carbon material.

[0027] The third aspect of the present application provides a silicon-carbon negative electrode material, comprising the boron-doped porous carbon material and nano-silicon particles located in the pores of the boron-doped porous carbon material.

[0028] A fourth aspect of the present application provides a lithium-ion battery, comprising the boron-doped porous carbon material or the silicon-carbon negative electrode material.

[0029] Compared with the prior art, the beneficial effects of this application include:

[0030] The present application provides a method for preparing a boron-doped porous carbon material, which comprises mixing a carbon source, a boron source and a pore-forming agent simultaneously to obtain a mixed material A, crushing the mixed material A to fully mix the mixed material A while reducing the particle size, and then performing a carbonization treatment to form a boron-doped soft and hard carbon composite material, and then performing a fusion treatment to twist the layered structure of the disordered and unstable layered carbon material to make its structure more compact.

[0031] The boron-doped porous carbon material provided by the present application, on the one hand, boron atoms are introduced into the lattice of the porous carbon material to replace the position of a part of carbon atoms, and the boron atoms have a higher electronegativity and can form chemical bonds different from those of carbon atoms in the graphite structure; on the second hand, the interaction between the boron atoms and the lithium ions can weaken the diffusion energy barrier of the lithium ions in the graphite material and increase the migration rate of the lithium ions; on the third hand, the porous carbon material of the present application is a soft and hard carbon composite material, lacking a long-range ordered structure and an ordered stacking structure, and the lamellar structure is distorted, disordered and unstable. The introduction of boron atoms can effectively play a pinning role and improve its stability, and the introduction of boron atoms changes the surface properties of the porous carbon material and introduces defects on the surface of the porous carbon material.

[0032] The silicon-carbon negative electrode material provided in the present application uses a boron-doped porous carbon material as a precursor, and the nano-silicon particles are located in the voids of the boron-doped porous carbon material. The weakly electronegative boron will change the electronic environment of the boron-doped porous carbon material carrier near the silicon particles, which is more conducive to the reduction and growth of silicon on the boron-doped porous carbon material during CVD deposition of silicon.

[0033] The lithium-ion battery provided in this application has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.

[0035] Figure 1 It is a schematic diagram of fusion processing;

[0036] Figure 2 A schematic diagram of a process for preparing a boron-doped porous carbon material provided in Example 1;

[0037] Figure 3 This is a schematic flow chart of the preparation method of the boron-doped porous carbon material provided in Comparative Example 5. DETAILED DESCRIPTION

[0038] As used herein:

[0039] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0040] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.

[0041] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values ​​and all integers and fractions within the range.

[0042] In these examples, parts and percentages are by mass unless otherwise indicated.

[0043] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.

[0044] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0045] The first aspect of the present application provides a method for preparing a boron-doped porous carbon material, comprising:

[0046] Mixing a carbon source, a boron source and a pore-forming agent to obtain a mixture A;

[0047] The mixed material A is crushed to obtain a crushed material B;

[0048] Carbonizing the crushed material B to obtain a carbonized material C;

[0049] The carbonized material is fused to obtain a boron-doped porous carbon negative electrode material.

[0050] In some embodiments, the carbon source includes one or more of asphalt, resin, glucose, and sucrose.

[0051] In some embodiments, the method for preparing the boron-doped porous carbon material satisfies at least one of the following conditions:

[0052] A. the boron source comprises boric acid;

[0053] B. The pore-forming agent includes one or more of sodium chloride, potassium chloride, sodium carbonate and potassium carbonate.

[0054] In some embodiments, the method for preparing the boron-doped porous carbon material satisfies at least one of the following conditions:

[0055] A. The mass ratio of the carbon source to the pore-forming agent is (6-9): (1-4);

[0056] Optionally, the mass ratio of the carbon source to the pore-forming agent may be 6:1, 7:2, 8:3, 9:4 or any value between (6-9):(1-4);

[0057] It should be noted that when the mass ratio of carbon source to pore former is (6-9):(1-4), the pore size of the resulting porous carbon material can effectively deposit silicon material without causing the overall structure to break.

