Self-extinguishing polyvinyl chloride composite material as well as preparation method and application thereof

By using magnesium hydroxide and potassium compounds as composite flame retardants in polyvinyl chloride composite materials, the decomposition problem of polyvinyl chloride composite materials under high temperature and light and the problem of insufficient flame retardant performance is solved, and efficient flame retardant is achieved and smoke suppression effects and reduce costs.

CN118879003AActive Publication Date: 2024-11-01JIANGXI GUANGYUAN CHEM +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411106631.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The polyvinyl chloride composite material decomposes under high temperature and light, and its flame retardant performance is insufficient, especially the limit oxygen index of magnesium hydroxide is not ideal. The traditional flame retardant combination will interfere with the smoke suppression effect, resulting in a decrease in smoke suppression ability.

Method used

Magnesium hydroxide and potassium compounds are used as composite flame retardants to generate composite flame retardants through activation reactions, and mixed with polyvinyl chloride resin, plasticizer and stabilizer to perform grafting and plasticization to form self-extinguishing polyvinyl chloride composite Material.

Benefits of technology

The flame retardant and mechanical properties of polyvinyl chloride composite materials are significantly improved, smoke suppression ability is maintained, the ultimate oxygen index, carbon residue rate and tensile strength are significantly improved, and the cost is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879003A_ABST
    Figure CN118879003A_ABST
Patent Text Reader

Abstract

The invention provides a self-extinguishing polyvinyl chloride composite material as well as a preparation method and application thereof, and belongs to the technical field of polyvinyl chloride composite material processing. The self-extinguishing polyvinyl chloride composite material is prepared from the following raw materials in parts by weight: 150-200 parts of polyvinyl chloride resin, 10-20 parts of a composite flame retardant, 20-50 parts of a plasticizer and 1-5 parts of a stabilizer, the preparation raw materials of the composite flame retardant comprise magnesium hydroxide and a potassium compound, potassium ions and magnesium hydroxide are blended, the flame retardant effect of the composite material is improved while the smoke suppression capacity of the material is guaranteed, and the self-extinguishing polyvinyl chloride composite material is obtained on the premise that safety and environmental friendliness are not sacrificed. The application value and the market competitiveness of the polyvinyl chloride composite material in the key fields of buildings, traffic, electronics and the like are greatly improved, and meanwhile the requirement for high-performance fireproof materials in the global range is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyvinyl chloride composite material processing, in particular to a self-extinguishing polyvinyl chloride composite material and a preparation method and application thereof. Background Art

[0002] Polyvinyl chloride is a thermoplastic resin and a general-purpose plastic that once ranked first in global production. Polyvinyl chloride can be found everywhere in many fields, including building materials, industrial products, daily necessities, floor coverings, floor tiles, artificial leather, pipes, wires and cables, packaging films, containers, foam materials, sealing materials, and fibers. Polyvinyl chloride products are known for their high dimensional stability, excellent surface finish, water resistance, oil resistance, and excellent corrosion resistance. However, polyvinyl chloride composites begin to decompose at temperatures of about 170°C and have poor stability to light and heat. When the temperature exceeds 100°C or is exposed to sunlight for a long time, the material will decompose to produce hydrogen chloride, which will catalyze further autodecomposition, resulting in color changes, and its physical and mechanical properties will also rapidly decline. Therefore, in practical applications, stabilizers must be added to improve the stability of polyvinyl chloride to heat and light.

[0003] In addition, phthalates need to be added to polyvinyl chloride materials to improve their mechanical properties. Although polyvinyl chloride itself has certain flame retardant properties, the addition of phthalates will significantly reduce the flame retardant properties of its composite materials. In view of the high performance requirements of the application industry for polyvinyl chloride composites, especially in terms of flame retardancy, antimony trioxide is usually added as a flame retardant. However, since antimony trioxide is expensive and may produce substances that are harmful to the environment and personal safety during the flame retardant process, the industry is seeking new flame retardants to replace antimony trioxide. Magnesium hydroxide is seen as an effective substitute, but the current challenge is that although the addition of magnesium hydroxide can significantly improve the smoke suppression performance of polyvinyl chloride composites, its limiting oxygen index is not ideal, which means that its flame retardant ability still needs to be further improved.

