Preparation method and application of porous graphitized carbon material
By first carbonizing waste biomass raw materials and then graphitizing, porous graphitized carbon materials with rich mesoporous and macroporous structures were prepared, which solved the problem of poor charging and discharging performance of graphite under high current density, and significantly improved lithium-ion batteries The cycle and rate performance have the potential to replace commercial graphite.
Patent Information
- Application Number
- CN202410810132.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-11-01
AI Technical Summary
The existing lithium-ion battery negative electrode material graphite has poor charging and discharge performance under high current density, and there is a risk of lithium-ion reaction and thermal runaway. There are few reports of porous graphitized carbon materials developed with waste biomass as raw materials, making it difficult to replace commercial graphite.
By crushing, washing and drying the waste biomass raw materials, carbonizing and then graphitizing, porous graphitized carbon materials with rich mesoporous and macroporous structures are prepared for lithium-ion battery negative electrode materials, and the materials are improved. Rate performance.
The prepared porous graphitized carbon materials have significant graphitization degree and structural differences, which significantly improve the circulation and rate performance of lithium-ion batteries, and have the potential to replace commercial graphite, especially in the popularization of negative electrode materials for fast charging lithium batteries. and have advantages in development.
Smart Images

Figure CN118877883A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a method for preparing a porous graphitized carbon material and an application thereof. Background Art
[0002] Under the "dual carbon" policy, new energy vehicles are developing rapidly, and the share of pure electric (EV) and hybrid (HEV) vehicles in the passenger car market is increasing year by year. Lithium-ion batteries have become the first choice for new energy vehicle power batteries due to their high energy density, long cycle life, low self-discharge, high operating voltage and no pollution. However, new energy vehicles, especially pure electric vehicles, still have some shortcomings that are difficult for consumers to accept, mainly the shorter driving range and longer charging time of lithium-ion batteries. Improving the charging rate of power batteries is an effective way to overcome mileage anxiety and promote the acceptance of pure electric vehicles. Graphite, as the main negative electrode material for commercial lithium-ion batteries, has high energy density, low production cost and stable electrochemical performance. However, when working at a higher current density, the charge and discharge capacity of graphite is greatly reduced, and there is a risk of lithium precipitation reaction and thermal runaway. Therefore, it is urgent to develop negative electrode materials with better rate performance to overcome the fast charging performance defects of graphite.
[0003] In recent years, researchers have modified and composited graphite materials to improve the performance of graphite in order to improve the material's cycle performance and rate performance, but due to factors such as cost, it is difficult to gain wide popularity in the market. As a potential resource on the earth (low cost, abundant reserves and variety, green and sustainable), biomass has attracted many researchers to develop promising energy storage materials using various types of biomass as raw materials. However, current research mostly uses biomass as raw material to develop hard carbon energy storage materials. Although hard carbon has high energy density and good rate performance, its large specific surface area and rich pore structure cause large active lithium consumption during charging and discharging, and low first coulomb efficiency. This is also an important reason why hard carbon is difficult to replace graphitized carbon and gain popularity in the market. At present, the rate performance of graphite negative electrode materials is poor, and there are few reports on the development of porous graphitized carbon using waste biomass as raw materials. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for preparing a porous graphitized carbon material and its application, so that the prepared graphitized carbon has a high degree of graphitization and a structure with abundant meso-macroporous pores surrounded by graphite sheets, and has the potential to replace commercial graphite, thus having good prospects in lithium-ion battery negative electrode materials.
[0005] The present invention solves the above technical problems by the following technical means:
[0006] A method for preparing a porous graphitized carbon material comprises the following steps:
[0007] S1. crushing the waste biomass raw material and passing it through a 40-60 mesh sieve to obtain granules;
[0008] S2. The particles are placed in deionized water and stirred for washing for 6 to 12 hours, filtered, and dried until completely dry to obtain a biomass precursor;
[0009] S3. The biomass precursor is placed in a graphite crucible and placed in a high temperature furnace, carbonized at 1200 to 1600°C, and then heated to 2600 to 3200°C for graphitization to obtain a black residue;
[0010] S4. The obtained black residue is placed in deionized water and stirred for washing for 6 to 12 hours, filtered, dried until completely dry, ball-milled, and passed through a 100 to 200 mesh sieve to obtain a porous graphitized carbon material.