[0058] B. The mass ratio of the carbon source to the boron source is (7-9):1.

[0059] Optionally, the mass ratio of the carbon source to the boron source can be 7:1, 8:1, 9:1 or any value between (7-9):1.

[0060] In some embodiments, the method for preparing the boron-doped porous carbon material satisfies at least one of the following conditions:

[0061] A. the carbonization treatment includes a first carbonization treatment and a second carbonization treatment;

[0062] The temperature of the first carbonization treatment is 350°C-650°C, and the time is 1h-3h;

[0063] Optionally, the temperature of the first carbonization treatment may be 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C or any value between 350°C and 650°C, and the time may be 1h, 2h, 3h or any value between 1h and 3h;

[0064] The temperature of the second carbonization treatment is 900°C-1300°C, and the time is 1h-3h;

[0065] Optionally, the temperature of the second carbonization treatment may be 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1250°C, 1300°C or any value between 900°C and 1300°C, and the time may be 1h, 2h, 3h or any value between 1h and 3h;

[0066] It should be noted that the crushed material undergoes dehydrogenation, chain breaking, condensation, polymerization and other reactions during the first carbonization treatment, i.e., low-temperature carbonization, so that the aromatic molecules continue to grow to form large planar lamellar molecules; when the molecular size reaches a certain extent, the aromatic molecules are stacked up under the action of the delocalized non-covalent large π-π bonds between the lamellar layers to form intermediate phase building units. In the early stage of intermediate phase formation, these building units act as the nucleus for further growth of the intermediate phase. Then, the second carbonization treatment is carried out, i.e., as the heat treatment deepens, the building units gradually appear, and these subsequently generated building units will accumulate on the core of the intermediate phase to form the intermediate phase. The growth process of the intermediate phase is a process of continuous accumulation of the continuously formed building units, and finally the carbonized material is formed.

[0067] B. The heating rate of the carbonization treatment is 1°C / min-5°C / min.

[0068] Optionally, the heating rate of the carbonization treatment may be 1°C / min, 2°C / min, 3°C / min, 4°C / min, or 5°C / min, and may be any value between 1°C / min and 5°C / min.

[0069] In some embodiments, the rotation speed of the fusion process is 1500r / min-2500r / min, and the fusion time is 5min-20min.

[0070] Optionally, the rotation speed of the fusion treatment can be 1500r / min, 2000r / min, 2500r / min or any value between 1500r / min-2500r / min, and the fusion time can be 5min, 10min, 15min, 20min or any value between 5min-20min.

[0071] It should be noted that if Figure 1 As shown, fusion processing means that the material moves at high speed under the drive of the rotor, and a blade is added to the path of the material to limit the width of the path, so that a certain force can be applied to the surface of the material.

[0072] It should also be noted that the carbonized material will have a certain structural expansion after carbonization. Through fusion treatment, a combination of compression force, shear force and impact force can be applied to the carbonized material, making the carbonized material structure denser without adhesive. In addition, through fusion treatment, the spike-like structure on the surface of the carbonized material can be polished smooth to reduce the polarization effect of the material.

[0073] In some embodiments, the fusion treatment is followed by washing and sieving to obtain the boron-doped porous carbon material;

[0074] The sieve aperture of the sieving is 100 mesh to 1000 mesh.

[0075] Optionally, the sieve hole diameter of the screening can be 100 mesh, 200 mesh, 300 mesh, 400 mesh, 500 mesh, 600 mesh, 700 mesh, 800 mesh, 900 mesh, 1000 mesh or any value between 100 mesh and 1000 mesh.

[0076] A second aspect of the present application provides a boron-doped porous carbon material, which is prepared by the method for preparing the boron-doped porous carbon material.

