Double-net-shaped composite hydrogel as well as preparation method and application thereof

Through the preparation of double-network composite hydrogel IA-PAAM/PAMPS, the problem that decontamination materials in the prior art are difficult to efficiently remove multiple radionuclides at the same time, and efficient removal of actinide elements and fission products is achieved. It has short action time and wide applicability.

CN118878747AInactive Publication Date: 2024-11-01SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410976015.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult for existing decontamination materials to remove multiple radionuclides efficiently at the site of nuclear accidents, and the effect time is long, so decontamination cannot be achieved in time.

Method used

The preparation method of double-network composite hydrogel IA-PAAM/PAMPS was used to prepare porous loose mesh structure hydrogel composed of AMPS, AAM and IA by in-situ polymerization impregnation, using N,N'-methylene group Bisacrylamide is used as a crosslinking agent and ammonium persulfate is used as an initiator. Combined with the expansion properties and acid-base stability of IA-PAAM/PAMPS, it achieves efficient adsorption of actinide elements and fission products.

Benefits of technology

Achieve efficient removal of a variety of radionuclides, especially the simultaneous removal rate of actinide elements (UO22+, Th4+) and fission products (Sr2+, Cs+) is greater than 90%, and has a short action time and wide application applicability. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118878747A_ABST
    Figure CN118878747A_ABST
Patent Text Reader

Abstract

The invention discloses double-net-shaped composite hydrogel as well as a preparation method and application thereof, and belongs to the technical field of radionuclide removal. According to the invention, through in-situ polymerization and impregnation, a dual-network composite hydrogel IA-PAAM / PAMPS with iminodiacetic acid, acrylamide and 2-acrylamide-2-methylpropanesulfonic acid as base materials is synthesized, and the preparation method comprises the following steps: (1) preparing an IA-PAAM hydrogel; (2) preparing an AMPS solution; and (3) soaking the IA-PAAM hydrogel in an AMPS (2-amino-2-methylpropanesulfonic acid) solution, so as to obtain the IA-PAAM / PAMPS double-net-shaped composite hydrogel. The double-net-shaped composite hydrogel can be used for removing nuclides in a solution or on the surface of a solid, and the problems that an existing decontamination material is long in acting time and lacks the capacity of generally removing various nuclides are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of radionuclide removal, and in particular relates to a double-net composite hydrogel and a preparation method and application thereof. Background Art

[0002] Nuclear energy has the advantages of low cost and no greenhouse effect, and has been developed rapidly. However, it also brings many potential dangers. For example, the radioactive nuclides leaked in nuclear accidents will cause uncertain harm to the human body and the surface of nuclear facilities, such as long-term tissue damage caused by radioactive nuclides entering the human body through the skin. Among various radioactive nuclides, actinides attached to solid surfaces (such as UO2 2+ and Th 4+ ) and fission products (such as Sr 2+ and Cs + ) is difficult to be completely removed due to its long half-life and high yield. Therefore, the development of decontamination materials for environmental remediation after nuclear accidents and their application in the nuclear industry are of great significance.

[0003] The decontamination methods currently used mainly include physical decontamination, chemical decontamination and electrochemical decontamination. Physical decontamination is the main method for achieving surface decontamination at nuclear accident sites. However, the use of traditional physical methods such as high-pressure water cannons or grinding not only destroys the overall structure of the building, but also causes secondary pollution to the environment. The technical methods of electrochemical decontamination are limited by underdeveloped technology and high costs. Relatively speaking, chemical decontamination is not only efficient, but also reduces secondary pollution to the environment. It is a very promising new method. Decontamination materials currently used to remove radionuclides from solid surfaces include chemical chelating detergents, strippable coatings, foams and hydrogels. However, due to the complexity of nuclear accident sites and the shortness of emergency response time, it is necessary to effectively decontaminate several radionuclides at the same time. However, most existing decontamination materials cannot meet the above two characteristics at the same time. For example, the most widely used material for solid surface purification is a strippable coating synthesized based on polyvinyl alcohol (PVA). Although the strippable coating has a high removal rate of surface radionuclides, due to its long drying time, decontamination cannot be achieved in time at the nuclear contaminated site of a nuclear accident. Therefore, it is necessary to develop highly efficient and versatile decontaminants to remove radionuclides from nuclear accident sites. Among the many materials for removing radionuclides, hydrogels have attracted much attention due to their good hydrophilicity and adsorption properties as well as low cost. In recent years, researchers have made breakthroughs in the application of hydrogels in bioremediation and mechanical properties, but their ability to remove radionuclides has not yet been verified. Summary of the invention

[0004] In view of the above-mentioned prior art, the present invention provides a double-network composite hydrogel and a preparation method and application thereof, which solve the problems that the existing decontamination materials have a long action time and lack the ability to universally remove various nuclides.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is: to provide a method for preparing a double-network composite hydrogel, comprising the following steps:

[0006] (1) Preparation of IA-PAAM hydrogel;

[0007] S1. dissolving acrylamide (AAM) in a solvent to obtain a solution with a concentration of 1 to 3 mol / L;

[0008] S2. Add N,N'-methylenebisacrylamide (MBAA), ammonium persulfate (APS), iminodiacetic acid (IA) and N,N,N',N'-tetramethyleneethylenediamine (TEMED) to the obtained solution, stir evenly to obtain a precursor solution; the amount of N,N'-methylenebisacrylamide, ammonium persulfate, iminodiacetic acid and N,N,N',N'-tetramethyleneethylenediamine and acrylamide is 25-35 mg: 4-5 mg: 0.1-0.2 g: 40-60 μL: 10-30 mmol;

