Solar evaporation device

By using carbon aerogel-covered polyethylene foam in solar evaporation devices, using its micron-scale three-dimensional fibrous network structure and efficient photothermal conversion capabilities, the poor stability and salt deposition problems in high-concentration saline in traditional technology are solved, and the problem of poor stability and salt deposition in high-concentration saline is achieved. Efficient and stable evaporation effect.

CN118877993AActive Publication Date: 2024-11-01TIANJIN UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411164038.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-01
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

Traditional solar evaporation technology has poor stability when operating in high concentration brine, and salt deposition of the photothermal absorption layer will reduce evaporation efficiency and damage the device structure.

Method used

Carbon aerogel covering the surface of polyethylene foam is used to avoid salt deposition through the micron-scale three-dimensional fibrous network structure of the carbon aerogel and the efficient photothermal conversion capability. The buoyancy is greater than gravity in the early stage of evaporation through the special design of the device. The salt is dissolved during evaporation, keeping the light-heat absorption layer clean.

Benefits of technology

It realizes efficient evaporation in high-concentrated brine, maintains long-term and stable operation, avoids the impact of salt deposition on evaporation efficiency, and ensures the continuous and efficient operation of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877993A_ABST
    Figure CN118877993A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solar evaporation, in particular to a solar evaporation device. The invention provides a solar evaporation device. The solar evaporation device comprises polyethylene foam and carbon aerogel coating the surface of the polyethylene foam, the polyethylene foam is a cylinder or a sphere. The solar evaporation device effectively solves the problem of salt deposition of the photo-thermal absorption layer, and meanwhile has high evaporation efficiency and excellent operation stability in strong brine.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar energy evaporation, and in particular to a solar energy evaporation device. Background Art

[0002] The development of solar evaporation technology has solved the two problems of limited fossil energy reserves and shortage of fresh water resources. The core of this technology is to convert solar energy into thermal energy to drive water evaporation. In traditional solar evaporation technology, the photothermal absorption layer is located at the bottom of the water body, and the heat is dispersed throughout the water body, reducing the evaporation efficiency. With the introduction of the concept of solar interfacial evaporation, its high efficiency and zero energy consumption have attracted widespread attention. This technology avoids the loss of heat to the water body by concentrating heat on the surface of the evaporating water, and has a high evaporation efficiency. However, to maintain the long-term stable and efficient operation of the solar evaporation device, the premise is that the photothermal absorption layer of the solar interfacial evaporation device will not deposit salt. The formation of salt deposition will affect the light absorption of the photothermal absorption layer, reduce the evaporation efficiency of the device, and even further damage the structure of the evaporation device. Most of the existing devices only focus on the design of evaporation devices that operate for a short time in fresh water or in salt water with low concentrations. The stability of the device in high-concentration salt water is poor. Summary of the invention

[0003] The object of the present invention is to provide a solar evaporation device, which effectively solves the problem of salt deposition in a photothermal absorption layer and has high evaporation efficiency and excellent operating stability in concentrated brine.

[0004] The present invention provides a solar evaporation device, comprising polyethylene foam and carbon aerogel coated on the surface of the polyethylene foam;

[0005] The polyethylene foam is in the shape of a cylinder or a sphere.

[0006] Preferably, the thickness of the carbon aerogel coated on the surface of the polyethylene foam is 1 to 3 mm.

[0007] Preferably, the pore structure of the carbon aerogel is a micrometer-scale three-dimensional fibrous network structure.

[0008] Preferably, the method for preparing the carbon aerogel comprises the following steps:

[0009] Degrading corrugated paper in a non-neutral solution and drying it to obtain wood cellulose;

[0010] After the lignocellulose and the solvent are mixed, the obtained mixed solution is sequentially frozen, freeze-dried and carbonized to obtain the carbon aerogel.

[0011] Preferably, the non-neutral solution is an acid solution or an alkali solution;

[0012] The acid solution includes one or more of phosphoric acid, hydrochloric acid and sulfuric acid;

[0013] The alkali solution includes potassium hydroxide solution and / or sodium hydroxide solution.