[0077] The third aspect of the present application provides a silicon-carbon negative electrode material, comprising the boron-doped porous carbon material and nano-silicon particles located in the pores of the boron-doped porous carbon material.

[0078] Exemplarily, the silicon-carbon negative electrode material is obtained by subjecting the boron-doped porous carbon material to CVD vapor deposition and depositing a certain amount of silicon material in its pores.

[0079] It should be noted that the boron-doped porous carbon material prepared in the present application is used as a porous carbon source precursor for the silicon-carbon negative electrode material. The silicon-carbon negative electrode material has the characteristics of high mechanical strength and adjustable pore size and porous density. When it is used for chemical vapor deposition to prepare silicon-carbon material, silane gas can enter the pores more easily, and it is beneficial for the silane gas to decompose and deposit in the pores at high temperature. The higher strength can not only keep the particle structure intact after rolling, but also avoid the problem of particle breakage caused by the violent expansion of silicon during the cycle, and avoid the problem of increased side reactions caused by the breakage of the material structure during the charge and discharge process, thereby improving the cycle stability of the material.

[0080] A fourth aspect of the present application provides a lithium-ion battery, comprising the boron-doped porous carbon material or the silicon-carbon negative electrode material.

[0081] It should be noted that the boron-doped porous carbon material prepared in the present application can be used as a porous carbon source precursor for silicon-carbon negative electrode materials, and can also be used as a negative electrode material for lithium-ion batteries.

[0082] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0083] Example 1

[0084] A first aspect of the present embodiment provides a method for preparing a boron-doped porous carbon material, comprising:

[0085] S1: taking a certain amount of asphalt, sodium chloride and boric acid and adding them into a mixer for mixing to obtain material A, the mixing speed is 2500 rpm, the mixing time is 5 min, the mass ratio of asphalt to sodium chloride is 6:4, and the mass ratio of asphalt to boric acid is 9:1;

[0086] S2: Add material A into a ball mill and perform ball milling to obtain material B. The particle size of material B can be adjusted according to the needs, such as the ball milling time. The particle size of this ball milling is about 1um.

[0087] S3: Carbonizing material B at a heating rate of 2°C / min, heating to 450°C and keeping the temperature for 2h, and then heating to 1200°C at the same heating rate and keeping the temperature for 2h to obtain material C;

[0088] S4: crushing material C and fusing it to obtain material D, with a fusing speed of 2000 rpm and a fusing time of 3 min;

[0089] S5: Finally, the material D is washed, dried and sieved to obtain a boron-doped porous carbon material, and the sieve aperture is 300 meshes.

[0090] The preparation method steps of this embodiment are as follows Figure 2 shown.

[0091] A second aspect of the present embodiment provides a boron-doped porous carbon material, which is prepared by the above-mentioned method for preparing the boron-doped porous carbon material.

[0092] A third aspect of this embodiment provides a lithium-ion battery, comprising the above-mentioned boron-doped porous carbon material.

[0093] Example 2

[0094] A first aspect of the present embodiment provides a method for preparing a boron-doped porous carbon material, comprising:

[0095] S1: Take a certain amount of asphalt, phenolic resin and glucose in a mass ratio of 4:1:1 and mix them to obtain a carbon source. Add the carbon source, sodium chloride and boric acid into a mixer and mix them to obtain material A. The mixing speed is 2500 rpm and the mixing time is 5 min. The mass ratio of asphalt to sodium chloride is 8:1, and the mass ratio of asphalt to boric acid is 9:1.

[0096] S2: Add material A into a ball mill and perform ball milling to obtain material B. The particle size of material B can be adjusted according to the needs, such as the ball milling time. The particle size of this ball milling is about 5um.

[0097] S3: Carbonizing material B at a heating rate of 2°C / min, heating to 550°C and keeping the temperature for 2h, and then heating to 1200°C at a heating rate of 3°C / min and keeping the temperature for 2h to obtain material C;

[0098] S4: crushing material C and fusing it to obtain material D, with a fusing speed of 2000 rpm and a fusing time of 3 min;

[0099] S5: Finally, the material D is washed, dried and sieved to obtain a boron-doped porous carbon material, and the sieve aperture is 300 meshes.