[0009] S3. The precursor solution is heated at 60-80°C for 4-6 hours to obtain IA-PAAM hydrogel;

[0010] (2) preparing an AMPS solution;

[0011] Dissolve 2-acrylamide-2-methylpropanesulfonic acid (AMPS), N,N'-methylenebisacrylamide and ammonium persulfate in a solvent and stir evenly to obtain an AMPS solution; the dosage of 2-acrylamide-2-methylpropanesulfonic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 5-15 mmol: 50-70 mg: 1-2 mg;

[0012] (3) Preparation of IA-PAAM / PAMPS double-network composite hydrogel;

[0013] The IA-PAAM hydrogel prepared in step (1) is immersed in the AMPS solution prepared in step (2) at room temperature for 10 to 14 hours, and then reacted at 60 to 80° C. for 4 to 6 hours to obtain the hydrogel.

[0014] The beneficial effect of the technical scheme adopted in the present invention is: an in-situ polymerization impregnation method is adopted, N,N'-methylenebisacrylamide is used as a cross-linking agent, and ammonium persulfate is used as an initiator to prepare a double-network composite hydrogel IA-PAAM / PAMPS composed of AMPS, AAM and IA, the raw materials for preparation are easy to obtain, and the preparation method is simple.

[0015] Based on the above technical solution, the present invention can also be improved as follows.

[0016] Further, the amount of N,N'-methylenebisacrylamide, ammonium persulfate, iminodiacetic acid and N,N,N',N'-tetramethyleneethylenediamine and acrylamide is in the relationship of 30 mg:4.5 mg:0.1 g:50 μL:20 mmol;

[0017] In S3, the heating temperature is 70°C and the heating time is 5h;

[0018] The dosage relationship of 2-acrylamide-2-methylpropanesulfonic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 10mmol:61.88mg:1.5mg;

[0019] In step (3), the room temperature immersion time is 12 hours, the reaction temperature is 70° C., and the reaction time is 5 hours.

[0020] Furthermore, the double-network composite hydrogel is prepared by the above-mentioned preparation method of the double-network composite hydrogel.

[0021] The beneficial effect of the further technical solution adopted in the present invention is that the double-network composite hydrogel IA-PAAM / PAMPS has a porous and loose network structure.

[0022] Furthermore, the double-network composite hydrogel is used in removing nuclides in solution or on a solid surface.

[0023] The beneficial effect of the above further technical solution of the present invention is that the double-network composite hydrogel can be applied to a variety of environments, has a wide range of applications, is highly practical, and has the advantage of a short action time.

[0024] Further, the nuclide is an actinide or a fission product.

[0025] Further, the actinide element is UO2 2+ or 4+ , the fission product is Sr 2+ or Cs + .

[0026] Further, the solid is glass, plastic or stainless steel.

[0027] Further, the method for removing nuclides from solid surfaces comprises the following steps:

[0028] The double-network composite hydrogel was pressurized at 0.35-1.2 g / cm 2 Apply an amount of the coating on a solid surface and keep it at 25-60°C for 10-30 minutes.

[0029] Further, the method for removing nuclides from the solution comprises the following steps:

[0030] The pH value of the solution containing the nuclide is adjusted to 2-9, and then the double-network composite hydrogel is added to the solution after the pH adjustment in an amount of 0.5-2 mg / mL, and maintained at 25-60° C. for 10-240 minutes.

[0031] Further, the double-network composite hydrogel was vacuum dried to obtain a freeze-dried double-network composite hydrogel, and the amount of the freeze-dried double-network composite hydrogel added to the solution was 1 mg / mL.

[0032] The beneficial effects of the present invention adopting the above further technical solution are: being able to effectively remove multiple nuclides and having the ability of highly efficient adsorption and universal decontamination of radioactive nuclides.

[0033] The beneficial effects of the present invention are as follows: the present invention successfully synthesized a double-network composite hydrogel IA-PAAM / PAMPS composed of AAM, IA and AMPS, and used it for radionuclide decontamination of solutions and solid surfaces. The hydrogel swelling experiment showed that the hydrogel had good swelling performance; the adsorption experiment of nuclides confirmed that IA-PAAM / PAMPS had excellent binding ability to nuclides, and had good affinity for Sr 2+ and UO2 2+ The maximum adsorption capacity of IA-PAAM / PAMPS was 267.3 mg / g and 659.0 mg / g respectively; IA-PAAM / PAMPS could maintain good adsorption capacity in different acid and alkaline environments; IA-PAAM / PAMPS was applied to the surface contaminated by radionuclides and showed good decontamination ability, and Sr was removed within 10 min. 2+ and UO2 2+ Most of the radionuclides on various solid surfaces contaminated by IA-PAAM / PAMPS have excellent universal decontamination performance for radionuclides, and can remove actinides (UO2 2+ , Th4 + ) and fission products (Sr 2+ , Cs + ) were removed simultaneously, with a removal rate of more than 90.0%; FT-IR, XPS, SEM-EDS and other analytical methods confirmed that radionuclides can specifically bind to the hydroxyl and sulfonic acid groups in IA-PAAM / PAMPS. Therefore, the double-network composite hydrogel IA-PAAM / PAMPS can be widely used as an efficient universal decontaminant for radionuclide solutions and solid nuclear contaminated surfaces. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a diagram showing the expansion characteristics test results of the double-network composite hydrogel;

