Synthesis method of three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material
By constructing a three-dimensional macroporous zinc oxide single crystal hexagonal rod structure, the problems of small specific surface area and poor adsorption performance of ZnO photocatalysts are solved, the photocatalytic reaction efficiency is significantly improved, and the efficient degradation of antibiotics is achieved. It has a wide range of market prospects and application potential.
Patent Information
- Application Number
- CN202411032123.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing ZnO photocatalysts have small specific surface area and poor adsorption performance, resulting in low degradation efficiency of antibiotics in wastewater.
By constructing a three-dimensional macroporous zinc oxide single-crystal hexagonal rod structure, using polystyrene microspheres as templates, the specific surface area of the material and carrier migration efficiency are significantly improved through hydrothermal reaction and heat treatment methods, and the photocatalytic reaction is enhanced. activity.
The photocatalytic reaction efficiency of ZnO is significantly improved, and the excellent photocatalytic degradation performance shows obvious advantages for antibiotics such as norfloxacin and ciprofloxacin, and has better stability and is suitable for the expansion of other functional semiconductor materials.
Smart Images

Figure CN118877925A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of inorganic nano photocatalysts, and in particular relates to a method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material. Background Art
[0002] With the increasing use of disinfectants and antibiotics in the medical and health field, their content in sewage has far exceeded the previous level, and the corresponding ecological and environmental pollution problems have become more serious. Norfloxacin (NFX) is a widely used antibiotic that cannot be completely metabolized in organisms. As a typical endocrine disruptor, NFX has potential negative effects on the aquatic environment. Ciprofloxacin (CIP), as a commonly used antibiotic, is also widely present in pharmaceutical wastewater generated by factories and domestic sewage in cities. Therefore, how to effectively degrade this type of wastewater containing norfloxacin and ciprofloxacin before it is discharged into the environment has attracted more and more attention and research. Photocatalytic technology can photocatalytically degrade organic pollutants in sewage. It is a green, environmentally friendly, low-cost, fast and effective method. In recent years, people have been studying photocatalysts more and more deeply.
[0003] As a common photocatalyst, ZnO has many advantages such as strong oxidation and excellent electron carrying capacity, but its specific surface area is small and its adsorption performance is poor. We found that constructing a three-dimensional single crystal macroporous structure can effectively improve these problems. The three-dimensional single crystal macroporous structure increases the specific surface area of the photocatalytic material and the utilization rate of carriers, and can effectively improve the photocatalytic reaction efficiency of ZnO; based on this, the present invention is specially proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material; the process of the present invention solves the problems of small specific surface area and poor adsorption performance of ordinary ZnO materials, and significantly improves the specific surface area of the photocatalytic material by constructing a three-dimensional macroporous structure, thereby improving the photocatalytic reaction efficiency of ZnO. The present invention selects polystyrene (PS) microspheres as a template to construct a three-dimensional macroporous zinc oxide single crystal photocatalytic material, and the prepared zinc oxide material has a three-dimensional macroporous single crystal hexagonal rod structure, which significantly improves the specific surface area of the catalyst, increases the active sites of the reaction, shortens the migration distance of the carriers, and reduces the recombination rate of the carriers, thereby improving the photocatalytic degradation performance of zinc oxide. In the application of photocatalytic degradation of antibiotics such as norfloxacin and ciprofloxacin, this method shows obvious advantages.
[0005] In order to achieve the above object, the present invention specifically adopts the following technical solutions: A method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material comprises the following steps: S1, using polyvinyl pyrrolidone and styrene as raw materials, adding an initiator for polymerization, and obtaining an orderly arranged polystyrene microsphere template; S2, adding a soluble zinc salt into methanol to dissolve to obtain a precursor solution, adding a polystyrene microsphere template into the precursor solution, vacuum degassing, washing and drying to obtain a sample A; S3, placing the obtained sample A into a mixture of ammonia water and methanol, vacuum degassing, hydrothermal reaction at 353-393 K for 10-14 h, washing and drying to obtain sample B; S4. Add sample B into N,N-dimethylformamide to remove the polystyrene microsphere template, centrifuge, wash and dry to obtain sample C, and heat-treat sample C to obtain a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material.
