Treatment method and application of thallium-containing nickel sulfate solution
By using a specific thallium remover to perform the chelation reaction when treating the nickel thallium sulfate solution, the problems of secondary pollution and high nickel loss in the prior art are solved, and the significant reduction in the thallium content and effective protection of nickel resources are achieved.
Patent Information
- Application Number
- CN202410948247.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is prone to the problems of secondary pollution and high nickel loss when treating nickel thallium-containing nickel sulfate solutions, resulting in environmental pollution and waste of resources.
Use xylene dithiophosphoric acid, O-isopropyl N-ethoxycarbonyl thiocarbamate or sulfosuccinamic acid tetrasodium salt as thallium removal agent, and use chelation reaction within a specific temperature and pH range. The treatment was carried out to generate a stable chelating precipitate, reducing thallium content and reducing nickel loss.
The thallium content of the thallium nickel sulfate solution is effectively reduced to 45μg/L, reducing nickel loss, avoiding secondary pollution, and improving resource utilization.
Smart Images

Figure CN118877959A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of treatment of thallium-containing nickel sulfate solution, and particularly relates to a treatment method and application of the thallium-containing nickel sulfate solution. Background Art
[0002] As a highly toxic heavy metal element, thallium is more toxic than lead and mercury and is comparable to arsenic. It is often found in nickel ores. Due to its strong mobility, thallium is easily released into the environment with the mining and use of nickel ores, causing heavy metal pollution and posing a serious risk of environmental pollution.
[0003] However, in the field of ternary battery materials, battery-grade refined nickel sulfate is the main source of nickel. Based on the environmental threat posed by thallium associated with nickel ore, in order to reduce or avoid environmental pollution risks, it is required that the thallium content in battery-grade refined nickel sulfate used in downstream users be less than 45μg / L.
[0004] At present, sodium sulfide is often used in common technology to reduce the thallium content of refined nickel sulfate. Sodium sulfide solid is added to the thallium-containing nickel sulfate solution at a dosage of 3.5 kg per cubic meter of nickel sulfate solution, and the mixture is stirred for reaction for 60 minutes and then filtered to obtain a thallium-free liquid. However, this method is prone to produce hydrogen sulfide gas, causing secondary pollution to the environment. At the same time, the nickel loss in this process is as high as more than 1%, resulting in unnecessary resource consumption. Summary of the invention
[0005] In order to solve the technical problems of secondary pollution and nickel loss in the nickel sulfate treatment process in the above-mentioned common technology, the present invention provides a method for treating a thallium-containing nickel sulfate solution, comprising the steps of:
[0006] adding a thallium removing agent to the thallium-containing nickel sulfate solution to carry out a chelating reaction;
[0007] The temperature of the thallium-containing nickel sulfate solution is 20° C. to 80° C., the pH is 3.0 to 8.0, the thallium content in the thallium-containing nickel sulfate solution is 1 mg / L to 50 mg / L, and the thallium removal agent includes one or more of dimethylphenol dithiophosphoric acid, O-isopropyl N-ethoxycarbonylthiocarbamate or tetrasodium sulfosuccinamate;
[0008] After the reaction is completed, the solid and liquid are separated to obtain a thallium-removed liquid, wherein the thallium content of the thallium-removed liquid is less than 45 μg / L.
[0009] Furthermore, the thallium-containing nickel sulfate solution includes a prefabricated nickel sulfate solution, which is a nickel sulfate solution after extraction and impurity removal, and the temperature of the prefabricated nickel sulfate solution is 40° C. to 60° C. and the pH is 3.0 to 6.0.
[0010] Furthermore, the temperature of the prefabricated nickel sulfate solution is 40° C. to 60° C., and the pH value is 3.0 to 6.0.
[0011] Furthermore, the composition of the prefabricated nickel sulfate solution includes Ni 90g / L~120g / L, Tl≤50mg / L, Co≤230mg / L, Ca≤30mg / L, Mg≤30mg / L, Mn≤5mg / L, Pb≤5mg / L, Cu≤3mg / L, Zn≤3mg / L, and Cr≤3mg / L.