[0035] Figure 2 The results of the acid-base stability test of the double-network composite hydrogel are shown in Figure 1.2 + The adsorption amount of IA-PAAM / PAMPS varies with pH value. 2+ The variation trend of adsorption amount with pH value;

[0036] Figure 3 The adsorption kinetics test results of the double-network composite hydrogel are shown in Figure 2, where a is Sr 2+ Adsorption kinetic curve of UO2 2+ Adsorption kinetics curve of

[0037] Figure 4 The adsorption kinetics test results of the double-network composite hydrogel are shown in Figure 2; a is Cs + Adsorption kinetic curve of Th 4+ Adsorption kinetics curve of

[0038] Figure 5 is the isothermal fitting curve of the double network composite hydrogel; where a is Sr 2+ Isotherm fitting curve of UO2 2+ Isotherm fitting curve of

[0039] Figure 6 The results of the detection of the decontamination ability of the double-network composite hydrogel on different solid surfaces; a~c are the decontamination performance of IA-PAAM / PAMPS on Sr 2+ The purification efficiency of contaminated surfaces (i.e., plastic, stainless steel, and glass), d~e are IA-PAAM / PAMPS for UO2 2+ Decontamination efficiency on contaminated surfaces (i.e. plastic, stainless steel and glass);

[0040] Figure 7 This is a diagram showing the universality experimental results of the double-network composite hydrogel;

[0041] Figure 8 This is a test result of the decontamination effect of the double-network composite hydrogel at 60°C;

[0042] Fig. 9 is a graph showing the relationship between the efficiency of decontamination radionuclides and the mass of gel per unit area;

[0043] Fig.10 This is a scanning electron microscope (SEM) test result of the double-network composite hydrogel;

[0044] Fig.11 This is a Fourier transform infrared spectroscopy (FT-IR) analysis result diagram of the double-network composite hydrogel;

[0045] Fig.12 XRD spectra of AAM, PAAM / PAMPS and IA-PAAM / PAMPS;

[0046] Fig.13 is the FT-IR spectrum of the double-net composite hydrogel after adsorption of nuclides; a is the double-net composite hydrogel adsorbing Sr 2+ , b is the double network composite hydrogel adsorbing UO2 2+ ;

[0047] Fig.14 To adsorb Sr 2+ Full XPS spectra of IA-PAAM / PAMPS before and after; a represents the XPS peak of Sr 3d, b represents the N1s spectrum; c represents the S2p spectrum, and d represents the O1S spectrum;

[0048] Fig.15 To adsorb UO2 2+ Full XPS spectra of IA-PAAM / PAMPS before and after; a represents the XPS peak of U4f, b represents the N1s spectrum; c represents the S2p spectrum, and d represents the O1S spectrum;

[0049] Fig.16 The double-network composite hydrogel can simultaneously adsorb actinide elements (UO2 2+ ,Th 4+ ) and fission products (Sr 2+ , Cs + ) after SEM image;

[0050] Fig.17 The double-network composite hydrogel can simultaneously adsorb actinide elements (UO2 2+ ,Th 4+ ) and fission products (Sr 2+ , Cs + ) after . DETAILED DESCRIPTION

[0051] The specific implementation modes of the present invention are described in detail below with reference to the embodiments.

[0052] Example 1

[0053] A double-network composite hydrogel IA-PAAM / PAMPS, the preparation steps of which are as follows:

[0054] (1) Preparation of IA-PAAM hydrogel

[0055] S1. Add 20 mmol AAM (acrylamide) to 10 mL deionized water and stir in a magnetic stirrer for 5 min to obtain a clear solution;

[0056] S2. 30 mg MBAA (N, N'-methylenebisacrylamide), 4.5 mg APS (ammonium persulfate) and 0.1 g IA (iminodiacetic acid) were added to the clear solution in sequence and stirred evenly;

[0057] S3. Add 50 μL TEMED (N,N,N',N'-tetramethyleneethylenediamine) to the solution and stir evenly;

[0058] S4. Heat the solution at 70°C for 5 h to obtain IA-PAAM hydrogel.

[0059] (2) Preparation of AMPS solution

[0060] S1. Add 10 mmol AMPS (2-acrylamide-2-methylpropanesulfonic acid) to 10 mL of deionized water and stir for 5 min to obtain a clear solution;

[0061] S2. Add 61.88 mg MBAA (N,N'-methylenebisacrylamide) and 1.5 mg APS (ammonium persulfate) to the clear solution and continue stirring to obtain an AMPS solution;

[0062] (3) Preparation of IA-PAAM / PAMPS double-network composite hydrogel

[0063] S1. Soak the IA-PAAM hydrogel prepared in step (1) in the AMPS solution prepared in step (2) at room temperature for 12 h;

[0064] S2. Place in a 70°C drying oven and react for 5 hours to obtain a double-network composite hydrogel IA-PAAM / PAMPS.

[0065] Example 2

[0066] A freeze-dried double-network composite hydrogel, the preparation steps of which are as follows:

[0067] (1) The prepared hydrogel was washed three times in deionized water and placed in a -20°C refrigerator for 24 h;

[0068] (2) The frozen hydrogel is placed in a freeze drying box for vacuum drying, and taken out after being completely dried.