[0006] Furthermore, the polystyrene microsphere template described in S1 is obtained by reacting polyvinyl pyrrolidone, deionized water, styrene and potassium persulfate at 75° C. for 24 hours and filtering.
[0007] Furthermore, the soluble zinc salt in S2 is any one of Zn(NO3)2·6H2O, ZnCl2 and Zn(CH3COO)2·2H2O.
[0008] Furthermore, the dosage ratio of the soluble zinc salt and the polystyrene microsphere template in S2 is (0.01-0.02):(6-8), mol:g.
[0009] Furthermore, the vacuum degassing in S2 has a pressure of 5-8 kPa and a time of 3-5 min.
[0010] Further, the ammonia water in S3 and the Zn in sample A 2+ The molar ratio is 1:(1-4), preferably 1:(2-4).
[0011] Furthermore, the vacuum degassing pressure in S3 is 6-10 kPa, and the time is 3-5 min; the hydrothermal reaction temperature is 373 K, and the time is 12 h.
[0012] Furthermore, the heat treatment in S4 is maintained at 723-823 K for 1-3 h, and the heating rate is 1-3°C / min.
[0013] The present invention uses PS microspheres as templates to construct three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic materials. First, a precursor solution formed by dissolving a soluble zinc salt in methanol is filled into the gaps of an ordered PS template to obtain a sample containing the precursor in the gaps of the ordered microsphere template. Then, the residual Zn on the surface of the PS template is fully washed with methanol. 2+ Then, the ammonia water mixed solution is filled and impregnated again, and the Zn2+ The molar ratio of Zn(OH)2 to ammonia water allows it to fully react in the gap to form Zn(OH)2 hexagonal rods, which are then subjected to a hydrothermal reaction. After washing and drying with anhydrous methanol, the PS template is removed by an organic solvent DMF, followed by centrifugal washing and drying. The resulting sample is further heat treated to convert Zn(OH)2 into ZnO and remove organic impurities, finally obtaining a three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material. The three-dimensional macroporous structure significantly increases the specific surface area, increases the active sites of the reaction, reduces the obstacles during carrier migration, and reduces the carrier recombination rate, thereby improving the photocatalytic performance of ZnO. This general synthetic strategy can extend the possibility of three-dimensional macroporous growth to other functional semiconductor materials.
[0014] The advantages and beneficial effects of the present invention are: 1. The present invention innovatively proposes a two-step impregnation method to prepare a three-dimensional macroporous single crystal structure ZnO grown in a PS template, which increases the specific surface area, increases the active sites of the reaction, and reduces the recombination rate of carriers, showing excellent photocatalytic ability. Compared with ordinary macroporous ZnO, it has better stability, is not easy to be destroyed, and is conducive to the photocatalytic reaction.
[0015] 2. Compared with ordinary rod-shaped ZnO, the three-dimensional macroporous ZnO single crystal hexagonal rod constructed by the present invention has a macroporous structure that can obtain a higher porosity, thereby improving the utilization rate of light and further facilitating the photocatalytic reaction.
[0016] 3. The symmetrical orientation and structural continuity of the single crystal network in the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material constructed by the present invention make the migration of carriers more efficient.
[0017] 4. The raw materials of the present invention are easily available, the preparation cost is low, the operation is simple, and the product performance is excellent. It is of great significance to improve the performance of zinc oxide and save product costs. Therefore, it has broad market prospects and is conducive to the promotion and application and the progress and development of industry technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the XRD pattern of three-dimensional macroporous ZnO single crystal hexagonal rod (3DMRZnO).
[0019] Figure 2 (a) is the SEM image of three-dimensional macroporous ZnO single crystal hexagonal rod (3DMR ZnO), and (b) is the SEM image of ordinary macroporous ZnO.
[0020] Figure 3 This is the photocatalytic degradation curve of norfloxacin (30 mg / L NFX) by three-dimensional macroporous ZnO single crystal hexagonal rods (3DMR ZnO) under full light.