[0014] Preferably, the mass percentage concentration of the acid solution is 0.5-10%;

[0015] The mass percentage concentration of the alkali solution is 1-15%.

[0016] Preferably, the solvent comprises water or polyvinyl alcohol aqueous solution;

[0017] The mass percentage concentration of polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 0.05-5%.

[0018] Preferably, the mass percentage concentration of the lignocellulosic fibers in the mixed solution is 1-5%.

[0019] Preferably, the freezing temperature is -10 to -50°C and the freezing time is 10 to 24 hours;

[0020] The freeze-drying time is 24 to 48 hours.

[0021] Preferably, the carbonization temperature is 800° C., the holding time is 4 to 8 hours, and the heating rate is 5 to 10° C. / min.

[0022] The present invention provides a solar evaporation device, comprising polyethylene foam (PE) and carbon aerogel coated on the surface of the polyethylene foam; the polyethylene foam is a cylinder or a sphere. The polyethylene foam described in the present invention has a relatively small density so that the buoyancy is greater than the gravity, and the entire evaporation device can float on the water surface. The incident sunlight is absorbed by the photothermal absorption layer (carbon aerogel) and converted into thermal energy. The lower thermal conductivity of PE can prevent heat from being transferred downward to the water body. Under the action of capillary force, seawater is transported to the top of the photothermal absorption layer, and then the seawater is heated and evaporated into water vapor, while impurities such as salt ions in the water are retained in the photothermal absorption layer. As the salt ions accumulate, the light absorption of the photothermal absorption layer will be affected; by limiting the shape of the solar evaporation device, the buoyancy it is subjected to in the initial stage of evaporation is greater than the gravity (such as Figure 1 As evaporation proceeds, the salt accumulated on the surface of the evaporator gradually increases, and the gravity of the evaporator gradually approaches the buoyancy (as shown in Fig. Figure 1 As shown in ii), the device will gradually tilt under the action of gravity. As the evaporation process continues, the gravity of the evaporation device is greater than the buoyancy, the evaporation device tilts, and the salt accumulated on the top of the light and heat absorption layer of the evaporation device is dissolved by seawater (as shown in Figure 1At this time, the new light and heat absorption layer of the evaporation device will be exposed to the sun again to continue the evaporation process, realizing the long-term stable operation of the anti-salting evaporation device in seawater (such as Figure 1 shown). BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the working principle of the solar evaporation device of the present invention;

[0024] Figure 2 is a SEM image of the carbon aerogel described in Example 1;

[0025] Figure 3 The water contact angle test of the carbon aerogel described in Example 1;

[0026] Figure 4 is a curve showing the effect of wavelength on the light absorption rate of the carbon aerogel described in Example 1;

[0027] Figure 5 This is the evaporation performance of the solar evaporation device described in Example 1. DETAILED DESCRIPTION

[0028] The present invention provides a solar evaporation device, comprising polyethylene foam and carbon aerogel coated on the surface of the polyethylene foam;

[0029] The polyethylene foam is in the shape of a cylinder or a sphere.

[0030] In the present invention, the thickness of the carbon aerogel coated on the surface of the polyethylene foam is preferably 1 to 3 mm, more preferably 1.5 to 2.5 mm, and most preferably 1.8 to 2.2 mm.

[0031] In the present invention, the pore structure of the carbon aerogel is preferably a micrometer-level three-dimensional fibrous network structure. In the present invention, the micrometer-level three-dimensional fibrous network structure strengthens the transport of water and the transmission of water vapor; the carbon aerogel has a strong absorption capacity for water, ensuring sufficient water source during the evaporation process; and the weighted average absorption rate of the carbon aerogel in the solar band is about 98%, with excellent light-to-heat conversion capacity.

[0032] In the present invention, the method for preparing the carbon aerogel preferably comprises the following steps:

[0033] Degrading corrugated paper in a non-neutral solution and drying it to obtain wood cellulose;

[0034] After the lignocellulose and the solvent are mixed, the obtained mixed solution is sequentially frozen, freeze-dried and carbonized to obtain the carbon aerogel.