[0069] Comparative Example 1

[0070] A PAAM / PAMPS hydrogel, the preparation steps of which are as follows:

[0071] (1) Preparation of PAAM hydrogel

[0072] S1. Add 20 mmol AAM to 10 mL deionized water and stir in a magnetic stirrer for 5 min to obtain a clear solution;

[0073] S2. Add 30 mg MBAA and 4.5 mg APS to the clear solution in sequence and stir evenly;

[0074] S3. Add 50 μL TEMED to the solution and stir evenly;

[0075] S4. Heat the solution at 70°C for 5 h to obtain PAAM hydrogel.

[0076] (2) Preparation of AMPS solution

[0077] S1. Add 10 mmol AMPS to 10 mL of deionized water and stir for 5 min to obtain a clear solution;

[0078] S2. Add 61.88 mg MBAA and 1.5 mg APS to the clear solution and continue stirring to obtain an AMPS solution;

[0079] (3) Preparation of PAAM / PAMPS double-network composite hydrogel

[0080] S1. Soak the PAAM hydrogel prepared in step (1) in the AMPS solution prepared in step (2) at room temperature for 12 h;

[0081] S2. Place in a 70°C drying oven and react for 5 hours to obtain the hydrogel PAAM / PAMPS.

[0082] (4) Freeze-dried PAAM / PAMPS hydrogel

[0083] The preparation steps are the same as those in Example 2.

[0084] Comparative Example 2

[0085] A PAAM hydrogel, the preparation steps of which are as follows:

[0086] S1. Add 20 mmol AAM to 10 mL deionized water and stir in a magnetic stirrer for 5 min to obtain a clear solution;

[0087] S2. Add 30 mg MBAA and 4.5 mg APS to the clear solution in sequence and stir evenly;

[0088] S3. Add 50 μL TEMED to the solution and stir evenly;

[0089] S4. The solution was heated at 70°C for 5 h to obtain a PAAM hydrogel;

[0090] S5. Freeze-dried PAAM hydrogel, the preparation steps of which are the same as those in Example 2.

[0091] Application Example 1

[0092] Double-net composite hydrogel swelling performance test:

[0093] A certain mass of freeze-dried hydrogel (IA-PAAM / PAMPS, PAAM / PAMPS, PAAM) was weighed and immersed in deionized water. It was taken out at a certain time (10, 20, 30, 60, 90 min), and the surface moisture was absorbed with absorbent paper. Finally, it was weighed and the data was recorded.

[0094] The expansion rate SR is calculated according to formula (1):

[0095]

[0096] Where M0 (mg) is the mass of freeze-dried hydrogel, M t (mg) is the mass of the gel after absorbing water at a certain moment.

[0097] The swelling properties of the double-network composite hydrogel were tested. Figure 1 As shown in the figure, IA-PAAM / PAMPS exhibits excellent water swelling properties and reaches swelling equilibrium within 30 min. The swelling rate of the gel reaches 6000%, which is much higher than that of PAAM and PAAM / PAMPS hydrogels. This indicates that the large amount of IA carboxyl groups contained in IA-PAAM / PAMPS improves the water binding properties of IA-PAAM / PAMPS.

[0098] Application Example 2

[0099] Acid and alkali resistance test of double-network composite hydrogel IA-PAAM / PAMPS

[0100] (1) Set up solutions with different pH values, where UO2 2+ The solution pH values ​​were set to 1, 1.5, 2, 3, 4, 5, and 6, respectively. 2+ The solution pH values ​​were set to 1, 2, 3, 4, 5, 6, 7, 8, and 9, respectively. 2+ and UO2 2+ The initial concentration of each is 100 ppm, and 5 mL of each nuclide solution is taken;

[0101] (2) Add 5 mg of freeze-dried double-network composite hydrogel to 5 mL of radionuclide contaminated solution and treat for 30 min at a temperature of 25°C.

[0102] After the radionuclide adsorption experiment was completed, the hydrogel in the solution was filtered and the concentration of radionuclide in the remaining solution was determined by ICP-OES. The radionuclide removal rate RE (%) was calculated according to formula (2):

[0103]

[0104] Where C0 (mg / L) and C e (mg / L) is the concentration before and after the removal of radionuclides.

[0105] The acid-base stability test results of the double-network composite hydrogel are as follows Figure 2 As shown in the figure, it is shown that the purification process of uranium and strontium is affected by the pH of the aqueous solution. In particular, the removal rate is relatively low when pH = 1. This is due to the high concentration of H + This causes the functional groups in the hydrogel to be protonated and unable to effectively bind to the nuclide. Figure 2 a It can be seen that the hydrogel has a strong effect on UO2 in the pH range of 2 to 6. 2+ Has good removal ability, by Figure 2 b It can be seen that in the pH range of 2 to 9, the Sr 2+ The removal rate is about 90%, indicating that IA-PAAM / PAMPS has excellent acid and alkali resistance and can be used in a wide range of scenarios.

[0106] Application Example 3

[0107] Adsorption kinetics: Effect of reaction time on the adsorption properties of hydrogels

[0108] At 25 °C, IA-PAAM / PAMPS freeze-dried double-network composite hydrogel was added at 1 mg / mL to a radionuclide contaminated solution with a concentration of 100 ppm and a pH of 4.5. The concentration of radionuclides in the solution was determined by ICP-OES at different times, and the adsorption amount of the hydrogel (q e ):

[0109]

[0110] Where C0 (mg / L) and C e (mg / L) is the concentration before and after the removal of radionuclides.