[0012] Furthermore, after the reaction is completed, the solid-liquid separation to obtain a thallium-free liquid also includes: after the reaction is completed, the solid-liquid separation to obtain a thallium slag, and the thallium content of the thallium slag is 5% to 15%.
[0013] Furthermore, the amount of the thallium removal agent added is 0.02kg to 1.25kg per cubic meter of the thallium-containing nickel sulfate solution.
[0014] Furthermore, the amount of the thallium removal agent added satisfies the stoichiometric ratio of the chelating reaction, and the stoichiometric ratio of the chelating reaction includes the following formula:
[0015] M=C Tl ×V×R1×10 -3 (kg)
[0016] Among them, C Tl is the thallium content (mg / L or g / m 3 );
[0017] V is the volume of the nickel sulfate solution containing thallium (m 3 );
[0018] R1 is the reaction coefficient, 20≤R1≤25.
[0019] Furthermore, the chelating reaction is carried out at a rotation speed of 60 r / min to 85 r / min for 30 to 60 min.
[0020] Furthermore, the thallium-removed liquid includes components Ni 90g / L-120g / L, Tl≤45μg / L, Co≤230mg / L, Ca≤30mg / L, Mg≤30mg / L, Mn≤5mg / L, Pb≤5mg / L, Cu≤3mg / L, Zn≤3mg / L, and Cr≤3mg / L.
[0021] The present invention also provides an application of any of the above treatment methods in the preparation of refined nickel sulfate.
[0022] Compared with the prior art, the present invention has at least the following advantages:
[0023] The invention provides a treatment method for a thallium-containing nickel sulfate solution, which specifically purifies and removes thallium from the thallium-containing nickel sulfate solution with a temperature of 20°C to 80°C and a pH of 3.0 to 8.0, thereby significantly reducing the thallium content of the thallium-containing nickel sulfate solution from 1 mg / L to 50 mg / L to 45 μg / L.
[0024] The present invention uses dimethylphenol dithiophosphoric acid, O-isopropyl N-ethoxycarbonyl thiocarbamate or sulfosuccinamic acid tetrasodium salt as a thallium removal agent, which has the following advantages:
[0025] 1. The thallium remover has a wide applicable temperature range (20℃~80℃) and does not require consumption of additional heat energy.
[0026] 2. The thallium remover is applicable to a wide pH range (3.0-8.0), and there is no need to adjust the pH, which simplifies the steps and reduces acid and alkali consumption.
[0027] 3. The thallium remover has strong selectivity and can react with thallium ions in nickel sulfate solution to form stable chelate precipitates. At the same time, the high selectivity of the thallium remover can also improve the hit rate of heavy metal chelation and reduce unnecessary metal loss in the liquid after thallium removal. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0029] Figure 1 The figure is a schematic diagram of the process of treating a thallium-containing nickel sulfate solution in one embodiment of the present invention. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0032] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.
[0033] The present invention provides a method for treating a thallium-containing nickel sulfate solution, comprising the steps of:
[0034] S1. adding a thallium removing agent to the thallium-containing nickel sulfate solution to carry out a chelating reaction.
[0035] In some embodiments, the thallium removing agent includes one or more of xylenol dithiophosphoric acid, O-isopropyl N-ethoxycarbonylthiocarbamate, or sulfosuccinamic acid tetrasodium salt.
[0036] Exemplarily, the thallium removing agent may be one or more of xylenol dithiophosphoric acid, O-isopropyl N-ethoxycarbonylthiocarbamate, or tetrasodium sulfosuccinamate.
[0037] The thallium remover used in the present invention has strong selectivity and can form a stable chelate precipitate with thallium ions in nickel sulfate. The thallium remover first reacts with a large amount of nickel ions in the nickel sulfate solution to form a chelate nickel precipitate. The anions released by the chelate nickel precipitate are gradually converted into a more stable chelate thallium precipitate after contacting the thallium ions.