[0035] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0036] The invention degrades the corrugated paper in a non-neutral solution and dries it to obtain wood cellulose.

[0037] Before the degradation, the present invention preferably pre-treats the corrugated paper, and the pre-treatment preferably includes crushing, soaking and washing in sequence. In the present invention, the corrugated paper is preferably waste corrugated paper. In the present invention, the soaking is preferably carried out in deionized water; the washing is preferably carried out under ultrasonic conditions; the present invention does not have any special restrictions on the crushing, soaking and ultrasonic processes, and can be carried out using processes well known to those skilled in the art.

[0038] In the present invention, the non-neutral solution is preferably an acid solution or an alkali solution; the acid solution preferably includes one or more of phosphoric acid, hydrochloric acid and sulfuric acid. When the acid solution is two or more of the above specific selections, the present invention has no special restrictions on the ratio of the above specific substances, and they can be mixed in any ratio; the alkali solution preferably includes potassium hydroxide solution and / or sodium hydroxide solution. When the alkali solution is potassium hydroxide solution and sodium hydroxide solution, the present invention has no special restrictions on the ratio of the potassium hydroxide solution and the sodium hydroxide solution, and they can be mixed in any ratio. In the present invention, the mass percentage concentration of the acid solution is preferably 0.5-10%, more preferably 2-8%, and most preferably 4-6%; the mass percentage concentration of the alkali solution is preferably 1-15%, more preferably 3-12%, and most preferably 5-9%.

[0039] In the present invention, the degradation is preferably carried out under stirring conditions, the stirring temperature is preferably 20-40°C; the rotation speed is preferably 200-400rpm, more preferably 250-350rpm; the time is preferably 5-10h, more preferably 6-8h.

[0040] After the degradation is completed, the present invention also preferably includes cleaning, and the cleaning is preferably performed with deionized water. The present invention does not have any special limitation on the cleaning process, and the cleaning process may be performed using a process well known to those skilled in the art.

[0041] In the present invention, the drying temperature is preferably 50-70°C, more preferably 50-60°C, most preferably 60°C; the drying time is preferably 1-3h, more preferably 2-3h, most preferably 2h. In the present invention, the drying is preferably carried out in a blast drying oven.

[0042] After obtaining the lignocellulose, the present invention mixes the lignocellulose with a solvent, and then sequentially freezes, freeze-dries and carbonizes the obtained mixed solution to obtain the carbon aerogel.

[0043] In the present invention, the solvent preferably includes water or polyvinyl alcohol aqueous solution; the mass percentage concentration of polyvinyl alcohol in the polyvinyl alcohol aqueous solution is preferably 0.05-5%, more preferably 1-4%, and most preferably 2-3%. In the present invention, the preparation of the polyvinyl alcohol aqueous solution preferably includes adding polyvinyl alcohol to deionized water for dissolution; the dissolution temperature is preferably 80-90°C, more preferably 85-90°C, and most preferably 90°C; the dissolution time is preferably 1-3h, more preferably 2-3h, and most preferably 2h. In the present invention, the dissolution is preferably carried out in a rotating water bath.

[0044] The present invention does not have any special limitation on the mixing process, and the mixing process may be carried out using a process well known to those skilled in the art.

[0045] In the present invention, the mass percentage concentration of the lignocellulosic fibers in the mixed solution is preferably 1 to 5%, more preferably 1 to 4%, and most preferably 2 to 3%.

[0046] In the present invention, the freezing temperature is preferably -10 to -50°C, more preferably -20 to -30°C, and most preferably -25 to -30°C; the time is preferably 10 to 24 hours, more preferably 12 to 15 hours, and most preferably 15 hours; the freeze-drying time is preferably 24 to 48 hours, more preferably 30 to 36 hours, and most preferably 36 hours.

[0047] In the present invention, the carbonization temperature is preferably 700-900°C, more preferably 700-800°C, and most preferably 800°C; the holding time is preferably 4-8h, more preferably 5-6h, and most preferably 6h; the heating rate is preferably 5-10°C / min, more preferably 5-7°C / min, and most preferably 5°C / min.