[0111] The adsorption kinetics curve of the double-network composite hydrogel is shown in Figure 3 As shown, Figure 3 a and 3b show the double-network composite hydrogel IA-PAAM / PAMPS for UO2 2+ and Sr 2+ The variation trend of adsorption amount over time; the adsorption kinetics results are nonlinearly fitted into two different adsorption kinetics models, namely the pseudo-first-order model and the pseudo-second-order model. The pseudo-first-order model is formula (4) and the pseudo-second-order model is formula (5):

[0112]

[0113]

[0114] The adsorption mechanism was discussed based on the correlation coefficient, where k1(min -1 ) and k2(g mg -1 min -1 ) are the rate constants of PFO and PSO, respectively, and t is the reaction time between hydrogel and nuclide.

[0115] like Figure 3 As shown in the figure, as time goes by, the hydrogel reacts with the nuclide, the nuclide is gradually adsorbed, and the adsorption equilibrium is reached within 300 minutes, with a removal rate of more than 95%. The Sr 2+ and UO2 2+ R 2 are 0.994 and 0.998 respectively, while the r values ​​of the two ions obtained by the PFO model are 2 0.978 and 0.994 respectively. For the same ion, the r 2 It is significantly larger than the PFO model, as shown in Table 1, indicating that the adsorption kinetics model of the hydrogel is more consistent with the PSO model. 2+ and UO2 2+ The adsorption conforms to the above-mentioned pseudo-second-order model, and chemical adsorption plays a major role in the adsorption process.

[0116] Table 1 Parameters of hydrogel adsorption kinetics model

[0117]

[0118] like Figure 4 As shown, the double-network composite hydrogel IA-PAAM / PAMPS is effective for Cs + and Th 4+ It also exhibits good affinity and has the potential to be used as a universal adsorbent.

[0119] Application Example 4

[0120] Effect of initial concentration on the adsorption properties of hydrogels

[0121] (1)UO2 2+ : Weigh a certain amount of uranyl nitrate hexahydrate and add it to deionized water to prepare UO2 2+ A solution with a concentration of 20 to 600 ppm and a pH of 4.5; 5 mg of freeze-dried double-net composite hydrogel was added to 5 mL of the prepared solution, and the resulting mixture was placed on a constant temperature stirring table for reaction for 12 hours at a reaction temperature of 37°C;

[0122] (2) Sr 2+ : Prepare Sr with a concentration of 20 to 600 ppm2+ solution, pH 4.5; 5 mg of freeze-dried double-network composite hydrogel was added to 5 mL of the prepared solution, and the obtained mixture was placed on a constant temperature stirring table for reaction for 12 hours at a reaction temperature of 37°C.

[0123] The concentration of the remaining nuclides in the solution was detected by ICP-OES, and the adsorption amount of the hydrogel (q e ). The adsorption isotherm is considered to be the best supporting evidence for the affinity between the adsorbent and the nuclide, and the theoretical maximum adsorption capacity can be calculated through the isotherm model.

[0124] The adsorption isotherm of the double network composite hydrogel is shown in Figure 5 As shown in Figure 2, the adsorption capacity of the hydrogel increases with the increase of the initial concentration of the nuclide and eventually reaches equilibrium. The Langmuir model and the Freundlich model were used to perform nonlinear fitting on the experimental results. The two models are expressed as formula (6) and formula (7), respectively:

[0125]

[0126] Where q m (mg g -1 ) is the maximum adsorption capacity, K L (L mg -1 ) and K F (mg g -1 (L mg- 1 )1 / n) represent the Langmuir constant and the Freundlich constant, respectively. As shown in Table 2, the correlation coefficient of the Langmuir model is significantly greater than that of the Freundlich model, indicating that IA-PAAM / PAMPS has a good effect on the degradation of UO2 2+ and Sr 2+ The chemical adsorption mechanism of q m (Sr 2+ ) is 267.3 mg / g, q m (UO2 2+ ) is 659.0 mg / g; the adsorption performance of the double-network composite hydrogel IA-PAAM / PAMPS for radionuclides is better than that of most materials mentioned in previous studies, indicating that the gel is a promising material for radioactive wastewater treatment.

[0127] Table 2 Hydrogel isothermal adsorption model parameters

[0128]

[0129] Application Example 5

[0130] Double-network composite hydrogels for removal of radionuclide contamination from different solid surfaces

[0131] (1) Plastic, stainless steel and glass were selected as radionuclide contaminated materials, 200 μL of 1000 ppm radionuclide contaminated solution was evenly applied on the surface of the above materials, and then the contaminated materials were placed in a drying oven to dry;

[0132] (2) The contaminated surface was treated with the double-network composite hydrogel IA-PAAM / PAMPS for 10, 20, 30, and 60 min at a temperature of 25°C, and the hydrogel was separated from the solid surface on time.

[0133] The solid surface was cleaned three times with 2% nitric acid solution, and the cleaning solution was collected to detect the radionuclide residue on the solid surface. The decontamination factor (DF) was calculated according to formula (8):

[0134] DF=(C0-C f ) / C0×100% (8)

[0135] Where C0 (mg / L) is the initial concentration of the nuclide, C f (mg / L) is the final concentration after metal surface decontamination.

[0136] Test results such as Figure 6 As shown in the figure, IA-PAAM / PAMPS can effectively remove radionuclides on various solid surfaces in a short time; Sr 2+ The removal rates within 10 min were 97.5%, 90.5% and 78.0%, respectively, and UO2 2+ The removal rates on the surfaces of the above materials were 92.0%, 97.0% and 82.0% respectively. The relatively low removal rate of IA-PAAM / PAMPS on the glass surface may be due to the glass surface being too smooth, resulting in unstable reaction between the hydrogel and the glass, and unable to achieve effective removal.