[0100] A second aspect of the present embodiment provides a boron-doped porous carbon material, which is prepared by the above-mentioned method for preparing the boron-doped porous carbon material.

[0101] The third aspect of this embodiment provides a silicon-carbon negative electrode material. 100 g of the boron-doped porous carbon material is added into a fixed bed of a fluidized bed reactor. The air inlets are connected to and adjusted to 500 cm nitrogen as a carrier gas. 3 / min, silane 10cm 3 / min, ethylene 5cm 3 / min of air intake, with a silane and ethylene feed ratio of 2:1, and deposition at a temperature of 500°C fluidized bed for 1 hour. After vapor deposition, the reactor temperature is raised to 1000°C, and the vapor deposited material is solid-phase sintered for 1 hour to obtain the silicon-carbon negative electrode material.

[0102] A fourth aspect of this embodiment provides a lithium-ion battery, comprising the above-mentioned silicon-carbon negative electrode material.

[0103] Example 3

[0104] A first aspect of the present embodiment provides a method for preparing a boron-doped porous carbon material, comprising:

[0105] S1: Take a certain amount of asphalt and phenolic resin in a mass ratio of 3:1 and mix them to obtain a carbon source. Add the carbon source, sodium chloride and boric acid into a mixer and mix them to obtain material A. The mixing speed is 2500 rpm and the mixing time is 5 min. The mass ratio of asphalt to sodium chloride is 6:4 and the mass ratio of asphalt to boric acid is 9:1.

[0106] S2: Add material A into a ball mill and perform ball milling to obtain material B. The particle size of material B can be adjusted according to the needs, such as the ball milling time. The particle size of this ball milling is about 5um.

[0107] S3: Carbonizing material B at a heating rate of 2°C / min, heating to 550°C and keeping the temperature for 2h, and then heating to 1300°C at a heating rate of 5°C / min and keeping the temperature for 2h to obtain material C;

[0108] S4: crushing material C and fusing it to obtain material D, with a fusing speed of 2000 rpm and a fusing time of 3 min;

[0109] S5: Finally, the material D is washed, dried and sieved to obtain a boron-doped porous carbon material, and the sieve aperture is 500 mesh.

[0110] A second aspect of the present embodiment provides a boron-doped porous carbon material, which is prepared by the above-mentioned method for preparing the boron-doped porous carbon material.

[0111] A third aspect of this embodiment provides a lithium-ion battery, comprising the above-mentioned boron-doped porous carbon material.

[0112] Comparative Example 1

[0113] This comparative example provides a porous carbon material and a preparation method thereof and a lithium ion battery. The difference from Example 1 is that in step S1 of this comparative example, no boron source is added, and other conditions are consistent with those of Example 1.

[0114] Comparative Example 2

[0115] This comparative example provides a boron-doped carbon material and a preparation method thereof and a lithium-ion battery. The difference from Example 1 is that in step S1 of this comparative example, no pore-forming agent is added, and other conditions are consistent with Example 1.

[0116] Comparative Example 3

[0117] This comparative example provides a boron-doped carbon material, a preparation method thereof, and a lithium-ion battery. The difference from Example 1 is that in step S1 of this comparative example, the mass ratio of the carbon source and the boron source of the pore-forming agent is 4:1:1, and other conditions are consistent with Example 1.

[0118] Comparative Example 4

[0119] This comparative example provides a boron-doped carbon material and a preparation method thereof and a lithium-ion battery. The difference from Example 1 is that the carbonization treatment in this comparative example is only performed for one stage at a temperature of 800° C., and other conditions are consistent with Example 1.

[0120] Comparative Example 5

[0121] This comparative example provides a boron-doped carbon material and a preparation method thereof and a lithium-ion battery. The difference from Example 1 is that this comparative example does not perform fusion treatment, and other conditions are consistent with Example 1.