[0048] In the present invention, the preparation method of the solar evaporation device preferably comprises the following steps:

[0049] The carbon aerogel is coated on the surface of the polyethylene foam to obtain the solar evaporation device.

[0050] The present invention does not have any special limitation on the coating process, and the coating process may be carried out using a process well known to those skilled in the art.

[0051] The solar evaporation device provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0052] Example 1

[0053] Crush the discarded corrugated paper (the size after crushing is 1×1cm 2) and then immersed in deionized water and ultrasonically cleaned, stirred in a phosphoric acid solution with a mass concentration of 5wt% (rotation speed of 200rpm) for 8h to complete the degradation of lignocellulose, washed with deionized water, and dried in a 60°C forced air drying oven for 2h to obtain lignocellulose;

[0054] Add 0.6 g of polyvinyl alcohol to 19.4 g of deionized water, and dissolve in a rotating water bath at 90° C. to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 3 wt %;

[0055] 0.7 g of lignocellulose and 20 g of the polyvinyl alcohol aqueous solution were mixed, and then sequentially frozen (temperature was -30°C, time was 15 h) and freeze-dried (time was 36 h), and then placed in a tubular furnace and heated to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept warm for 6 h to obtain a carbon aerogel;

[0056] The carbon aerogel is coated on the surface of polyethylene foam (with a radius of 1.5 cm and a height of 4 cm) to obtain the solar evaporation device (the thickness of the carbon aerogel layer is 1 mm);

[0057] The carbon aerogel was subjected to SEM test, and the test results are as follows Figure 2 As shown by Figure 2 It can be seen that the carbon aerogel microstructure has an obvious fibrous network, which is crucial for water transport during interfacial evaporation. These fibers are interwoven to form a three-dimensional network, providing a large number of micron-sized pores, which are conducive to the transport of water and water vapor. On the other hand, the three-dimensional pore structure provides more surface area for light absorption for evaporation, which helps to improve evaporation performance;

[0058] The carbon aerogel was tested for water contact angle using a water contact angle tester. The test results are as follows: Figure 3 As shown by Figure 3 It can be seen that water droplets can be completely absorbed by carbon aerogel in a very short time (~0.05s), which shows that carbon aerogel has a strong water transport capacity and can ensure sufficient water source during the evaporation process;

[0059] The effect of wavelength on the absorptivity of the carbon aerogel was tested using an ultraviolet-visible-near infrared spectrophotometer (UV-VIS-NIR). Figure 4 As shown by Figure 4 It can be seen that carbon aerogel has a strong absorption capacity for light in the solar band (weighted average absorption rate ~98%);

[0060] The solar evaporation device was tested for evaporation performance. The test process was to use a solar simulator (AM 1.5) to provide input solar energy, and use a computer and an electronic balance (accuracy 0.0001g, counting frequency 2s) to record mass data in real time to monitor the mass change of simulated seawater. Before the experiment, the irradiance of the simulator was calibrated using a solar power meter to ensure that the radiation intensity irradiated to the surface of the carbon aerogel was 1kWm -2 To ensure the accuracy of the experiment, the temperature and humidity of the laboratory were stabilized at 24℃ and around 65%, respectively.

[0061] Test results such as Figure 5 As shown by Figure 5 It can be seen that the measured evaporation rate of the solar evaporation device under standard solar irradiation is 1.43 kg·m -2 ·h -1 The evaporation efficiency is 97.3%. In a sodium chloride solution with a mass concentration of 15wt%, the solar evaporation device can operate continuously for more than 6 hours and no salt deposition occurs in the photothermal absorption layer (carbon aerogel).