[0137] Application Example 6

[0138] Universal Experiment of Double-Network Composite Hydrogel IA-PAAM / PAMPS

[0139] (1) Stainless steel was selected as the radionuclide contamination material, and 200 μL of 1000 ppm radionuclide (Sr 2+ , Cs + 、UO2 2 + ,Th 4+ ) The contaminated solution is evenly applied on the surface of the above-mentioned material, and then the contaminated material is placed in a drying oven to dry;

[0140] (2) The double-network composite hydrogel IA-PAAM / PAMPS was coated on the contaminated solid surface, and the treatment time was 10, 20, 30, and 60 min at a treatment temperature of 25°C.

[0141] The solid surface was cleaned three times with 2% nitric acid solution, and samples were collected for detecting radionuclide residues on the solid surface; the decontamination factor (DF) was calculated according to formula (8).

[0142] The scenario of stainless steel surface being contaminated by actinides and fission products was simulated. The results are as follows: Figure 7 As shown, within 10 minutes Sr 2+ , Cs + and UO2 2+ The removal rate of Th is over 95.0%. 4+ The removal rate is relatively low, but still 70.0%.

[0143] Application Example 7

[0144] Decontamination performance of double-network composite hydrogel at 60°C

[0145] (1) Stainless steel was selected as the radionuclide contamination material, and 200 μL of 1000 ppm radionuclide (Sr 2+ 、UO2 2+ ) The contaminated solution is evenly applied on the surface of the above-mentioned material, and then the contaminated material is placed in a drying oven to dry;

[0146] (2) The double-network composite hydrogel IA-PAAM / PAMPS was coated on the contaminated solid surface, and the treatment time was 10, 20, 30, and 60 min at a treatment temperature of 60°C.

[0147] The solid surface was cleaned three times with 2% nitric acid solution, and samples were collected for detecting radionuclide residues on the solid surface; the decontamination factor (DF) was calculated according to formula (8).

[0148] The results are as follows Figure 8 As shown, Figure 7 Compared with the medium removal efficiency, the removal rate shows a downward trend with the increase of temperature. When the treatment time reaches 60 minutes, the removal rate can reach about 80%.

[0149] Application Example 8

[0150] Effect of gel mass per unit area on decontamination efficiency

[0151] (1) Stainless steel was selected as the radionuclide contamination material, and 200 μL of 1000 ppm radionuclide (Sr 2+ , Cs + 、UO2 2 + ,Th4+ ) The contaminated solution is evenly applied on the surface of the above-mentioned material, and then the contaminated material is placed in a drying oven to dry;

[0152] (2) The double-network composite hydrogel IA-PAAM / PAMPS was prepared at 0.35, 0.68, 0.97, and 1.2 g / cm 2 The amount of the coating is applied to the contaminated solid surface, the treatment time is 30 minutes, and the treatment temperature is 25°C.

[0153] The solid surface was cleaned three times with 2% nitric acid solution, and samples were collected for detecting radionuclide residues on the solid surface; the decontamination factor (DF) was calculated according to formula (8).

[0154] The results are as follows Fig. 9 As shown, the gel unit area mass is 0.35~1.2g / cm 2 When the gel unit area mass reaches 0.97 g / cm 2 When the gel mass is 0.35 g / cm2, the decontamination efficiency is the best, and the removal rate of all target nuclides is 90.0%. As the gel mass increases, the nuclide removal rate also increases, indicating that the thickness of the gel increases and the storage space of the nuclides also increases. In addition, a small gel mass can also achieve a relatively high nuclide removal rate. When the gel mass per unit area is 0.35 g / cm2, the removal rate of all target nuclides is 90.0%. 2 When Th 4+ In addition, the removal rates of other radionuclides reached 90.0%, which further proved that IA-PAAM / PAMPS has strong practicality.

[0155] Experimental examples and result analysis

[0156] 1. A high-resolution cold field emission scanning electron microscope (Regulus 8230, Hitachi, Ltd.) was used to detect the double-network composite hydrogel IA-PAAM / PAMPS. The results are as follows: Fig.10 As shown, it can be seen that the hydrogel has a porous and loose network structure. The surface of the hydrogel is smooth in the wet state and has high transparency.

[0157] 2. Use Fourier transform infrared spectroscopy (FT-IR, IR-8400, USA) to record 400-4000 cm -1 The bonding relationship between polymers in the double-network composite hydrogel IA-PAAM / PAMPS within the range of Fig.11 As shown, 1170 cm in IA-PAAM / PAMPS -1 ~1230cm -1 The peak intensity between the bands is weakened, indicating that the CH plane bending vibration contained in AAM is weakened; at 1034cm -1and 618cm -1 The peaks at 1395 cm-1 and 1396 cm-2 correspond to the asymmetric and symmetric stretching of the S=O bond and SO bond in the sulfonic acid group, respectively, indicating that the addition of AMPS increases the number of sulfonic acid groups; the symmetric stretching vibration and bending vibration of -COOH are 1395 cm-1 and 1396 cm-2, respectively. -1 and 2985cm -1 The enhanced peak of C=O contained in carboxylic acid appears at 1565cm -1 , these phenomena indicate that IA-PAAM / PAMPS is the cross-linked product of IA, AAM and AMPS.