[0004] In view of the limitations of magnesium hydroxide in improving the flame retardant properties of polyvinyl chloride composites, the mainstream solution on the market focuses on the use of compounding technology, that is, combining magnesium hydroxide with other types of flame retardants in order to achieve a synergistic enhancement of the flame retardant properties of polyvinyl chloride composites. However, this approach introduces a new problem: although the flame retardancy of the material can be significantly improved by adding traditional flame retardants and blending with magnesium hydroxide, other components in the composite flame retardant will interfere with the smoke suppression effect of magnesium hydroxide, thereby negatively affecting the smoke suppression ability of the composite material. Summary of the invention

[0005] The object of the present invention is to provide a self-extinguishing polyvinyl chloride composite material and a preparation method and application thereof, which can improve the flame retardancy of the polyvinyl chloride composite material while maintaining its smoke suppression ability.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a self-extinguishing polyvinyl chloride composite material, comprising the following raw materials in parts by weight:

[0008] 150-200 parts of polyvinyl chloride resin, 10-20 parts of composite flame retardant, 20-50 parts of plasticizer and 1-5 parts of stabilizer;

[0009] The raw materials for preparing the composite flame retardant include magnesium hydroxide and potassium compounds.

[0010] Preferably, the plasticizer comprises phthalate.

[0011] Preferably, the stabilizer includes one or more of zinc stearate, cadmium stearate, calcium stearate, dibutyltin dilaurate, dibutyltin dimaleate and hydrotalcite calcium zinc stabilizer.

[0012] Preferably, the potassium compound includes one or more of potassium carbonate, potassium perchlorate, potassium chlorate, potassium formate, potassium nitrate, potassium sulfate and potassium hypochlorite.

[0013] Preferably, the mass ratio of the magnesium hydroxide to the potassium compound is 2:8 to 1:9.

[0014] The present invention provides a method for preparing the self-extinguishing polyvinyl chloride composite material described in the above technical solution, comprising the following steps:

[0015] The magnesium hydroxide, the potassium compound and the activator are mixed to perform an activation reaction to obtain a composite flame retardant;

[0016] The polyvinyl chloride resin, the composite flame retardant, the plasticizer and the stabilizer are mixed, grafted and plasticized, and extruded to obtain a self-extinguishing polyvinyl chloride composite material.

[0017] Preferably, the activator includes one of ethanol, methanol, propanol or ethylene glycol; the mass of the activator is 10-15% of the total mass of the magnesium hydroxide and the potassium compound.

[0018] Preferably, the activation reaction is carried out at a temperature of 80 to 130° C., a time of 10 to 120 min, and a stirring speed of 800 to 1000 r / min.

[0019] Preferably, the grafting and plasticizing temperature is 30-180° C., the time is 10-90 min, and the stirring speed is 800-1000 r / min.

[0020] The present invention provides the use of the self-extinguishing polyvinyl chloride composite material described in the above technical solution or the self-extinguishing polyvinyl chloride composite material prepared by the preparation method described in the above technical solution in fireproof materials.

[0021] Beneficial effects of the present invention:

[0022] The present invention adds a composite flame retardant to a traditional polyvinyl chloride resin, and the obtained self-extinguishing polyvinyl chloride composite material has good flame retardant properties; wherein the composite flame retardant includes magnesium hydroxide and potassium compounds, and under the catalytic action of potassium ions, the polyvinyl chloride alkane side chains are more easily rearranged and disconnected, thereby helping the polyvinyl chloride to burn quickly and completely when the surface polyvinyl chloride just contacts the flame, and will not fall into incomplete combustion products, and will generate more CO2 and water vapor, and quickly absorb surrounding heat, so that the ignition point is instantly reduced during the combustion process, and at the same time, the combustible gas and the combustion-supporting gas in the air are significantly diluted, and the combustion quenching is achieved by isolating the combustion-supporting gas to quickly reach a self-extinguishing state, thereby improving the flame retardant effect of the composite material.

