Method for preparing silicon carbide ceramic-based composite material through continuous polycarbosilane dipping, pyrolysis and sintering
Through the continuous polycarbosilane impregnation and sintering method, the processing flow of the fiber preform is optimized, the problems of long process cycles and high costs in the existing technology are solved, and the preparation of high-efficiency and low-energy consumption of silicon carbide ceramic composite materials is realized. Improves the density and performance of the material.
Patent Information
- Application Number
- CN202411139531.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-01
AI Technical Summary
The existing polycarbosilane impregnation pyrolysis methods have long cycles, high costs and residual stress problems, which affect the performance of the material.
Using continuous polycarbosilane impregnation pyrolysis sintering method, through specific equipment and step processes, including multiple cycles of impregnation, pyrolysis and sintering processes, optimize the processing of fiber preforms, reduce the production cycle and energy consumption of materials, and improve the production cycle of materials and improve the The density and strength of the material.
It significantly improves the production efficiency of the product, shortens the process cycle, reduces raw material waste and energy consumption, improves the strength and fracture strain performance of ceramic matrix composite materials, and reduces costs.
Smart Images

Figure CN118878342A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a silicon carbide ceramic-based composite material, in particular to a method for preparing a silicon carbide ceramic-based composite material by continuous polycarbosilane impregnation, pyrolysis and sintering. Background Art
[0002] The polycarbosilane impregnation and pyrolysis (PIP) method is a technology used to prepare silicon carbide ceramic-based composites. It usually involves the impregnation of a polymer (such as polycarbosilane) and a subsequent high-temperature pyrolysis process. Compared with other methods, it has significant advantages and characteristics:
[0003] Good density. During the preparation process, polymers (such as polycarbosilane) repeatedly fill the pores in the composite material through an impregnation and pyrolysis process. After each cycle, the density of the material will be improved. This layer-by-layer construction method makes the final product have extremely high density, which is crucial to improving the overall performance of the material, especially for applications that need to withstand high pressure and high temperature. Good density can significantly improve the durability and service life of the material.
[0004] Lower manufacturing temperature. Because polycarbosilane can undergo pyrolysis chemical reactions at lower temperatures, the PIP method can prepare silicon carbide ceramics at relatively low temperatures (around 1200°C). This feature not only reduces energy consumption and production costs, but also helps to reduce the material performance degradation that may occur at high temperatures, especially for silicon carbide fibers and alumina fibers. In addition, lower manufacturing temperatures also mean that a wider range of equipment and tools can be used, increasing process flexibility.
[0005] Good fiber wettability. The polymer can well wet the reinforcing fibers during the impregnation stage by regulating the composition and surface tension. The polymer can penetrate deeply into the fiber and completely cover each fiber. This good fiber wettability helps to improve the microstructure of the matrix and reduce the porosity, thereby improving the overall strength and toughness of the composite material. For high-performance applications, this improved interface bonding is crucial because it directly affects the tensile strength and impact resistance of the material.
[0006] Easy to shape. In the polymer state before pyrolysis, the material has good plasticity, which makes it easy to shape, process and punch it before finally converting it into ceramics. The PIP method is very suitable for manufacturing parts with complex geometries. This feature provides designers with greater freedom, allowing them to create structural parts that better meet the needs of practical applications, while also reducing manufacturing costs because no additional processing steps are required to form complex shapes.
[0007] Controllable chemical composition. By selecting different polymer raw materials, the chemical composition of the final ceramic matrix can be adjusted to tailor the performance of the material according to specific application requirements. For example, the wear resistance, corrosion resistance or other key properties of the composite material can be changed by adding specific additives. This flexibility makes the PIP method an ideal choice for developing new high-performance ceramic-based composites for specific environmental conditions.
[0008] However, the current PIP method still has some shortcomings:
[0009] Long cycle: The PIP process requires multiple cycles to obtain a sufficiently dense material. Each cycle includes steps such as impregnation, drying, and pyrolysis, which results in a long overall process cycle.
[0010] Higher cost: Although the temperature of a single operation is low, the overall cost is still high considering the need for multiple cycles and the use of special polymer raw materials.
[0011] Residual stress: Multiple pyrolysis treatments at high temperatures during the pyrolysis process produce large residual stresses, which may affect the performance of the material.