[0021] Figure 4 This is the photocatalytic degradation curve of ciprofloxacin (20 mg / L CIP) by three-dimensional macroporous ZnO single crystal hexagonal rods (3DMR ZnO) under full light. DETAILED DESCRIPTION
[0022] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0023] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0024] Example 1 A method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material, comprising: 1. First, add 500 mL of deionized water and 2.5 g of polyvinylpyrrolidone (PVP) into a 1 L three-necked round-bottom flask, add 65 mL of styrene after removing the inhibitor, then heat the solution to 75°C, add K2S2O8 (1g K2S2O8 / 50mLH2O) aqueous solution for 24 hours to initiate polymerization. The obtained milky white dispersion was ultrasonically treated for 30 minutes. Then it was poured into a filter funnel equipped with an organic filter membrane with a pore size of 0.2 μm, and the negative pressure was controlled at 0.05 Mpa. After filtering for 3 days, a solid filter cake was obtained, and the PS template was obtained after drying at 50°C overnight.
[0025] 2. Take Zn(NO3)2·6H2O (0.01 mol) and add it to 20 mL of anhydrous methanol, stir and dissolve to obtain a precursor solution. Then put a piece of PS template (7 g) into the precursor solution, let it stand at room temperature for 1 h, vacuum degas for 5 min (pressure is 8 kPa), wash it three times with 21 mL of anhydrous methanol, and dry it at 323 K for 6 h to obtain sample A containing Zn(NO3)2 in the template.
[0026] 3. Take 0.68 mL of ammonia water (25%), add 9.32 mL of deionized water, and then mix with 10 mL of anhydrous methanol. Add sample A to the above ammonia water mixed solution, vacuum degas for 5 min (pressure is 6 kPa), transfer to a hydrothermal reactor at 373 K and react for 12 h. Wash twice with 14 mL of anhydrous methanol and dry in an oven at 323 K for 6 h to obtain sample B.
[0027] 4. Sample B was added to DMF and stirred for 8 h to remove the PS template (the ratio of DMF to PS template was 20 mL / g). The mixture was centrifuged and washed several times with 25 mL DMF and 25 mL anhydrous methanol respectively, and then dried in an oven at 353 K to obtain sample C.
[0028] 5. Place sample C in a muffle furnace, heat it to 773 K at 2 °C / min, maintain it for 2 h, cool it to room temperature, and collect the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material.
[0029] Example 2 A method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material, comprising: 1. First, add 500 mL of deionized water and 2.5 g of polyvinylpyrrolidone (PVP) into a 1 L three-necked round-bottom flask, add 65 mL of styrene after removing the inhibitor, then heat the solution to 75°C, add K2S2O8 (1g K2S2O8 / 50mLH2O) aqueous solution for 24 hours to initiate polymerization. The obtained milky white dispersion was ultrasonically treated for 30 minutes. Then it was poured into a filter funnel equipped with an organic filter membrane with a pore size of 0.2 μm, and the negative pressure was controlled at 0.05 Mpa. After filtering for 3 days, a solid filter cake was obtained, and the PS template was obtained after drying at 50°C overnight.
[0030] 2. Take Zn(NO3)2·6H2O (0.02 mol) and add it to 20 mL of anhydrous methanol, stir and dissolve to obtain a precursor solution. Then put a piece of PS template (7 g) into the precursor solution, let it stand at room temperature for 1 h, vacuum degas for 5 min (pressure is 8 kPa), wash it three times with 21 mL of anhydrous methanol, and dry it at 323 K for 6 h to obtain sample A containing Zn(NO3)2 in the template.
[0031] 3. Take 0.68 mL of ammonia water (25%), add 9.32 mL of deionized water, and then mix with 10 mL of anhydrous methanol. Add sample A to the above ammonia water mixed solution, vacuum degas for 5 min (pressure is 6 kPa), transfer to a hydrothermal reactor at 373 K and react for 12 h. Wash twice with 14 mL of anhydrous methanol and dry in an oven at 323 K for 6 h to obtain sample B.