[0062] Example 2

[0063] Crush the discarded corrugated paper (the size after crushing is 1×1cm 2 ) and then immersed in deionized water and ultrasonically cleaned, stirred in a phosphoric acid solution with a mass concentration of 0.5% (rotation speed of 200 rpm) for 8 hours to complete the degradation of lignocellulose, washed with deionized water, and dried in a 60° C. forced air drying oven for 2 hours to obtain lignocellulose;

[0064] Add 0.6 g of polyvinyl alcohol to 19.4 g of deionized water and dissolve in a rotating water bath at 90° C. to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 3%;

[0065] 0.7 g of lignocellulose and 20 g of the polyvinyl alcohol aqueous solution were mixed, and then sequentially frozen (temperature was -30°C, time was 15 h) and freeze-dried (time was 36 h), and then placed in a tubular furnace and heated to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept warm for 6 h to obtain a carbon aerogel;

[0066] The carbon aerogel is coated on the surface of polyethylene foam (with a radius of 1.5 cm and a height of 4 cm) to obtain the solar evaporation device (the thickness of the carbon aerogel layer is 1 mm);

[0067] The solar evaporation device was tested for evaporation performance. The test process was to use a solar simulator (AM 1.5) to provide input solar energy, and use a computer and an electronic balance (accuracy 0.0001g, counting frequency 2s) to record mass data in real time to monitor the mass change of simulated seawater. Before the experiment, the irradiance of the simulator was calibrated using a solar power meter to ensure that the radiation intensity irradiated to the surface of the carbon aerogel was 1kWm -2 To ensure the accuracy of the experiment, the temperature and humidity of the laboratory were stabilized at 24°C and 65% respectively. The measured evaporation rate of the solar evaporation device under standard solar irradiation was 1.12 kg·m -2 ·h -1 The evaporation rate is 76.2%. In a sodium chloride solution with a mass concentration of 15 wt%, the solar evaporation device can operate continuously for more than 6 hours and no salt deposition occurs in the photothermal absorption layer (carbon aerogel).

[0068] Example 3

[0069] Crush the discarded corrugated paper (the size after crushing is 1×1cm 2 ) and then immersed in deionized water and ultrasonically cleaned, stirred in a phosphoric acid solution with a mass concentration of 5% (rotation speed of 200 rpm) for 8 hours to complete the degradation of lignocellulose, washed with deionized water, and dried in a 60° C. forced air drying oven for 2 hours to obtain lignocellulose;

[0070] Add 0.6 g of polyvinyl alcohol to 19.4 g of deionized water and dissolve in a rotating water bath at 90° C. to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 3%;

[0071] 0.7 g of lignocellulose and 20 g of the polyvinyl alcohol aqueous solution were mixed, and then sequentially frozen (temperature was -30°C, time was 15 h) and freeze-dried (time was 36 h), and then placed in a tubular furnace and heated to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept warm for 6 h to obtain a carbon aerogel;

[0072] The carbon aerogel is coated on the surface of polyethylene foam (with a radius of 1.5 cm and a height of 4 cm) to obtain the solar evaporation device (the thickness of the carbon aerogel layer is 3 mm);

[0073] The solar evaporation device was tested for evaporation performance. The test process was to use a solar simulator (AM 1.5) to provide input solar energy, and use a computer and an electronic balance (accuracy 0.0001g, counting frequency 2s) to record mass data in real time to monitor the mass change of simulated seawater. Before the experiment, the irradiance of the simulator was calibrated using a solar power meter to ensure that the radiation intensity irradiated to the surface of the carbon aerogel was 1kWm -2To ensure the accuracy of the experiment, the temperature and humidity of the laboratory were stabilized at 24°C and 65% respectively. The measured evaporation rate of the solar evaporation device under standard solar irradiation was 0.72 kg·m -2 ·h -1 The evaporation rate is 48.9%. In a sodium chloride solution with a mass concentration of 15 wt%, the solar evaporation device can operate continuously for more than 6 hours and no salt deposition occurs in the photothermal absorption layer (carbon aerogel).