[0012] In summary, the PIP method is an effective means to prepare high-performance silicon carbide ceramic matrix composites, especially when good density and complex shapes are required. However, it also has certain limitations, such as high cost and long production cycle. Summary of the invention
[0013] To solve the above problems, the present invention aims to provide a method for preparing a silicon carbide ceramic matrix composite material by continuous polycarbosilane impregnation pyrolysis sintering, wherein the schematic diagram of the preparation equipment is shown in Figure 1 , including 10 covers, 20 quartz tubes, 30 liquid inlet tubes, 40 induction coils, 50 induction crucibles, 60 fiber preforms, 70 brackets, 80 balances, 90 solution tanks, 100 liquid outlet tubes, 110 vacuum pumps, and 120 air inlet tubes. The positions of the liquid outlet tubes 100, 110 vacuum pumps, and 120 air inlet tubes shown in the figure are interchangeable at the upper and lower ends of the quartz tube, and are mainly used for preparing silicon carbide ceramic-based composites by rapid polycarbosilane impregnation, pyrolysis, and sintering.
[0014] A method for preparing a silicon carbide ceramic-based composite material by continuous polycarbosilane impregnation pyrolysis sintering, characterized in that it comprises the following steps in order: (1) placing a fiber preform, a preform, and a woven part into an induction crucible, and recording the weight using a balance; (2) injecting a liquid organic solution into a solution tank, preferably kerosene, transformer oil, xylene, or a mixed oil with silicone rubber and polycarbosilane, and introducing the oil into the induction crucible through a liquid inlet pipe. After being fully immersed, the oil is discharged into the solution tank through a liquid outlet pipe; (3) starting After the vacuum pump is turned on, the power supply of the induction coil is started, maintained for a certain period of time, and the power supply of the induction coil is turned off, and the mass indicated on the electronic balance is recorded; (4) A mixed solution of polycarbosilane and solvent is injected into the solution tank, and under a negative pressure environment, polycarbosilane is introduced into the induction crucible through the liquid inlet pipe. After sufficient immersion, the vacuum pump is turned off, gas is injected into the quartz tube, and the polycarbosilane is guided into the solution tank through the liquid outlet pipe; (5) After starting the vacuum pump, the power supply of the induction coil is started, and air is introduced, and maintained at 200-400°C for 2-5 hours; the air is replaced with nitrogen Gas, continue to heat to 700-1000℃ for pyrolysis, keep for 1-2 hours, turn off the power of the induction coil, and record the mass shown on the electronic balance; (6) repeat steps (4) and (5) 2-4 times, when the weight gain of the fiber preform is less than 2-5%, stop repeating, and record the mass shown on the electronic balance; (7) continue to heat to 1100-1400℃ for sintering, keep warm for 0.5-2.5 hours, and record the mass shown on the electronic balance; (8) repeat steps (4)(5)(6)(7), and record the mass shown on the electronic balance. (9) When the weight gain rate after sintering at 1100-1400°C is less than 1%, stop the cycle, the fiber preform has become a ceramic matrix composite blank, open the quartz tube furnace to take out the blank, grind the surface into a semi-finished product, the grinding depth is 1-3 mm, clean with an organic solvent, weigh the semi-finished product after drying, continue to put it into the quartz tube furnace, and record the mass shown on the electronic balance; (10) Repeat steps (4)(5)(6)(7)(8)(9) 1-3 times, and the density of the semi-finished product reaches 1.9 g / cm 3 , the open porosity is less than 10%; (11) the semi-finished product is impregnated with xylene solution under pressure, the mass percentage of polycarbosilane in the xylene solution is 15-35%, and after the impregnation is completed, it is placed in a quartz tube furnace; (12) repeating step (5), the pyrolysis temperature is 900-1000°C, recording the mass shown on the electronic balance, and taking out the finished product; (13) repeating steps (11) and (12) 2-5 times, repeating step (7) once; (14) repeating step (13) 1-5 times, when the density of the finished product is greater than 2.1g / cm 3 , or it is greater than the production demand, stop the above experiment, perform surface finishing on the sample, and complete the production process.