[0023] The self-extinguishing polyvinyl chloride composite material prepared by the present invention has a tensile strength of ≥9.60MPa, an elongation at break ≥165%, a limiting oxygen index ≥27.8, a carbon residue rate ≥70.4%, a maximum smoke density ≤79.66%, and a smoke density grade ≤71.59. While having an excellent flame retardant effect, its smoke suppression ability is also maintained; and the potassium compound is more advantageous in price than traditional flame retardants such as antimony trioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is the TGA diagram of the pyrolysis of the residual carbon layer of the composite material condensed phase caused by the change of the composite flame retardant composition in a nitrogen atmosphere. DETAILED DESCRIPTION

[0025] The present invention provides a self-extinguishing polyvinyl chloride composite material, comprising the following raw materials in parts by weight:

[0026] 150-200 parts of polyvinyl chloride resin, 10-20 parts of composite flame retardant, 20-50 parts of plasticizer and 1-5 parts of stabilizer;

[0027] The raw materials for preparing the composite flame retardant include magnesium hydroxide and potassium compounds.

[0028] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.

[0029] In the present invention, the mass fraction of the polyvinyl chloride resin is 150 to 200 parts, and more preferably 170 to 200 parts; the present invention has no special limitation on the source of the polyvinyl chloride resin, and any commercially available product known in the art can be used; in an embodiment of the present invention, the polyvinyl chloride resin is preferably derived from Gansu Yinda Chemical Co., Ltd.

[0030] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the composite flame retardant of the present invention is preferably 10 to 20 parts, and more preferably 10 to 15 parts. The raw materials for preparing the composite flame retardant of the present invention include magnesium hydroxide and potassium compounds; in the present invention, the magnesium hydroxide is preferably ultrafine magnesium hydroxide, and the mesh number of the ultrafine magnesium hydroxide is preferably ≥2000 mesh, and more preferably 6000 mesh; the ultrafine magnesium hydroxide is preferably derived from Jiangxi Guangyuan Chemical Group, and the product number is GY-6000; the magnesium hydroxide used in the present invention is an ultra-high mesh magnesium hydroxide product produced by crushing the original ore, which has strong hydrophilicity, a large contact area with polyvinyl chloride, and a good modification effect on polyvinyl chloride.

[0031] In the present invention, the potassium compound preferably includes one or more of potassium carbonate, potassium chloride, potassium chlorate, potassium formate, potassium nitrate, potassium sulfate and potassium hypochlorite, and further preferably includes one or more of potassium chlorate, potassium formate, potassium nitrate, potassium sulfate and potassium hypochlorite; when the potassium compound is two or more of the above, the present invention has no special limitation on the ratio of different types of potassium compounds, as long as the mass ratio of magnesium hydroxide to potassium compound is 1:9; the addition of potassium ions can improve the flame retardant properties of the composite material.

[0032] In the present invention, the mass ratio of the magnesium hydroxide to the potassium compound is preferably 2:8 to 1:9, and more preferably 1:9.

[0033] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the plasticizer in the present invention is preferably 20 to 50 parts, and more preferably 30 to 50 parts; the present invention has no special limitation on the type of the plasticizer, and any plasticizer commonly used in the art can be used; in an embodiment of the present invention, the plasticizer is preferably a phthalate, and the phthalate is sourced from Shanghai McLean Biochemical Technology Co., Ltd.

[0034] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the stabilizer of the present invention is preferably 1 to 5 parts, and more preferably 2 to 5 parts; the stabilizer preferably includes one or more of zinc stearate, cadmium stearate, calcium stearate, dibutyl tin dilaurate, dibutyl tin dimaleate and hydrotalcite calcium zinc stabilizer, and more preferably includes one or more of zinc stearate, cadmium stearate, calcium stearate and hydrotalcite calcium zinc stabilizer.

[0035] The present invention provides a method for preparing the self-extinguishing polyvinyl chloride composite material described in the above technical solution, comprising the following steps:

[0036] The magnesium hydroxide, the potassium compound and the activator are mixed to perform an activation reaction to obtain a composite flame retardant;

[0037] The polyvinyl chloride resin, the composite flame retardant, the plasticizer and the stabilizer are mixed, grafted and plasticized, and extruded to obtain a self-extinguishing polyvinyl chloride composite material.

[0038] In the present invention, the activator preferably includes one of ethanol, methanol, propanol or ethylene glycol, and is more preferably ethanol; the mass of the activator is preferably 10-15% of the total mass of the magnesium hydroxide and the potassium compound, and is more preferably 10-12%; the activator can activate the surface of the potassium compound and the magnesium hydroxide, and stimulate the combination of the two.