[0038] The thallium remover used in the present invention also has the advantage of a wide range of applications. The performance and structure of the thallium remover are stable under the conditions of a temperature of 20°C to 80°C and a pH of 3.0 to 8.0. It can be applied in a temperature range of 20°C to 80°C and a pH range of 3.0 to 8.0 without consuming additional heat energy or additionally adjusting the pH, thereby saving processes and effectively avoiding secondary pollution.
[0039] Based on this, the thallium-containing nickel sulfate solution may include a prefabricated nickel sulfate solution, the temperature of which is 40° C. to 60° C. and the pH value is 3.0 to 6.0. Exemplarily, the temperature of the prefabricated nickel sulfate solution may be 40° C. to 50° C. and the pH value may be 4.0 to 5.0.
[0040] The prefabricated nickel sulfate solution can be a nickel sulfate solution after extraction and impurity removal, that is, a nickel sulfate solution that has been extracted to remove copper, manganese and zinc by P204, extracted to remove cobalt, calcium and magnesium by C272, and a plurality of extractants and a multi-stage extraction process to remove most of the metal impurities.
[0041] In some embodiments, the amount of the thallium removal agent added may be 0.02 kg to 1.25 kg per cubic meter of the prefabricated nickel sulfate solution.
[0042] Exemplarily, the amount of thallium removal agent added may be 1.20 kg per cubic meter of the prefabricated nickel sulfate solution.
[0043] In other embodiments, the amount of the thallium removal agent added can satisfy the stoichiometric ratio of the chelating reaction, and the stoichiometric ratio of the chelating reaction includes the following formula:
[0044] M=C Tl ×V×R1×10 -3 (kg)
[0045] Among them, C Tl is the thallium content (mg / L or g / m 3 );
[0046] V is the volume of the prefabricated nickel sulfate solution (m 3 );
[0047] R1 is the reaction coefficient, 20≤R1≤25.
[0048] The calculation method (M = C Tl ×V×R1×10 -3 (kg)) The amount of thallium remover added can be adaptively adjusted according to its type, which can accurately hit the appropriate amount of thallium remover added, further optimizing the treatment effect of thallium-containing nickel sulfate solution.
[0049] Exemplarily, the size of R1 may satisfy 20≤R1≤25.
[0050] When the thallium removal agent is used to remove thallium from the prefabricated nickel sulfate solution, nickel chelation can be avoided in a targeted manner, thereby reducing nickel loss in the prefabricated nickel sulfate. Exemplarily, the nickel loss caused by thallium precipitation in the present invention is only 0.1% to 0.2% of the total nickel amount.
[0051] At the same time, when the thallium remover is used in the prefabricated nickel sulfate solution, only 0.02kg to 1.25kg of thallium remover is used per cubic meter of nickel sulfate solution, and only 60g to 800g of thallium slag is produced per cubic meter of nickel sulfate solution. Among them, even the addition of a very small amount of thallium remover can achieve deep recovery of thallium. For example, the thallium content in the nickel sulfate solution can be reduced from 1mg / L to 50mg / L to below 45μg / L.
[0052] Although the process of removing thallium is accompanied by the generation of thallium slag, the thallium slag in the present invention is small in quantity and high in quality. The high-grade thallium slag with a thallium content of 5.0% to 15.0% can be directly used to produce metallic thallium. This also means that the present invention effectively solves the technical problems of the difficulty in recycling thallium-containing solid waste and the secondary pollution of the thallium precipitation process in the commonly used technology, and has significant economic and environmental benefits.
[0053] In comparison, the commonly used technology often uses sodium sulfide to prepare low-thallium refined nickel sulfate. In the thallium-containing nickel sulfate solution, sodium sulfide solid is added at an amount of 3.5 kg per cubic meter of nickel sulfate solution, and the mixture is stirred for 60 minutes and then filtered to obtain a thallium-free liquid. In this process, the amount of sodium sulfide added is more than 3 times the amount of the thallium removal agent in the present invention, which is also accompanied by the generation of a large amount of hydrogen sulfide. Under acidic conditions, the sulfur ions generated by the dissolution of sodium sulfide combine with hydrogen ions to generate hydrogen sulfide gas. 2- +2H + →H2S↑, which is easy to cause environmental burden and form secondary pollution. At the same time, the accuracy and efficiency of the sodium sulfide chelating effect are far inferior to the thallium removal agent in the present invention, and usually causes about 1% nickel loss.