[0015] Compared with the prior art, the present invention has the following beneficial effects: (1) the product production efficiency is high and the cycle is short, which is 30% higher than the existing method; (2) less waste of raw materials and 10% cost saving; (3) improved thermal efficiency and 20% reduction in energy consumption; (4) less fiber damage, the strength of the ceramic-based composite material is increased by 40%, and the fracture strain is increased by 50%. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a schematic diagram of the equipment for preparing silicon carbide ceramic-based composite materials according to the present invention.
[0017] In the figure, 10 is a cover, 20 is a quartz tube, 30 is a liquid inlet pipe, 40 is an induction coil, 50 is an induction crucible, 60 is a fiber preform, 70 is a bracket, 80 is a balance, 90 is a solution tank, 100 is a liquid outlet pipe, 110 is a vacuum pump, and 120 is an air inlet pipe. DETAILED DESCRIPTION
[0018] The present invention is further explained below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art are all within the scope of the claims attached to this application.
[0019] Example 1 Silicon carbide fiber reinforced silicon carbide ceramic matrix composite bearing tube
[0020] The equipment includes 10 a cover, 20 a quartz tube, 30 a liquid inlet tube, 40 an induction coil, 50 an induction crucible, 60 a fiber preform, 70 a bracket, 80 a balance, 90 a solution tank, 100 a liquid outlet tube, 110 a vacuum pump, 120 an air inlet tube, and the pipeline connecting the vacuum and the quartz tube 110 and the air inlet tube 120 can be at the bottom of the quartz tube.
[0021] The preparation method comprises the following steps in order: (1) placing the fiber cloth-wrapped bearing tube preform together with the mold flatly into an induction carbon / carbon composite material crucible, and recording the weight by a balance; (2) injecting kerosene into a solution tank, and introducing the oil into the induction crucible through a liquid inlet pipe. After soaking for 1 hour, the kerosene is discharged into the solution tank through a liquid outlet pipe; (3) after starting the vacuum pump, starting the induction coil power supply, heating the crucible to 1000°C in 5 minutes, maintaining it for 30 minutes, turning off the induction coil power supply, and recording the mass indicated by the electronic balance. (4) A mixed solution of polycarbosilane and xylene solvent was injected into the solution tank in a mass ratio of 1:1. Under negative pressure, polycarbosilane was introduced into the induction crucible through the liquid inlet pipe. After soaking for 2 hours, the vacuum pump was turned off, air was injected into the quartz tube to increase the pressure, and the polycarbosilane solution was led out to the solution tank through the liquid outlet pipe; (5) After starting the vacuum pump, the power supply of the induction coil was started, and air was introduced, and maintained at 400°C for 2 hours; the air was replaced with nitrogen, and the temperature was continued to rise to 700°C for pyrolysis, maintained for 1 hour, and the induction was turned off. Coil power supply, record the mass shown on the electronic balance; (6) repeat steps (4) and (5) 4 times, the pyrolysis temperature is increased by 50°C each time the cycle is repeated, when the fiber preform weight gain is less than 2%, stop repeating, record the mass shown on the electronic balance; (7) continue to heat to 1150°C for sintering, keep warm for 1 hour, record the mass shown on the electronic balance; (8) repeat steps (4)(5)(6)(7) 3 times, record the mass shown on the electronic balance; (9) after 3 times the weight gain is 0.8%, which is less than 1%, stop the cycle, the fiber preform weight gain is less than 1%, stop the cycle, the fiber preform weight gain is less than 2 ... The fiber preform has become a ceramic-based composite blank. Open the quartz tube furnace to take out the blank, remove the mold, grind the surface of the fiber bearing tube preform into a semi-finished product with a grinding depth of 2 mm, clean with acetone, weigh the semi-finished product after drying, and put it into the quartz tube furnace upright to record the mass shown on the electronic balance; (10) Repeat steps (4)(5)(6)(7)(8)(9) 2 times, and reduce the grinding depth by 1 mm for the second time. The processing depth ensures the minimum product size. The density of the semi-finished product is 2.1 g / cm 3 , open porosity 8%; (11) the semi-finished product is impregnated with a xylene solution of polycarbosilane under pressure at a pressure of 5 atmospheres, the mass percentage of polycarbosilane in the xylene solution is 20%, and after impregnation, it is placed in a quartz tube furnace; (12) step (5) is repeated, the pyrolysis temperature is 900°C, the mass shown on the electronic balance is recorded, and the finished product is taken out; (13) steps (11) and (12) are repeated twice, each time the pyrolysis temperature is increased by 50°C, step (7) is repeated once, and the sintering temperature is 1200°C; (14) step (13) is repeated twice, and the density of the semi-finished product is 2.4g / cm 3 , stop the above experiment, perform surface finishing on the sample, complete the production process, and obtain the silicon carbide fiber reinforced silicon carbide ceramic matrix composite bearing tube.