[0039] In the present invention, the activation reaction temperature is preferably 80-130° C., more preferably 90-120° C., the time is preferably 10-120 min, more preferably 10-100 min, and the stirring speed is preferably 800-1000 r / min.

[0040] In the present invention, the temperature of the heating reaction is preferably 30 to 180° C., more preferably 60 to 180° C., the time is preferably 10 to 90 min, more preferably 10 to 55 min, and the stirring speed is preferably 800 to 1000 r / min.

[0041] The present invention provides the use of the self-extinguishing polyvinyl chloride composite material described in the above technical solution or the self-extinguishing polyvinyl chloride composite material prepared by the preparation method described in the above technical solution in fireproof materials.

[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0043] The polyvinyl chloride resin used in Examples 1 to 10 of the present invention and Comparative Examples 1 to 4 is sourced from Gansu Yinda Chemical Co., Ltd.; the mesh size of the magnesium hydroxide used is 6000 mesh, sourced from Jiangxi Guangyuan Chemical Group, and the product number is GY-6000; the phthalate used is sourced from Shanghai McLean Biochemical Technology Co., Ltd.

[0044] The potassium compounds and stabilizers used in Examples 1 to 10 of the present invention and Comparative Examples 1 to 4 are all commercially available products, and there is no specific requirement for their sources.

[0045] Example 1

[0046] 18 g of magnesium hydroxide, 2 g of potassium chlorate and 15 mL of ethanol were mixed, and an activation reaction was carried out at 120° C. for 10 min under a stirring condition of 800 rpm to obtain a composite flame retardant;

[0047] The composite flame retardant was mixed with 200 g of polyvinyl chloride resin, 30 g of phthalate and 2 g of hydrotalcite calcium zinc stabilizer, and heated to react at 170° C. for 15 min under stirring at 800 rpm to obtain the self-extinguishing polyvinyl chloride composite material of Example 1.

[0048] Example 2

[0049] The only difference from Example 1 is that

[0050] The potassium compound used was potassium formate;

[0051] The stabilizer used was zinc stearate;

[0052] The self-extinguishing polyvinyl chloride composite material of Example 2 was obtained.

[0053] Example 3

[0054] The only difference from Example 1 is that

[0055] The potassium compound used is potassium nitrate;

[0056] The stabilizer used was cadmium stearate;

[0057] The self-extinguishing polyvinyl chloride composite material of Example 3 was obtained.

[0058] Example 4

[0059] The only difference from Example 1 is that

[0060] The potassium compound used is potassium sulfate;

[0061] The stabilizer used was calcium stearate;

[0062] The self-extinguishing polyvinyl chloride composite material of Example 4 was obtained.

[0063] Example 5

[0064] The only difference from Example 1 is that

[0065] The potassium compound used is potassium hypochlorite;

[0066] The self-extinguishing polyvinyl chloride composite material of Example 5 was obtained.

[0067] Example 6

[0068] The only difference from Example 1 is that

[0069] The mass of magnesium hydroxide is 9g, the mass of potassium chlorate is 1g, the temperature of the activation reaction is 90℃, and the time is 30min;

[0070] The heating reaction temperature was 150°C and the time was 25 min;

[0071] The self-extinguishing polyvinyl chloride composite material of Example 6 was obtained.

[0072] Example 7

[0073] The only difference from Example 2 is that

[0074] The mass of magnesium hydroxide is 9g, the mass of potassium formate is 1g, the temperature of the activation reaction is 90℃, and the time is 30min;

[0075] The heating reaction temperature was 150°C and the time was 25 min;

[0076] The self-extinguishing polyvinyl chloride composite material of Example 7 was obtained.

[0077] Example 8

[0078] The only difference from Example 3 is that

[0079] The mass of magnesium hydroxide is 9g, the mass of potassium nitrate is 1g, the temperature of activation reaction is 90℃, and the time is 30min;

[0080] The heating reaction temperature was 150°C and the time was 25 min;

[0081] The self-extinguishing polyvinyl chloride composite material of Example 8 was obtained.