[0011] According to the above technical means, by crushing, washing and drying the waste biomass raw materials, impurities such as water-soluble inorganic salts and ash in the waste biomass particles that affect the subsequent activation steps can be removed, and then through two-stage activation, the waste biomass raw materials can be carbonized first and then graphitized, so as to prepare a porous graphitized carbon material in a simple way. The porous graphitized carbon material has rich mesopores and macropores, and its microscopic morphology is a graphite sheet structure surrounding the mesopores and macropores, which is significantly different from the graphite layer structure of commercial graphite stacking, and has the potential to replace commercial graphite.
[0012] Preferably, the waste biomass raw materials include one or more combinations of pine wood chips, corn stalks, rice stalks, pine bark, birch bark, ginkgo leaves, corn leaves, coconut shells, walnut shells, rice husks, corn cobs, and cotton.
[0013] More preferably, the waste biomass raw material is pine sawdust.
[0014] According to the above technical means, pine sawdust has a porous structure, low bound water content, low ash content, high cellulose content, and especially high lignin content, which is conducive to the formation of graphitized structure during the activation process. Corn cobs, cotton and other low-lignin waste biomass are not used because their graphitization effect is poor.
[0015] Preferably, in the step S1, during the pulverization, one or more combinations of a crusher, a ball mill and a pulverizer are used.
[0016] Preferably, in steps S2 and S4, during filtration, one or more combinations of normal pressure filtration, reduced pressure filtration, vacuum filtration, centrifugal filtration and membrane filtration are used.
[0017] More preferably, during filtration, normal pressure filtration is adopted.
[0018] Preferably, in steps S2 and S4, during drying, one or more combinations of forced air drying, vacuum drying, spray drying, reduced pressure drying, far infrared radiation drying, heating drying and natural drying are used.
[0019] More preferably, vacuum drying is used during drying.
[0020] Preferably, in the step S3, during carbonization, the carbonization time is 1 to 3 hours.
[0021] According to the above technical means, the complete carbonization of the material can be ensured while saving energy.
[0022] Preferably, in the step S3, the temperature is increased at a heating rate of 1 to 5°C / min.
[0023] Preferably, in the step S3, during graphitization, the graphitization time is 1 to 3 hours.
[0024] According to the above technical means, the degree of graphitization can be made as high as possible under the premise of saving energy consumption.
[0025] Further preferably, during graphitization, one of an Acheson graphitization furnace, an inner-string graphitization furnace, an induction graphitization furnace and a carbon tube furnace is used.
[0026] The present application also discloses an application of a graphitized carbon material prepared by the method for preparing the porous graphitized carbon material as shown above, which is used as a negative electrode material for lithium-ion batteries.
[0027] Preferably, when preparing the negative electrode material for a lithium ion battery, the following steps are included:
[0028] S10. The graphitized carbon material, the conductive carbon black and the polyvinylidene fluoride are mixed in N-methylpyrrolidone and stirred for 6 to 12 hours to form a slurry;
[0029] S20. The slurry is coated on a copper foil and dried in a vacuum oven at 90° C. to prepare a negative electrode material.
[0030] Further preferably, in the step S10, the mass ratio of the graphitized carbon material, the conductive carbon black and the polyvinylidene fluoride is 8:1:1.
[0031] More preferably, in the step S20, when the slurry is coated on the copper foil, the coating thickness is 100-150 μm.
[0032] The present application adopting the above scheme has the following advantages:
[0033] 1. The present application uses two-stage activation to first carbonize and then graphitize the waste biomass raw materials, thereby preparing a porous graphitized carbon material in a simple way. The porous graphitized carbon material has a rich mesoporous and macroporous structure, and its microscopic morphology is a graphite sheet structure surrounding the mesopores and macropores, which is significantly different from the graphite layer structure of commercial graphite stacking, and has the potential to replace commercial graphite;
[0034] 2. By using porous pine sawdust graphitized carbon as the negative electrode material for lithium batteries, under the same conditions, it has better cycle performance and rate performance than commercial graphite, which is conducive to the popularization and development of fast-charging negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The present application may be further illustrated by non-limiting examples given in the accompanying drawings;
[0036] Figure 1 is a Raman spectrum comparison diagram of the porous graphitized carbon material and commercial graphite in the embodiment of the present application;
[0037] Figure 2 is a comparison diagram of the pore size distribution of the porous graphitized carbon material and commercial graphite in the embodiment of the present application;
[0038] Figure 3 is a SEM comparison diagram of the porous graphitized carbon material and commercial graphite in the embodiment of the present application;
[0039] Figure 4 It is a comparison chart of the rate performance test of the porous graphitized carbon material and commercial graphite in the embodiment of the present application. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention:
[0041] Example 1, Preparation method of porous graphitized carbon material
[0042] S1. The porous pine sawdust is crushed by a crusher and passed through a 40-60 mesh sieve to obtain granules;
[0043] S2. The particles are placed in deionized water and stirred for washing for 6 to 12 hours, filtered under normal pressure, and vacuum dried until completely dry to obtain a biomass precursor;
[0044] S3. The biomass precursor is placed in a graphite crucible and placed in a graphitization furnace, carbonized at 1200°C for 3 hours, then heated to 2600°C at a heating rate of 1-5°C / min, and graphitized at 2600°C for 1 hour to obtain a black residue;
[0045] S4. The obtained black residue is placed in deionized water and stirred for washing for 6 to 12 hours, filtered at normal pressure, vacuum dried until completely dry, ball-milled, and sieved through a 100 to 200 mesh screen to obtain a porous graphitized carbon material.