[0054] The chelating reaction can be carried out at a rotation speed of 60 r / min to 85 r / min for 30 to 60 min. Under the rotation speed conditions, the mass transfer efficiency between the components can be significantly improved, thereby promoting the progress of the chelating reaction.
[0055] S2. After the reaction is completed, the solid and liquid are separated to obtain a thallium-free liquid, wherein the thallium content in the thallium-free liquid is less than 45 μg / L.
[0056] In some embodiments, a plate-frame filter press can be used for filtration to achieve solid-liquid separation to obtain thallium-free liquid and thallium slag. The working pressure per unit area of the plate-frame filter press is (0.10Mpa-0.30Mpa), for example, it can be (0.10, 0.15, 0.20, 0.25 or 0.30)Mpa, and the pore size of the filter cloth of the filter press is (2.0μm-5.0μm), for example, it can be (2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0)μm.
[0057] The thallium content in the liquid after thallium removal is less than 45 μg / L, which meets the content requirement of refined nickel sulfate.
[0058] In some embodiments, the thallium-removed solution of the prefabricated nickel sulfate solution also includes components Ni 90g / L~120g / L, Tl≤45μg / L, Co≤230mg / L, Ca≤30mg / L, Mg≤30mg / L, Mn≤5mg / L, Pb≤5mg / L, Cu≤3mg / L, Zn≤3mg / L, and Cr≤3mg / L.
[0059] It can be seen that by limiting the type and content of thallium removal agents, the metal impurity thallium can be selectively chelated, while taking into account the loss suppression of metallic nickel, and directly producing refined nickel sulfate that meets the quality requirements of high-end materials such as ternary batteries.
[0060] The present invention also provides an application of any of the above treatment methods in the preparation of refined nickel sulfate.
[0061] In order to facilitate those skilled in the art to further understand the present invention, examples are given below:
[0062] Example 1
[0063] Nickel sulfate solution after extraction and impurity removal (prefabricated nickel sulfate solution, i.e. nickel sulfate solution containing thallium, the same below), volume: 30.0m 3 . Its components include: nickel: 100.2g / L, thallium: 35.0mg / L.
[0064] A method for treating a thallium-containing nickel sulfate solution comprises the following steps:
[0065] (1) Detection: Detect the temperature of the prefabricated nickel sulfate solution: 42.3°C, pH: 4.6, and thallium: 35.0 mg / L. If the temperature and pH of the prefabricated nickel sulfate solution are within the applicable range of the thallium remover, the thallium remover can be directly added. The thallium remover is a mixture of dimethylbenzene dithiophosphoric acid and tetrasodium sulfosuccinamate in a mass ratio of 4:1.
[0066] (2) Calculation: Calculate the amount of thallium removal agent according to the formula = C Tl ×V×R1×10 -3 (kg) = 35.0 × 30.0 × 25 × 10 -3 (kg)=26.3kg.
[0067] (3) Thallium removal: at 30.0m 3 26.3 kg of thallium removal agent was added to the prefabricated nickel sulfate solution, stirred at a speed of 75 r / min, and reacted for 45 minutes.
[0068] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25Mpa, and the pore size of the filter cloth was 2.0μm. The thallium-free liquid and thallium residue were obtained by filtration. The thallium content of the thallium-free liquid was 10.6μg / L, which met the requirements.
[0069] According to the detection and calculation, 1m 3 A prefabricated nickel sulfate solution with a nickel content of 100.2 g / L and a thallium content of 35.0 mg / L requires 0.88 kg of thallium removal agent, produces 597.4 g of thallium slag, has a nickel loss of 0.15%, and contains 5.86% thallium in the thallium slag.
[0070] Example 2
[0071] Nickel sulfate solution after extraction and impurity removal (prefabricated nickel sulfate solution), volume: 20.0m 3 ; Nickel: 108.7g / L, Thallium: 47.3mg / L.