[0022] Example 2 Preparation of carbon fiber reinforced silicon carbide ceramic matrix composite liquid rocket engine nozzle
[0023] The equipment includes 10 a cover, 20 a quartz tube, 30 a liquid inlet tube, 40 an induction coil, 50 an induction crucible, 60 a fiber preform, 70 a support, 80 a balance, 90 a solution tank, 100 a liquid outlet tube, 110 a vacuum pump, 120 an air inlet tube, 110 a pipeline connecting the vacuum and the quartz tube, and 120 an air inlet tube at the top of the quartz tube.
[0024] The preparation method comprises the following steps in order: (1) placing a three-dimensional four-way woven carbon fiber liquid rocket engine preform together with a mold upright into an induction crucible, and recording the weight using a balance; (2) injecting an oil solution having a mass fraction ratio of 1 part of polycarbosilane: 1 part of kerosene: 1 part of methyl vinyl silicone rubber: 1 part of xylene into a solution tank, and introducing the oil into the induction crucible through a liquid inlet pipe. After soaking for 2 hours, the oil is discharged into the solution tank through a liquid outlet pipe; (3) starting a vacuum pump and then starting a power supply for the induction coil, and then heating the induction coil for 10 minutes. The temperature was raised to 800°C and maintained for 1 hour. The power supply of the induction coil was turned off and the mass indicated on the electronic balance was recorded. (4) A mixed solution of polycarbosilane and xylene solvent was injected into the solution tank in a mass ratio of 2:1. Under negative pressure, polycarbosilane was introduced into the induction crucible through the liquid inlet pipe. After soaking for 2 hours, the vacuum pump was turned off, gas was injected into the quartz tube, and polycarbosilane was led out to the solution tank through the liquid outlet pipe. (5) After starting the vacuum pump, the power supply of the induction coil was started and air was introduced. The temperature was kept at 350°C for 3 hours. The air was replaced with nitrogen. Continue to heat up to 800°C for pyrolysis, keep it for 2 hours, turn off the power supply of the induction coil, and record the mass shown on the electronic balance; (6) Repeat steps (4) and (5) 3 times. When the weight gain of the fiber preform is less than 3%, stop repeating and record the mass shown on the electronic balance; (7) Continue to heat up to 1200°C for sintering, keep it warm for 1 hour, and record the mass shown on the electronic balance; (8) Repeat steps (4)(5)(6)(7) 3 times. After each repetition, change the mixed solution of polycarbosilane and xylene solvent to a mass ratio of 1:1.1. Gradually increase, and record the mass shown on the electronic balance; (9) After sintering, the weight gain rate is less than 0.9%, stop the cycle, the fiber preform has become a ceramic-based composite material blank, open the quartz tube furnace to take out the blank, remove the mold, grind the surface into a semi-finished product, the grinding depth is 1mm, clean with an organic solvent, weigh the semi-finished product after drying, and continue to put it into the quartz tube furnace, and record the mass shown on the electronic balance; (10) Repeat steps (4)(5)(6)(7)(8)(9) 3 times, and the density of the semi-finished product reaches 2.0g / cm 3, the open porosity is less than 10%; (11) the semi-finished product is impregnated with xylene solution under pressure, the mass percentage of polycarbosilane in the xylene solution is 15-35%, and after the impregnation is completed, it is placed in a quartz tube furnace; (12) repeat step (5), the pyrolysis temperature is 1000℃, record the mass shown on the electronic balance, and take out the finished product; (13) repeat steps (11) and (12) twice, repeat step (7) once; (14) repeat step (13) twice, the density of the finished product is greater than 2.2g / cm 3 , stop the above experiment, perform surface finishing on the sample, complete the production process, and obtain the liquid rocket engine nozzle.