[0158] 3. X-ray diffraction (XRD, X Pert pro, Panaco, Netherlands) was used to study the synthesis mechanism and crystal structure of the hydrogel. The XRD spectra of AAM, PAAM / PAMPS and IA-PAAM / PAMPS are shown in Fig.12 As shown, the diffraction peak shifted to the left and became sharper, indicating that AAM was successfully cross-linked with AMPS.

[0159] 4. Some surface-specific decontamination substances mentioned in previous studies were collected, as shown in Table 3. In comparison, the double-network composite hydrogel IA-PAAM / PAMPS has a highly efficient and universally applicable decontamination function, indicating that the gel has great decontamination potential in reality.

[0160] Table 3 Decontamination performance of different materials

[0161]

[0162] 5. Mechanism of removing nuclides.

[0163] Scanning electron microscopy, Fourier transform infrared spectroscopy and X-ray photoelectron spectroscopy (XPS, ThermoScientific K-Alpha, USA) were used to study the mechanism of radionuclide adsorption by the double-network composite hydrogel. Fig.13 As shown in a, IA-PAAM / PAMPS-Sr 2+ The FT-IR spectrum shows that at 1394 cm -1 The OH peak intensity at 1042 cm-1 changed significantly, while the typical peak of sulfonic acid group (S=O and SO bond) was at 1042 cm-1. -1 and 622cm -1 The red shift of OH and SO indicates that chemical adsorption has occurred; the red shift of carboxyl also indicates that COO - Also participated in Sr 2+ The results show that the hydroxyl oxygen of carboxylic acid and sulfonic acid groups is Sr 2+ The main binding site of Sr 2+ Capture of. Fig.13 b, IA-PAAM / PAMPS-UO2 2+ The FT-IR spectrum shows that IA-PAAM / PAMPS has a strong adsorption capacity on UO2 2+ After that, in the infrared spectrum at 938cm -1 A new peak appears at [O=U=O] stretching vibration; the peaks of OH and S=O are red-shifted, and COO - The red shift is accompanied by a significant change in peak intensity, indicating that the sulfonic acid group and the carboxylic acid group participate in the reaction of UO2 2+ adsorption.

[0164] The adsorption mechanism of IA-PAAM / PAMPS on nuclides was further studied by X-ray photoelectron spectroscopy (XPS). The full XPS spectra of IA-PAAM / PAMPS before and after the adsorption of nuclides are shown in Figure 2. Fig.14 and Fig.15 As shown in Figure 2, after adsorption, Sr 3d and U 4f peaks appear in the spectrum ( Fig.14 a and Fig.15 a), indicating that UO2 2+ and Sr 2+ It was successfully combined with double-net composite hydrogel. Fig.14 As shown in a, the XPS peaks of Sr3d show that the peaks at 135.60 eV and 133.86 eV after adsorption belong to divalent strontium; Fig.14 As shown in b, in the XPS high-resolution spectrum of N1s, the peak of O=NC at 401.44 eV and the peak of C-NH2 at 399.65 eV after adsorption moved toward the direction of stronger binding energy; the appearance of O=CN is the strongest evidence of acylation during the gel preparation process, and also indicates that -NH2 is involved in the adsorption reaction; Fig.14 c As shown in the XPS high-resolution spectrum of S2p, the binding energies of the sulfonic acid group SO and SC bonds are 168.72 eV and 167.69 eV, respectively. Compared with the S2p spectrum of IA-PAAM / PAMPS, the binding energies of the sulfonic acid group SO and SC bonds of IA-PAAM / PAMPS-Sr 2+ The two peaks of Sr shifted toward the direction of stronger binding energy, and there was an obvious shift at 168.72eV (+0.47eV), indicating that Sr 2+ It mainly combines with the SO oxygen atom in AMPS, such as Fig.14 d, PAAM / PAMPS-Sr 2+ This is also supported by the increase in OH binding energy in the O1S spectrum.

[0165] To explain UO2 2+ The adsorption mechanism of Fig.15 As shown, IA-PAAM / PAMPS and UO2 2+The XPS spectra before and after the reaction were analyzed. Fig.15 As shown in a, in the high-resolution spectrum of the U 4f peak, 393.33eV and 382.59eV belong to U(VI), and 391.91eV and 381.26eV belong to U(IV); the peaks of N1s, S2p and O1S were fitted, as shown in Fig.15 As shown in Figures 15b, 15c, and 15d, it was found that in the XPS high-resolution spectrum of S2p, the peaks of IA-PAAM / PAMPS at 168.72 eV and 167.69 eV belonged to SO and SC, respectively; after adsorption, the binding energy of SO decreased, while that of SC increased; this may be because the outer electrons of the O atom in the sulfonic acid group were attracted by the metal ions with stronger bond energy, resulting in weaker SO bond energy; in the XPS high-resolution spectrum of O1S, the binding energy of OH increased; in the XPS high-resolution spectrum of N1s, the binding energy of O=NC decreased significantly, which may be due to the adsorption of UO2 2+ The structure of the amide has changed.

[0166] Fig.16 The double-network composite hydrogel IA-PAAM / PAMPS can simultaneously adsorb actinides (UO2 2+ ,Th 4+ ) and fission products (Sr 2+ , Cs + ) after adsorption, the results showed that the pore channels in the hydrogel remained intact and the adsorption process did not lead to the collapse of the porous structure.