[0082] Example 9

[0083] The only difference from Example 4 is that

[0084] The mass of magnesium hydroxide is 9g, the mass of potassium sulfate is 1g, the temperature of the activation reaction is 90℃, and the time is 30min;

[0085] The heating reaction temperature was 150°C and the time was 25 min;

[0086] The self-extinguishing polyvinyl chloride composite material of Example 9 was obtained.

[0087] Example 10

[0088] The only difference from Example 5 is that

[0089] The mass of magnesium hydroxide is 9g, the mass of potassium hypochlorite is 1g, the temperature of the activation reaction is 90℃, and the time is 30min;

[0090] The heating reaction temperature was 150°C and the time was 25 min;

[0091] The self-extinguishing polyvinyl chloride composite material of Example 10 was obtained.

[0092] Comparative Example 1

[0093] The only difference from Example 1 is that

[0094] Without adding potassium chlorate, the mass of magnesium hydroxide is 20 g;

[0095] The self-extinguishing polyvinyl chloride composite material of Comparative Example 1 was obtained.

[0096] Comparative Example 2

[0097] The only difference from Example 1 is that

[0098] Without adding potassium chlorate, the mass of magnesium hydroxide is 10 g;

[0099] The self-extinguishing polyvinyl chloride composite material of Comparative Example 2 was obtained.

[0100] Comparative Example 3

[0101] The only difference from Example 1 is that

[0102] Without adding magnesium hydroxide, the mass of potassium chlorate is 20 g;

[0103] The self-extinguishing polyvinyl chloride composite material of Comparative Example 3 was obtained.

[0104] Comparative Example 4

[0105] The only difference from Example 1 is that

[0106] No magnesium hydroxide was added, and the mass of potassium chlorate was 10 g;

[0107] The self-extinguishing polyvinyl chloride composite material of Comparative Example 4 was obtained.

[0108] Performance Testing

[0109] The composite materials prepared in the above Examples 1 to 10 and Comparative Examples 1 to 4 were subjected to performance tests, and the test results are recorded in Table 1:

[0110] (1) Tensile strength and breaking productivity test: Tested in accordance with GB / T10400.1-2018 standard.

[0111] (2) Limiting oxygen index test: Tested in accordance with GB / T2406.2-2009 standard.

[0112] (3) Determination of residual carbon rate: Take the standard sample in (1) and weigh it before combustion. After the combustion test, weigh the remaining mass. The residual carbon rate is calculated by the ratio of the remaining mass to the initial mass.

[0113] (4) Maximum smoke density and smoke density level test: Tested in accordance with GB / T8627-2007 standard.

[0114] Table 1 Test results of composite materials obtained from Examples 1 to 10 and Comparative Examples 1 to 4

[0115]

[0116]

[0117] It can be seen from the results of Example 1 and Comparative Examples 1 and 3 that in the absence of one of the composite flame retardant components, the flame retardant properties and mechanical properties of the polyvinyl chloride composite material are significantly different, which indicates that there is an obvious coordinated flame retardant effect between magnesium hydroxide and potassium compounds, and potassium compounds need to be combined with magnesium hydroxide to show an obvious flame retardant effect, indicating that the catalytic flame retardant effect of potassium compounds is synergistic flame retardant, and magnesium hydroxide is the main flame retardant. When the composite flame retardant is added, the flame retardant properties and mechanical properties of the polyvinyl chloride composite material are significantly enhanced, and the limiting oxygen index, residual carbon rate, tensile strength and elongation at break are significantly improved.

[0118] After the smoke density level and maximum smoke density of the sample were tested, the condensed phase residual carbon layer of the sample was collected. In a nitrogen atmosphere, the mass changes of the condensed phase residual carbon layer of the self-extinguishing polyvinyl chloride composite material prepared by the composite flame retardant in Example 1, the magnesium hydroxide alone in Comparative Example 1, and the potassium compound alone in Comparative Example 3 at different temperatures were measured by a thermogravimetric analyzer, and the results were obtained. Figure 1 .from Figure 1 It can be seen that there are differences in the pyrolysis curves of the three. The pyrolysis curves of only one of them as a flame retardant are similar, and the residual carbon rate is low; while the composite material with the composite flame retardant has a higher residual carbon rate. This is because the composite flame retardant can catalyze the recombination and breakage of the high molecular alkane molecular chain during the combustion process, so that the combustion is completely produced CO2 and H2O, resulting in self-extinguishing phenomenon, maintaining a high residual carbon rate; at the same time, the two synergistically flame retardant to produce a series of physical barriers with magnesium oxide as the main body while quenching in a short time, isolating the continuous spread of combustion; potassium compounds are environmentally friendly while maintaining excellent flame retardant properties compared to traditional flame retardants such as antimony trioxide, and are more price-friendly, which can broaden the application of potassium compound catalytic flame retardant, and further obtain polyvinyl chloride composite materials with better flame retardant properties.