[0122] The schematic diagram of the process of this comparative example is as follows Figure 3 shown.

[0123] The electrochemical performance tests were performed on the above embodiments and comparative examples, and the specific test results are shown in Table 1.

[0124] Table 1 Electrochemical performance test

[0125]

[0126] As can be seen from Table 1, the initial calibration of the material in Example 1 reaches 88.2% and the capacity retention rate reaches 95.6%, which is significantly better than the comparative materials. The silicon-carbon negative electrode material prepared from the boron-doped porous carbon material prepared by the present invention (Example 2) also exhibits good electrochemical properties.

[0127] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.

[0128] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.

Claims

1. A method for preparing a boron-doped porous carbon material, characterized in that: include: Mixing a carbon source, a boron source and a pore-forming agent to obtain a mixture A; The mixed material A is crushed to obtain a crushed material B; Carbonizing the crushed material B to obtain a carbonized material C; The carbonized material is fused to obtain a boron-doped porous carbon negative electrode material.

2. The method for preparing a boron-doped porous carbon material according to claim 1, characterized in that: The carbon source includes one or more of asphalt, resin, glucose and sucrose.

3. The method for preparing a boron-doped porous carbon material according to claim 1, characterized in that: At least one of the following conditions is met: A. the boron source comprises boric acid; B. The pore-forming agent includes one or more of sodium chloride, potassium chloride, sodium carbonate and potassium carbonate.

4. The method for preparing a boron-doped porous carbon material according to claim 1, characterized in that: At least one of the following conditions is met: A. The mass ratio of the carbon source to the pore-forming agent is (6-9): (1-4); B. The mass ratio of the carbon source to the boron source is (7-9):

1.

5. The method for preparing a boron-doped porous carbon material according to claim 1, characterized in that: At least one of the following conditions is met: A. the carbonization treatment includes a first carbonization treatment and a second carbonization treatment; The temperature of the first carbonization treatment is 350°C-650°C, and the time is 1h-3h; The temperature of the second carbonization treatment is 900°C-1300°C, and the time is 1h-3h; B. The heating rate of the carbonization treatment is 1°C / min-5°C / min.

6. The method for preparing a boron-doped porous carbon material according to claim 1, characterized in that: The rotation speed of the fusion process is 1500r / min-2500r / min, and the fusion time is 5min-20min.

7. The method for preparing a boron-doped porous carbon material according to claim 1, characterized in that: After the fusion treatment, washing and screening are performed to obtain the boron-doped porous carbon material; The sieve aperture of the sieving is 100 mesh to 1000 mesh.

8. A boron-doped porous carbon material, characterized in that: The boron-doped porous carbon material is prepared by the preparation method of any one of claims 1 to 7.

9. A silicon-carbon negative electrode material, characterized in that: The method comprises the boron-doped porous carbon material as claimed in claim 8 and nano-silicon particles located in the pores of the boron-doped porous carbon material.

10. A lithium ion battery, characterized in that: It includes the boron-doped porous carbon material as described in claim 8 or the silicon-carbon negative electrode material as described in claim 9.

Citation Information

Patent Citations

  • Method for preparing boron-doped porous carbon spheres

    CN107346821A

  • Preparation method of boron-doped porous carbon material and application of boron-doped porous carbon material in potassium ion battery

    CN114530601A

  • Silicon-carbon composite material, preparation method thereof and lithium ion battery

    CN117133910A

  • Silicon-carbon negative electrode material for battery and preparation method of silicon-carbon negative electrode material

    CN117878276A

Cited By

  • Spherical porous carbon as well as preparation method and application thereof

    CN119976806A

  • A spherical porous carbon, its preparation method and application

    CN119976806B

  • Boron-fluorine co-doped porous carbon material, preparation method thereof and silicon-carbon negative electrode material

    CN122685069A