[0046] Example 2, Preparation Method 2 of Porous Graphitized Carbon Material
[0047] S1. The porous pine sawdust is crushed by a crusher and passed through a 40-60 mesh sieve to obtain granules;
[0048] S2. The particles are placed in deionized water and stirred for washing for 6 to 12 hours, filtered under normal pressure, and vacuum dried until completely dry to obtain a biomass precursor;
[0049] S3. The biomass precursor is placed in a graphite crucible and placed in a graphitization furnace, carbonized at 1500°C for 2h, then heated to 2800°C at a heating rate of 1-5°C / min, and graphitized at 2800°C for 2h to obtain a black residue;
[0050] S4. The obtained black residue is placed in deionized water and stirred for washing for 6 to 12 hours, filtered at normal pressure, vacuum dried until completely dry, ball-milled, and passed through a 100 to 200 mesh sieve to obtain a porous graphitized carbon material.
[0051] Example 3, Preparation Method of Porous Graphitized Carbon Material III
[0052] S1. The porous pine sawdust is crushed by a crusher and passed through a 40-60 mesh sieve to obtain granules;
[0053] S2. The particles are placed in deionized water and stirred for washing for 6 to 12 hours, filtered under normal pressure, and vacuum dried until completely dry to obtain a biomass precursor;
[0054] S3. The biomass precursor is placed in a graphite crucible and placed in a graphitization furnace, carbonized at 1600°C for 1 h, then heated to 3000°C at a heating rate of 1-5°C / min, and graphitized at 3000°C for 3 h to obtain a black residue;
[0055] S4. The obtained black residue is placed in deionized water and stirred for washing for 6 to 12 hours, filtered at normal pressure, vacuum dried until completely dry, ball-milled, and passed through a 100 to 200 mesh sieve to obtain a porous graphitized carbon material.
[0056] In Examples 1-3, Example 2 is the best example. The porous graphitized carbon material prepared in Example 2 was subjected to Raman spectroscopy test, pore size distribution test and electron microscope scanning, and compared with commercial graphite. The results are as follows: Figure 1-3 shown.
[0057] from Figure 1 As can be seen from the results, since Raman mainly indicates the degree of graphitization of the material, I G / I D The larger the graphite, the higher the degree of graphitization of the material. Compared with commercial graphite, the material I prepared in this application G / I D The values are comparable, indicating that the material prepared in the present application has a good degree of graphitization, which is close to that of commercial graphite.
[0058] from Figure 2-3 From the results, it can be seen that commercial graphite is a tightly stacked graphite layer, while the porous graphitized carbon prepared in the present application is a graphite layer surrounding mesopores / macropores, that is, the material prepared in the present application has significantly more mesopores and macropores than commercial graphite. The meso-macroporous structure is conducive to the rapid transmission of lithium ions during the charge and discharge process, thereby improving the rate performance.
[0059] Example 4, performance test
[0060] The prepared porous graphitized carbon material made of pine sawdust and commercial graphite were used to test the electrochemical properties of lithium-ion battery negative electrode materials under the same experimental conditions, and the electrochemical properties of the material were tested using CR2032 button batteries.
[0061] S10. The porous graphitized carbon material of pine sawdust, conductive carbon black (Super P Li) and polyvinylidene fluoride (PVDF) were mixed in N-methylpyrrolidone (NMP) at a mass ratio of 8:1:1, and stirred for 6 to 12 hours to form a slurry;
[0062] S20. The slurry is coated on a copper foil with a coating thickness of 100 to 150 μm, and then vacuum dried in a vacuum oven at 90° C. for 12 hours to prepare a negative electrode material.
[0063] Lithium metal was used as the counter electrode and reference electrode, and the electrolyte was 1M LiPF6 dissolved in a mixed solution of ethylene carbonate (EC), dimethyl carbonate (DMC) and diethyl carbonate (DEC) (EC:DMC:DEC=1:1:1). CR2032 button cells were assembled in a glove box filled with Ar, and the battery was left to stand for 12 hours before the charge and discharge cycle and rate performance tests were performed on a CT4008 battery tester, with a test voltage range of 0.01 to 3V.