[0119] It can be seen from the above embodiments that the present invention provides a self-extinguishing polyvinyl chloride composite material with a tensile strength of ≥9.60MPa, an elongation at break ≥165%, a limiting oxygen index ≥27.8, a carbon residue rate ≥70.4%, a maximum smoke density ≤79.66%, and a smoke density level ≤71.59. While not affecting the smoke suppression effect, the flame retardant properties of the self-extinguishing polyvinyl chloride composite material are significantly improved, so that the self-extinguishing polyvinyl chloride composite material has high added value, and the application field of the polyvinyl chloride composite material is further expanded.

[0120] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A self-extinguishing polyvinyl chloride composite material, characterized in that: The preparation comprises the following raw materials in parts by weight: 150-200 parts of polyvinyl chloride resin, 10-20 parts of composite flame retardant, 20-50 parts of plasticizer and 1-5 parts of stabilizer; The raw materials for preparing the composite flame retardant include magnesium hydroxide and potassium compounds.

2. The self-extinguishing polyvinyl chloride composite material according to claim 1, characterized in that: The plasticizers include phthalates.

3. The self-extinguishing polyvinyl chloride composite material according to claim 1, characterized in that: The stabilizer includes one or more of zinc stearate, cadmium stearate, calcium stearate, dibutyltin dilaurate, dibutyltin dimaleate and hydrotalcite calcium zinc stabilizer.

4. The self-extinguishing polyvinyl chloride composite material according to claim 1, characterized in that: The potassium compound includes one or more of potassium carbonate, potassium perchlorate, potassium chlorate, potassium formate, potassium nitrate, potassium sulfate and potassium hypochlorite.

5. The self-extinguishing polyvinyl chloride composite material according to claim 1 or 4, characterized in that: The mass ratio of the magnesium hydroxide to the potassium compound is 2:8 to 1:

9.

6. The method for preparing the self-extinguishing polyvinyl chloride composite material according to any one of claims 1 to 5, characterized in that: The following steps are involved: The magnesium hydroxide, the potassium compound and the activator are mixed to perform an activation reaction to obtain a composite flame retardant; The polyvinyl chloride resin, the composite flame retardant, the plasticizer and the stabilizer are mixed, grafted and plasticized, and extruded to obtain a self-extinguishing polyvinyl chloride composite material.

7. The preparation method according to claim 6, characterized in that: The activator comprises one of ethanol, methanol, propanol or ethylene glycol; the mass of the activator is 10-15% of the total mass of the magnesium hydroxide and the potassium compound.

8. The preparation method according to claim 6, characterized in that: The activation reaction is carried out at a temperature of 80 to 130° C., for a time of 10 to 120 minutes, and at a stirring speed of 800 to 1000 r / min.

9. The preparation method according to claim 6, characterized in that: The grafting and plasticizing temperature is 30-180° C., the time is 10-90 min, and the stirring speed is 800-1000 r / min.

10. Use of the self-extinguishing polyvinyl chloride composite material according to any one of claims 1 to 5 or the self-extinguishing polyvinyl chloride composite material prepared by the preparation method according to any one of claims 6 to 9 in fireproof materials.

Citation Information

Patent Citations

  • Cable material as well as preparation method and application thereof

    CN114133655A

  • Modified magnesium hydroxide, preparation method and application thereof, and polyvinyl chloride composite material

    CN116496642A

  • Polyvinyl chloride resin composition, polyvinyl chloride resin composition sheet, insulated wire and cable

    JP2018184529A

  • Flame-retardant and smoke-suppressing soft polyvinyl chloride composite material having good mechanical performance and preparation method therefor

    WO2020233028A1

  • Preparation method for montmorillonite-magnesium hydroxide composite microencapsulated flame retardant

    WO2022068065A1