[0032] 4. Sample B was added to DMF and stirred for 8 h to remove the PS template (the ratio of DMF to PS template was 20 mL / g). The mixture was centrifuged and washed several times with 25 mL DMF and 25 mL anhydrous methanol respectively, and then dried in an oven at 353 K to obtain sample C.
[0033] 5. Place sample C in a muffle furnace, heat it to 773 K at 2 °C / min, maintain it for 2 h, cool it to room temperature, and collect the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material.
[0034] Example 3 A method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material, comprising: 1. First, add 500 mL of deionized water and 2.5 g of polyvinylpyrrolidone (PVP) into a 1 L three-necked round-bottom flask, add 65 mL of styrene after removing the inhibitor, then heat the solution to 75°C, add K2S2O8 (1g K2S2O8 / 50mLH2O) aqueous solution for 24 hours to initiate polymerization. The obtained milky white dispersion was ultrasonically treated for 30 minutes. Then it was poured into a filter funnel equipped with an organic filter membrane with a pore size of 0.2 μm, and the negative pressure was controlled at 0.05 Mpa. After filtering for 3 days, a solid filter cake was obtained, and the PS template was obtained after drying at 50°C overnight.
[0035] 2. Take ZnCl2 (0.02 mol) and add it to 20 mL of anhydrous methanol, stir and dissolve to obtain a precursor solution. Then put a piece of PS template (7 g) into the precursor solution, let it stand at room temperature for 1 h, vacuum degas for 5 min (pressure is 8 kPa), wash it three times with 21 mL of anhydrous methanol, and dry it at 323 K for 6 h to obtain sample A containing ZnCl2 in the template.
[0036] 3. Take 0.68 mL of ammonia water (25%), add 9.32 mL of deionized water, and then mix with 10 mL of anhydrous methanol. Add sample A to the above ammonia water mixed solution, vacuum degas for 5 min (pressure is 6 kPa), transfer to a hydrothermal reactor at 373 K and react for 12 h. Wash twice with 14 mL of anhydrous methanol and dry in an oven at 323 K for 6 h to obtain sample B.
[0037] 4. Sample B was added to DMF and stirred for 8 h to remove the PS template (the ratio of DMF to PS template was 20 mL / g). The mixture was centrifuged and washed several times with 25 mL DMF and 25 mL anhydrous methanol respectively, and then dried in an oven at 353 K to obtain sample C.
[0038] 5. Place sample C in a muffle furnace, heat it to 773 K at 2 °C / min, maintain it for 2 h, cool it to room temperature, and collect the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material.
[0039] Example 4 A method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material, comprising: 1. First, add 500 mL of deionized water and 2.5 g of polyvinylpyrrolidone (PVP) into a 1 L three-necked round-bottom flask, add 65 mL of styrene after removing the inhibitor, then heat the solution to 75°C, add K2S2O8 (1g K2S2O8 / 50mLH2O) aqueous solution for 24 hours to initiate polymerization. The obtained milky white dispersion was ultrasonically treated for 30 minutes. Then it was poured into a filter funnel equipped with an organic filter membrane with a pore size of 0.2 μm, and the negative pressure was controlled at 0.05 Mpa. After filtering for 3 days, a solid filter cake was obtained, and the PS template was obtained after drying at 50°C overnight.
[0040] 2. Take Zn(CH3COO)2·2H2O (0.02 mol) and add it to 20 mL of anhydrous methanol, stir and dissolve to obtain a precursor solution. Then put a piece of PS template (7 g) into the precursor solution, let it stand at room temperature for 1 h, vacuum degas for 5 min (pressure is 8 kPa), wash it three times with 21 mL of anhydrous methanol, and dry it at 323 K for 6 h to obtain sample A containing ZnCl2 in the template.
[0041] 3. Take 0.68 mL of ammonia water (25%), add 9.32 mL of deionized water, and then mix with 10 mL of anhydrous methanol. Add sample A to the above ammonia water mixed solution, vacuum degas for 5 min (pressure is 6 kPa), transfer to a hydrothermal reactor at 373 K and react for 12 h. Wash twice with 14 mL of anhydrous methanol and dry in an oven at 323 K for 6 h to obtain sample B.