[0064] The test results are as follows Figure 4 As shown, according to Figure 4As we know, at 0.1Ag -1 At the current density, the first discharge capacity of pine sawdust graphitized carbon is 323.06 mAh g -1 , first coulombic efficiency 72.23%, capacity after 100 cycles 337.18 mAh g -1 ; The first discharge capacity of commercial graphite is 376.02 mAh g -1 , first coulombic efficiency 70.71%, capacity after 100 cycles 317.67mAh g -1 , the recycling performance of pine sawdust graphitized carbon is slightly higher than that of commercial graphite.
[0065] Compared with the commercial graphite, the graphitized carbon from pine sawdust has a great improvement in rate performance. -1 ,0.5Ag -1 ,1Ag -1 ,2Ag -1 The current density increased by 119 mAh g -1 ,93mAh g -1 ,53mAg g -1 ,25mAg g -1 .
[0066] Judging from the results of cycle and rate performance tests, pine sawdust graphitized carbon has the potential to replace commercial graphite as a low-cost fast-charging lithium-ion battery negative electrode material.
[0067] The above is a detailed introduction to a method for preparing a porous graphitized carbon material and its application provided by the present invention. The description of the specific embodiment is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
[0068] It should be noted that if no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be purchased commercially.
[0069] The above examples are intended to provide a better understanding of the present invention, and are not intended to be limiting of the best implementation mode described herein, nor are they intended to limit the content and protection scope of the present invention. Any product identical or similar to the present invention that is derived by anyone under the inspiration of the present invention or by combining the present invention with features of other prior arts shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a porous graphitized carbon material, characterized in that: The following steps are involved: S1. crushing the waste biomass raw material and passing it through a 40-60 mesh sieve to obtain granules; S2. The particles are placed in deionized water and stirred for washing for 6 to 12 hours, filtered, and dried until completely dry to obtain a biomass precursor; S3. The biomass precursor is placed in a graphite crucible and placed in a high temperature furnace, carbonized at 1200 to 1600°C, and then heated to 2600 to 3200°C for graphitization to obtain a black residue; S4. The obtained black residue is placed in deionized water and stirred for washing for 6 to 12 hours, filtered, dried until completely dry, ball-milled, and passed through a 100 to 200 mesh sieve to obtain a porous graphitized carbon material.
2. The preparation method according to claim 1, characterized in that: The waste biomass raw materials include one or more combinations of pine sawdust, corn stalks, rice stalks, pine bark, birch bark, ginkgo leaves, corn leaves, coconut shells, walnut shells, rice husks, corn cobs, and cotton.
3. The preparation method according to claim 1, characterized in that: In the step S1, during the pulverization, one or more combinations of a crusher, a ball mill, and a pulverizer are used.
4. The preparation method according to claim 1, characterized in that: In the steps S2 and S4, during filtration, one or more combinations of normal pressure filtration, reduced pressure filtration, vacuum filtration, centrifugal filtration, and membrane filtration are used.
5. The preparation method according to claim 1, characterized in that: In the steps S2 and S4, during drying, one or more combinations of forced air drying, vacuum drying, spray drying, reduced pressure drying, far infrared radiation drying, heating drying, and natural drying are used.
6. The preparation method according to claim 1, characterized in that: In the step S3, during carbonization, the carbonization time is 1 to 3 hours.
7. The preparation method according to claim 1, characterized in that: In the step S3, the temperature is increased at a heating rate of 1 to 5°C / min.
8. The preparation method according to claim 1, characterized in that: In the step S3, during graphitization, the graphitization time is 1 to 3 hours.
9. An application of a graphitized carbon material prepared by the method for preparing a porous graphitized carbon material according to any one of claims 1 to 8, characterized in that: Used as negative electrode material for lithium-ion batteries.
10. The use according to claim 9, characterized in that: When preparing the negative electrode material of the lithium ion battery, the following steps are included: S10. The graphitized carbon material, the conductive carbon black and the polyvinylidene fluoride are mixed in N-methylpyrrolidone and stirred for 6 to 12 hours to form a slurry; S20. The slurry is coated on a copper foil and dried in a vacuum oven at 90° C. to prepare a negative electrode material.
Citation Information
Cited By
Biomass-derived graphitized porous activated carbon negative electrode for lithium ion battery and preparation method of biomass-derived graphitized porous activated carbon negative electrode