[0072] A method for purifying and removing thallium from a nickel sulfate solution (prefabricated nickel sulfate solution) after extraction and impurity removal, comprising the following steps:
[0073] (1) Detection: Detect the temperature of the prefabricated nickel sulfate solution: 50.7°C, pH: 5.0, and thallium: 47.3 mg / L. If the temperature and pH of the prefabricated nickel sulfate solution are within the applicable range of the thallium remover, the thallium remover can be directly added. The thallium remover is a mixture of dimethylbenzene dithiophosphoric acid and tetrasodium sulfosuccinamate in a mass ratio of 4:1.
[0074] (2) Calculation: Calculate the amount of thallium removal agent according to the formula = C Tl ×V×R1×10 -3 (kg) = 47.3 × 20.0 × 25 × 10 -3 (kg)=23.7kg.
[0075] (3) Thallium removal: at 20.0m 3 23.7 kg of thallium removal agent was added to the prefabricated nickel sulfate solution, stirred at a speed of 80 r / min, and reacted for 60 minutes.
[0076] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25Mpa, and the pore size of the filter cloth was 2.0μm. The thallium-free liquid and thallium residue were obtained by filtration. The thallium content of the thallium-free liquid was 20.5μg / L, which met the requirements.
[0077] According to the detection and calculation, 1m 3 A prefabricated nickel sulfate solution with a nickel content of 108.7 g / L and a thallium content of 47.3 mg / L requires 1.19 kg of thallium removal agent, produces 372.4 g of thallium slag, has a nickel loss of 0.14%, and the thallium slag contains 12.70% thallium.
[0078] Example 3
[0079] Nickel sulfate solution after extraction and impurity removal (prefabricated nickel sulfate solution), volume: 30.0m 3 ; Nickel: 106.5g / L, Thallium: 5.3mg / L.
[0080] A method for purifying and removing thallium from a nickel sulfate solution (prefabricated nickel sulfate solution) after extraction and impurity removal, comprising the following steps:
[0081] (1) Detection: Detect the temperature of the prefabricated nickel sulfate solution: 46.2°C, pH: 4.7, and thallium: 5.3 mg / L. If the temperature and pH of the prefabricated nickel sulfate solution are within the applicable range of the thallium remover, the thallium remover can be directly added. The thallium remover is a mixture of dimethylbenzene dithiophosphoric acid and tetrasodium sulfosuccinamate in a mass ratio of 4:1.
[0082] (2) Calculation: Calculate the amount of thallium removal agent according to the formula = C Tl ×V×R1×10 -3 (kg) = 5.3 × 30.0 × 25 × 10 -3 (kg)=4.0kg.
[0083] (3) Thallium removal: at 30.0m 3 4.0 kg of thallium removal agent was added to the prefabricated nickel sulfate solution, stirred at a speed of 78 r / min, and reacted for 60 min.
[0084] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.20Mpa and the pore size of the filter cloth was 2.0μm. The thallium-free liquid and thallium residue were obtained by filtration. The thallium content of the thallium-free liquid was 37.2μg / L, which met the requirements.
[0085] According to the detection and calculation, 1m 3 A prefabricated nickel sulfate solution with a nickel content of 106.5 g / L and a thallium content of 5.3 mg / L requires 0.13 kg of thallium removal agent, produces 89.6 g of thallium slag, has a nickel loss of 0.06%, and contains 5.92% thallium in the thallium slag.
[0086] Example 4
[0087] Nickel sulfate solution after extraction and impurity removal (prefabricated nickel sulfate solution), volume: 30.0m 3 ; Nickel: 104.7g / L, Thallium: 21.7mg / L.
[0088] A method for purifying and removing thallium from a nickel sulfate solution (prefabricated nickel sulfate solution) after extraction and impurity removal, comprising the following steps:
[0089] (1) Detection: Detect the temperature of the prefabricated nickel sulfate solution: 46.3°C, pH: 4.4, and thallium: 21.7 mg / L. If the temperature and pH of the prefabricated nickel sulfate solution are within the applicable range of the thallium remover, the thallium remover can be directly added. The thallium remover is a mixture of dimethylbenzene dithiophosphoric acid and tetrasodium sulfosuccinamate in a mass ratio of 4:1.