[0042] 4. Sample B was added to DMF and stirred for 8 h to remove the PS template (the ratio of DMF to PS template was 20 mL / g). The mixture was centrifuged and washed several times with 25 mL DMF and 25 mL anhydrous methanol respectively, and then dried in an oven at 353 K to obtain sample C.
[0043] 5. Place sample C in a muffle furnace, heat it to 773 K at 2 °C / min, maintain it for 2 h, cool it to room temperature, and collect the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material.
[0044] The samples prepared in the above examples have the following morphology, structure and properties: Figure 1-Figure 4 shown.
[0045] Depend on Figure 1 It can be seen that the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic materials prepared by filling the gaps between PS spheres with precursors of different concentrations of Zn(NO3)2·6H2O are all pure phase ZnO.
[0046] Depend on Figure 2 It can be seen that three-dimensional macropores were successfully constructed, and the three-dimensional macroporous ZnO single crystal hexagonal rods maintained high porosity and integrity.
[0047] Depend on Figure 3 , Figure 4 It can be seen that the three-dimensional macroporous ZnO single crystal hexagonal rods exhibited excellent photocatalytic degradation activity during the photocatalytic degradation of norfloxacin (30 mg / L NFX) and ciprofloxacin (20 mg / L CIP) solutions.
[0048] The results of the examples show that the three-dimensional macroporous ZnO single crystal hexagonal rod photocatalytic material prepared by the present invention has excellent photocatalytic degradation performance.
[0049] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material, characterized in that: The steps include: S1, using polyvinyl pyrrolidone and styrene as raw materials, adding an initiator for polymerization, and obtaining an orderly arranged polystyrene microsphere template; S2, adding a soluble zinc salt into methanol to dissolve to obtain a precursor solution, adding a polystyrene microsphere template into the precursor solution, vacuum degassing, washing and drying to obtain a sample A; S3, placing the obtained sample A into a mixture of ammonia water and methanol, vacuum degassing, hydrothermal reaction at 353-393 K for 10-14 h, washing and drying to obtain sample B; S4. Add sample B into N,N-dimethylformamide to remove the polystyrene microsphere template, centrifuge, wash and dry to obtain sample C, and heat-treat sample C to obtain a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material.
2. According to the method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, it is characterized in that: The polystyrene microsphere template described in S1 is obtained by reacting polyvinyl pyrrolidone, deionized water, styrene and potassium persulfate at 75° C. for 24 hours and filtering.
3. The method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, characterized in that: S2 The soluble zinc salt is any one of Zn(NO3)2·6H2O, ZnCl2 and Zn(CH3COO)2·2H2O.
4. The method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, characterized in that: The dosage ratio of the soluble zinc salt and the polystyrene microsphere template described in S2 is (0.01-0.02):(6-8), mol:g.
5. The method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, characterized in that: The vacuum degassing pressure in S2 is 5-8 kPa and the time is 3-5 min.
6. The method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, characterized in that: S3 The ammonia water and Zn in sample A 2+ The molar ratio is 1:(1-4).
7. The method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, characterized in that: The vacuum degassing pressure in S3 is 6-10 kPa, and the time is 3-5 min; the hydrothermal reaction temperature is 373 K, and the time is 12 h.
8. The method for synthesizing a three-dimensional macroporous zinc oxide single crystal hexagonal rod photocatalytic material according to claim 1, characterized in that: The heat treatment in S4 is maintained at 723-823 K for 1-3 h, and the heating rate is 1-3°C / min.
Citation Information
Patent Citations
Preparation method of self-assembled hexagonal prim-shaped zinc oxide
CN109399692A
Synthesis method of two-dimensional single crystal period macroporous zinc oxide photocatalytic material
CN118062874A
Cited By
High-performance silicon-carbon negative electrode porous carbon material and preparation method thereof
CN121651365A
High-performance silicon-carbon negative electrode porous carbon material and preparation method thereof
CN121651365B