[0167] Fig.17 The double-network composite hydrogel IA-PAAM / PAMPS can simultaneously adsorb actinides (UO2 2+ ,Th 4+ ) and fission products (Sr 2+ , Cs + ) after ionization, indicating that the adsorbed nuclides are well distributed on the pore walls and in the pores of IA-PAAM / PAMPS and effectively bind to S and O, demonstrating that these porous structures can effectively capture actinides and fission products.

[0168] The present invention successfully synthesized a double-network composite hydrogel IA-PAAM / PAMPS composed of AAM, IA and AMPS, and used it for radionuclide decontamination of solutions and solid surfaces. The hydrogel swelling experiment showed that the hydrogel had good swelling performance; the adsorption experiment of nuclides confirmed that IA-PAAM / PAMPS had excellent binding ability to nuclides, and had good affinity for Sr 2+ and UO2 2+The maximum adsorption capacity of IA-PAAM / PAMPS was 267.3 mg / g and 659.0 mg / g respectively; IA-PAAM / PAMPS could maintain good adsorption capacity in different acid and alkaline environments; IA-PAAM / PAMPS was applied to the surface contaminated by radionuclides and showed good decontamination ability, and Sr was removed within 10 min. 2+ and UO2 2+ Most of the radionuclides on various solid surfaces contaminated by IA-PAAM / PAMPS have excellent universal decontamination performance for radionuclides, and can remove actinides (UO2 2+ , Th4 + ) and fission products (Sr 2+ , Cs + ) were removed simultaneously, with a removal rate of more than 90.0%; FT-IR, XPS, SEM-EDS and other analytical methods confirmed that radionuclides can specifically bind to the hydroxyl and sulfonic acid groups in IA-PAAM / PAMPS. Therefore, the double-network composite hydrogel IA-PAAM / PAMPS can be widely used as an efficient universal decontaminant for radionuclide solutions and solid nuclear contaminated surfaces.

[0169] Although the specific implementation of the present invention is described in detail in conjunction with the embodiments, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for preparing a double-network composite hydrogel, characterized in that: The following steps are involved: (1) Preparation of IA-PAAM hydrogel; S1. dissolving acrylamide in a solvent to obtain a solution with a concentration of 1 to 3 mol / L; S2. Add N,N'-methylenebisacrylamide, ammonium persulfate, iminodiacetic acid and N,N,N',N'-tetramethyleneethylenediamine to the resulting solution and stir evenly to obtain a precursor solution; the amount of N,N'-methylenebisacrylamide, ammonium persulfate, iminodiacetic acid and N,N,N',N'-tetramethyleneethylenediamine and acrylamide is 25-35 mg: 4-5 mg: 0.1-0.2 g: 40-60 μL: 10-30 mmol; S3. The precursor solution is heated at 60-80°C for 4-6 hours to obtain IA-PAAM hydrogel; (2) preparing an AMPS solution; Dissolve 2-acrylamide-2-methylpropanesulfonic acid, N,N'-methylenebisacrylamide and ammonium persulfate in a solvent and stir evenly to obtain an AMPS solution; the dosage of 2-acrylamide-2-methylpropanesulfonic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 5-15 mmol: 50-70 mg: 1-2 mg; (3) Preparation of IA-PAAM / PAMPS double-network composite hydrogel; The IA-PAAM hydrogel prepared in step (1) is immersed in the AMPS solution prepared in step (2) at room temperature for 10 to 14 hours, and then reacted at 60 to 80° C. for 4 to 6 hours to obtain the hydrogel.

2. The method for preparing the double-network composite hydrogel according to claim 1, characterized in that: The dosage of N,N'-methylenebisacrylamide, ammonium persulfate, iminodiacetic acid and N,N,N',N'-tetramethyleneethylenediamine and acrylamide is in the following relationship: 30 mg: 4.5 mg: 0.1 g: 50 μL: 20 mmol; In S3, the heating temperature is 70°C and the heating time is 5h; The dosage of 2-acrylamide-2-methylpropanesulfonic acid, N,N'-methylenebisacrylamide and ammonium persulfate is 10mmol:61.88mg:1.5mg; In step (3), the room temperature immersion time is 12 hours, the reaction temperature is 70° C., and the reaction time is 5 hours.

3. A double-network composite hydrogel prepared by the method for preparing a double-network composite hydrogel according to claim 1 or 2.

4. The double-network composite hydrogel according to claim 3 is used for removing nuclides in a solution or on a solid surface.

5. The use according to claim 4, characterized in that: The nuclide is an actinide element or a fission product.

6. The use according to claim 5, characterized in that: The actinide element is UO2 2+ or 4+ , the fission product is Sr 2+ or Cs + .

7. The use according to claim 6, characterized in that: The solid is glass, plastic or stainless steel.

8. The use according to claim 7, characterized in that: The method for removing radionuclides from solid surfaces comprises the following steps: The double-network composite hydrogel was pressurized at 0.35-1.2 g / cm 2 Apply an amount of the coating on a solid surface and keep it at 25-60°C for 10-30 minutes.

9. The use according to claim 6, characterized in that: The method for removing nuclides from a solution comprises the following steps: The pH value of the solution containing the nuclide is adjusted to 2-9, and then 0.5-2 mg / mL of freeze-dried double-network composite hydrogel is added to the pH-adjusted solution, and the solution is kept at 25-60° C. for 10-240 minutes.

10. The use according to claim 9, characterized in that: The double-network composite hydrogel is vacuum dried to obtain the freeze-dried double-network composite hydrogel, and the amount of the freeze-dried double-network composite hydrogel added to the solution is 1 mg / mL.