[0090] (2) Calculation: Calculate the amount of thallium removal agent according to the formula = C Tl ×V×R1×10 -3 (kg) = 21.7 × 30.0 × 25 × 10 -3 (kg)=16.3kg.
[0091] (3) Thallium removal: at 30.0m 3 16.3 kg of thallium removal agent was added to the prefabricated nickel sulfate solution, stirred at a speed of 82 r / min, and reacted for 60 min.
[0092] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25Mpa, and the pore size of the filter cloth was 2.0μm. The thallium-free liquid and thallium residue were obtained by filtration. The thallium content of the thallium-free liquid was 14.9μg / L, which met the requirements.
[0093] According to the detection and calculation, 1m 3 A prefabricated nickel sulfate solution with a nickel content of 104.7 g / L and a thallium content of 21.7 mg / L requires 0.54 kg of thallium removal agent, produces 296.1 g of thallium slag, has a nickel loss of 0.19%, and contains 7.33% thallium in the thallium slag.
[0094] Comparative Example 1
[0095] Nickel sulfate solution after extraction and impurity removal (prefabricated nickel sulfate solution), volume: 30.0m 3 ; Nickel: 101.5g / L, Thallium: 34.2mg / L.
[0096] Compared with the embodiment, the other steps of this comparative example 1 remain unchanged, only the thallium removal agent is replaced with sodium sulfide for use in prefabricated nickel sulfate to remove thallium, and at the same time, the amount of sodium sulfide added is adjusted accordingly, including the steps of:
[0097] (1) Detection: Detect the temperature of the prefabricated nickel sulfate solution: 43.5°C, pH: 4.4, and thallium: 34.2 mg / L. If the temperature and pH of the prefabricated nickel sulfate solution are within the applicable range of sodium sulfide, sodium sulfide can be directly added.
[0098] (2) Calculation: Calculate the amount of sodium sulfide according to the formula = C Tl ×V×R2×10 -3 (kg) = 34.2 × 30.0 × 75 × 10 -3 (kg)=77.0kg.
[0099] (3) Thallium removal: at 30.0m 3 77.0 kg of sodium sulfide was added to the prefabricated nickel sulfate solution, stirred at a speed of 75 r / min, and reacted for 45 minutes.
[0100] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25Mpa, and the pore size of the filter cloth was 2.0μm. The thallium-free liquid and thallium residue were obtained by filtration. The thallium content of the thallium-free liquid was 37.4μg / L, which met the requirements.
[0101] According to the detection and calculation, 1m 3The prefabricated nickel sulfate solution with a nickel content of 101.5 g / L and a thallium content of 34.2 mg / L requires 2.57 kg of sodium sulfide, produces 3334.6 g of thallium slag, has a nickel loss of 1.14%, and the thallium slag contains 1.03% thallium.
[0102] Comparative Example 2
[0103] Nickel sulfate solution after extraction and impurity removal (prefabricated nickel sulfate solution), volume: 20.0m 3 ; Nickel: 107.3g / L, Thallium: 46.9mg / L.
[0104] The other steps of this comparative example remain unchanged, only the thallium removal agent is replaced with sodium sulfide for use in prefabricated nickel sulfate to remove thallium, and at the same time, the amount of sodium sulfide added is adjusted accordingly, including the steps of:
[0105] (1) Detection: The temperature of the prefabricated nickel sulfate solution is 52.1°C, the pH is 4.8, and the thallium is 46.9 mg / L. If the temperature and pH of the prefabricated nickel sulfate solution are within the applicable range of sodium sulfide, sodium sulfide can be directly added.
[0106] (2) Calculation: Calculate the amount of sodium sulfide according to the formula = C Tl ×V×R1×10 -3 (kg) = 46.9 × 20.0 × 75 × 10 -3 (kg)=70.4kg.