Claims
1. A method for preparing a silicon carbide ceramic-based composite material by continuous polycarbosilane impregnation pyrolysis sintering, characterized in that The preparation equipment includes 10 covers, 20 quartz tubes, 30 liquid inlet pipes, 40 induction coils, 50 induction crucibles, 60 fiber preforms, 70 brackets, 80 balances, 90 solution tanks, 100 liquid outlet pipes, 110 vacuum pumps, 120 air inlet pipes, and the pipes connected to the vacuum pump 110 and the air inlet pipes 120 are adjusted in position according to product requirements.
2. The method according to claim 1, characterized in that The steps include: (1) Place the fiber preform, preform, and braided part into an induction crucible and record the weight using a balance; (2) injecting a liquid organic solution into the solution tank, preferably kerosene, transformer oil, xylene, or a mixed oil with silicone rubber or polycarbosilane, and introducing the oil into the induction crucible through the liquid inlet pipe. After being fully immersed, the oil is guided into the solution tank through the liquid outlet pipe; (3) After starting the vacuum pump, start the induction coil power supply, keep the crucible heated for a certain period of time, turn off the induction coil power supply, and record the mass shown on the electronic balance; (4) A mixed solution of polycarbosilane and solvent is injected into the solution tank. Under negative pressure, the polycarbosilane solution is introduced into the induction crucible through the liquid inlet pipe. After sufficient immersion, the vacuum pump is turned off, gas is injected into the quartz tube, and the polycarbosilane is led out to the solution tank through the liquid outlet pipe; (5) After starting the vacuum pump, start the power supply of the induction coil and introduce air, and keep it at 200-400°C for 2-5 hours; replace the air with nitrogen, continue to heat up to 700-1000°C for pyrolysis, keep it for 1-2 hours, turn off the power supply of the induction coil, and record the mass shown on the electronic balance; (6) Repeat steps (4) and (5) 2 to 4 times. When the weight gain of the fiber preform is less than 2 to 5%, stop repeating and record the mass shown by the electronic balance. (7) Continue to heat up to 1100-1400°C for sintering, keep warm for 0.5-2.5 hours, and record the mass shown on the electronic balance; (8) Repeat steps (4), (5), (6), (7) and record the mass indicated by the electronic balance; (9) When the weight gain rate after sintering at 1100-1400° C. is less than 1%, the cycle is stopped, and the fiber preform has become a ceramic matrix composite material blank. The quartz tube furnace is opened to take out the blank, and the surface is ground into a semi-finished product with a grinding depth of 0.5-3 mm. The semi-finished product is cleaned with an organic solvent, and then weighed after drying, and then put into the quartz tube furnace again, and the mass shown by the electronic balance is recorded; (10) Repeat steps (4)(5)(6)(7)(8)(9) 1 to 3 times until the semi-finished product density reaches 1.9 g / cm 3 , open porosity is less than 10%; (11) impregnating the semi-finished product with a xylene solution of polycarbosilane under pressure, wherein the mass percentage of polycarbosilane in the xylene solution is 15 to 35%, and placing the semi-finished product in a quartz tube furnace after the impregnation is completed; (12) Repeat step (5) at a pyrolysis temperature of 900-1000° C., record the mass indicated by the electronic balance, and take out the semi-finished product; (13) Repeat steps (11) and (12) 2 to 5 times, and repeat step (7) once; (14) Repeat step (13) 1 to 5 times. When the density of the finished product is greater than 2.1 g / cm 3 , or it is greater than the production demand, stop the above experiment, perform surface finishing on the sample, and complete the production process.
Citation Information
Patent Citations
Method for preparing carbon-fiber-reinforced silicon carbide composite material
CN102249721A
Device for impregnating carbon fiber preform in SiC precursor solution and process method thereof
CN103373857A
Preparation method for ultra-high-temperature ceramic modified C / C composite material
CN105016760A
Method for manufacturing ceramic matrix composite boron nitride interface coating
CN105463403A
Preparation method for binary ceramic modified C / C composite material
CN106478120A