[0074] Example 4

[0075] Crush the discarded corrugated paper (the size after crushing is 1×1cm 2 ) and then immersed in deionized water and ultrasonically cleaned, stirred in a phosphoric acid solution with a mass concentration of 0.5% (rotation speed of 200 rpm) for 8 hours to complete the degradation of lignocellulose, washed with deionized water, and dried in a 60° C. forced air drying oven for 2 hours to obtain lignocellulose;

[0076] Add 0.01 g of polyvinyl alcohol to 19.99 g of deionized water and dissolve in a rotating water bath at 90°C to obtain a polyvinyl alcohol aqueous solution with a mass concentration of 0.05%;

[0077] 0.7 g of lignocellulose and 20 g of the polyvinyl alcohol aqueous solution were mixed, and then sequentially frozen (temperature was -30°C, time was 15 h) and freeze-dried (time was 36 h), and then placed in a tubular furnace and heated to 800°C at a heating rate of 5°C / min in a nitrogen atmosphere and kept warm for 6 h to obtain a carbon aerogel;

[0078] The carbon aerogel is coated on the surface of polyethylene foam (with a radius of 1.5 cm and a height of 4 cm) to obtain the solar evaporation device (the thickness of the carbon aerogel layer is 1 mm);

[0079] The solar evaporation device was tested for evaporation performance. The test process was to use a solar simulator (AM 1.5) to provide input solar energy, and use a computer and an electronic balance (accuracy 0.0001g, counting frequency 2s) to record mass data in real time to monitor the mass change of simulated seawater. Before the experiment, the irradiance of the simulator was calibrated using a solar power meter to ensure that the radiation intensity irradiated to the surface of the carbon aerogel was 1kWm -2 To ensure the accuracy of the experiment, the temperature and humidity in the laboratory were kept stable at 24°C and 65% respectively. The measured evaporation rate of the solar evaporation device under standard sunlight was 0.98 kg·m -2 ·h -1The evaporation rate is 66.7%. In a sodium chloride solution with a mass concentration of 15 wt%, the solar evaporation device can operate continuously for more than 6 hours and no salt deposition occurs in the photothermal absorption layer (carbon aerogel).

[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A solar evaporation device, characterized in that: It comprises polyethylene foam and carbon aerogel coated on the surface of the polyethylene foam; The polyethylene foam is in the shape of a cylinder or a sphere.

2. The solar evaporation device according to claim 1, characterized in that: The thickness of the carbon aerogel coated on the surface of the polyethylene foam is 1 to 3 mm.

3. The solar evaporation device according to claim 1 or 2, characterized in that: The pore structure of the carbon aerogel is a micrometer-level three-dimensional fibrous network structure.

4. The solar evaporation device according to claim 3, characterized in that: The preparation method of the carbon aerogel comprises the following steps: Degrading corrugated paper in a non-neutral solution and drying it to obtain wood cellulose; After the lignocellulose and the solvent are mixed, the obtained mixed solution is sequentially frozen, freeze-dried and carbonized to obtain the carbon aerogel.

5. The solar evaporation device according to claim 4, characterized in that: The non-neutral solution is an acid solution or an alkali solution; The acid solution includes one or more of phosphoric acid, hydrochloric acid and sulfuric acid; The alkali solution includes potassium hydroxide solution and / or sodium hydroxide solution.

6. The solar evaporation device according to claim 5, characterized in that: The mass percentage concentration of the acid solution is 0.5-10%; The mass percentage concentration of the alkali solution is 1-15%.

7. The solar evaporation device according to claim 4, characterized in that: The solvent includes water or polyvinyl alcohol aqueous solution; The mass percentage concentration of polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 0.05-5%.

8. The solar evaporation device according to claim 4 or 7, characterized in that: The mass percentage concentration of the wood cellulose fibers in the mixed solution is 1-5%.

9. The solar evaporation device according to claim 4, characterized in that: The freezing temperature is -10 to -50°C and the freezing time is 10 to 24 hours; The freeze-drying time is 24 to 48 hours.

10. The solar evaporation device according to claim 4, characterized in that: The carbonization temperature is 700-900° C., the heat preservation time is 4-8 hours, and the heating rate is 5-10° C. / min.

Citation Information

Patent Citations

  • Self-cleaning light absorption medium for photo-thermal seawater desalination and preparation method thereof

    CN111392794A

  • Modified lignin-based biomass gel and preparation method thereof

    CN114920979A

  • Floating ball for continuously evaporating solar seawater through photothermal conversion and application

    CN115403092A

  • Carbon aerogel for interface evaporation and heat absorption from environment and preparation method thereof

    CN115716967A

  • Biomass-based novel solar water evaporator and preparation method and application thereof