[0107] (3) Thallium removal: at 20.0m 3 70.4 kg of sodium sulfide was added to the prefabricated nickel sulfate solution, stirred at a speed of 80 r / min, and reacted for 60 min.
[0108] (4) Filtration: The working pressure per unit area of the plate and frame filter press was set to 0.25Mpa, and the pore size of the filter cloth was 2.0μm. The thallium-free liquid and thallium residue were obtained by filtration. The thallium content of the thallium-free liquid was 28.1μg / L, which met the requirements.
[0109] According to the detection and calculation, 1m 3 The prefabricated nickel sulfate solution with a nickel content of 107.3 g / L and a thallium content of 46.9 mg / L requires 3.52 kg of sodium sulfide, produces 3696.9 g of thallium slag, has a nickel loss of 1.23%, and contains 1.27% thallium in the thallium slag.
[0110] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.
Claims
1. A method for treating a thallium-containing nickel sulfate solution, characterized in that: Includes steps: adding a thallium removing agent to the thallium-containing nickel sulfate solution to carry out a chelating reaction; The temperature of the thallium-containing nickel sulfate solution is 20° C. to 80° C., the pH is 3.0 to 8.0, the thallium content in the thallium-containing nickel sulfate solution is 1 mg / L to 50 mg / L, and the thallium removal agent includes one or more of dimethylphenol dithiophosphoric acid, O-isopropyl N-ethoxycarbonylthiocarbamate or tetrasodium sulfosuccinamate; After the reaction is completed, the solid and liquid are separated to obtain a thallium-removed liquid, wherein the thallium content of the thallium-removed liquid is less than 45 μg / L.
2. The processing method according to claim 1, characterized in that: The thallium-containing nickel sulfate solution comprises a prefabricated nickel sulfate solution, wherein the prefabricated nickel sulfate solution is a nickel sulfate solution after extraction and impurity removal, and the temperature of the prefabricated nickel sulfate solution is 40° C. to 60° C. and the pH value is 3.0 to 6.
0.
3. The processing method according to claim 1, characterized in that: The temperature of the prefabricated nickel sulfate solution is 40° C. to 60° C., and the pH value is 3.0 to 6.
0.
4. The processing method according to claim 2, characterized in that: The composition of the prefabricated nickel sulfate solution includes Ni90g / L-120g / L, Tl≤50mg / L, Co≤230mg / L, Ca≤30mg / L, Mg≤30mg / L, Mn≤5mg / L, Pb≤5mg / L, Cu≤3mg / L, Zn≤3mg / L, and Cr≤3mg / L.
5. The processing method according to claim 1, characterized in that: After the reaction is completed, the solid-liquid separation to obtain the thallium-removed liquid also includes: after the reaction is completed, the solid-liquid separation to obtain thallium slag, the thallium content of the thallium slag is 5% to 15%.
6. The processing method according to claim 4, characterized in that: The amount of the thallium removal agent added is 0.02kg to 1.25kg per cubic meter of the thallium-containing nickel sulfate solution.
7. The processing method according to claim 4, characterized in that: The amount of the thallium removal agent added satisfies the stoichiometric ratio of the chelating reaction, and the stoichiometric ratio of the chelating reaction includes the following formula: M=C Tl ×V×R1×10 -3 (kg) Among them, C Tl is the thallium content (mg / L or g / m 3 ); V is the volume of the nickel sulfate solution containing thallium (m 3 ); R1 is the reaction coefficient, 20≤R1≤25.
8. The processing method according to claim 1, characterized in that: The chelating reaction is carried out at a rotation speed of 60 r / min to 85 r / min for 30 to 60 min.
9. The processing method according to claim 4, characterized in that: The thallium-removed liquid includes components of Ni 90g / L-120g / L, Tl≤45μg / L, Co≤230mg / L, Ca≤30mg / L, Mg≤30mg / L, Mn≤5mg / L, Pb≤5mg / L, Cu≤3mg / L, Zn≤3mg / L, and Cr≤3mg / L.
10. Use of the treatment method according to any one of claims 1 to 9 in the preparation of refined nickel sulfate.