Self-extinguishing low-smoke polyvinyl chloride composite material as well as preparation method and application thereof
By adding magnesium hydroxide and manganese compounds to the polyvinyl chloride resin, a self-extinguishing low-smoke type polyvinyl chloride composite material is solved, and the problem of insufficient flame retardant performance and smoke suppression ability of the polyvinyl chloride composite material is achieved efficient resistance The combustion and smoke suppression effect and reduce combustion smoke and gas emissions, with a price advantage.
Patent Information
- Application Number
- CN202411111015.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The flame retardant properties and smoke suppression ability of polyvinyl chloride composites are insufficient. Traditional flame retardants such as antimony trioxide are expensive and have environmental hazards. The flame retardant components in the existing compounding scheme have a conflicting effect on magnesium hydroxide. Alkane-repressing properties of composite materials.
Magnesium hydroxide and manganese compounds are added to the polyvinyl chloride resin, and a self-extinguishing low-smoke polyvinyl chloride composite material is formed through activation reaction and graft plasticization. Manganese ions catalyzed oxidation of PVC alkanes branched into hydroxyl or carboxyl groups, and oxidation with hydroxide Magnesium forms organic bonding, producing a condensed phase residual carbon layer, enhancing flame retardant properties and smoke suppression capabilities.
The flame retardant properties and smoke suppression ability of polyvinyl chloride composite materials are significantly improved, with a maximum smoke density of ≤45.00, smoke density level ≤38.46, limit oxygen index ≥30.8, and carbon residue rate ≥60.4%, while reducing the dissipation of combustion smoke And gas emissions, the price advantage is more than that of traditional antimony trioxide.
Smart Images

Figure CN118879004A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyvinyl chloride composite material processing, in particular to a self-extinguishing low-smoke polyvinyl chloride composite material and a preparation method and application thereof. Background Art
[0002] Polyvinyl chloride (PVC) is a thermoplastic resin. It was once the world's largest general-purpose plastic. It is widely used in building materials, industrial products, daily necessities, floor coverings, floor tiles, artificial leather, pipes, wires and cables, packaging films, bottles, foaming materials, sealing materials, fibers, etc. PVC products have high dimensional stability, good surface finish, water resistance, oil resistance, and excellent corrosion resistance. However, PVC composite materials have poor light and heat stability. They will decompose to produce hydrogen chloride above 100°C or after long-term exposure to sunlight, and further autocatalytic decomposition, causing discoloration and rapid decline in physical and mechanical properties. In practical applications, stabilizers must be added to improve the stability to heat and light, and plasticizers will also be added to improve the mechanical properties. The addition of plasticizers will significantly deteriorate the flame retardant properties of PVC composite materials. In order to improve its flame retardant properties, antimony trioxide is generally added as a flame retardant. However, due to the high price of antimony trioxide and the easy production of a large number of products that endanger the environment and personal safety, the industry is currently seeking new flame retardants to replace antimony trioxide. Magnesium hydroxide is considered to be an effective flame retardant to replace antimony trioxide. However, after magnesium hydroxide is added to PVC composite materials, although there is a significant improvement in smoke suppression, the limiting oxygen index is not high and the flame retardant ability needs to be improved.
[0003] Based on this situation, the solution that has emerged on the market is mainly to compound magnesium hydroxide, hoping to improve the flame retardant properties of composite materials by introducing other flame retardant ingredients to compound magnesium hydroxide. The problem encountered is that although the composite flame retardant formed by introducing traditional flame retardants and compounding magnesium hydroxide can significantly improve the flame retardant properties of composite materials, the traditional flame retardant ingredients conflict with magnesium hydroxide in terms of smoke suppression, which will seriously affect the smoke suppression ability of the composite material. Summary of the invention
[0004] The object of the present invention is to provide a self-extinguishing low-smoke polyvinyl chloride composite material and a preparation method and application thereof, so as to simultaneously improve the flame retardant performance and smoke suppression ability of the composite material.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a self-extinguishing low-smoke polyvinyl chloride composite material, comprising the following raw materials in parts by weight:
[0007] 150-200 parts of polyvinyl chloride resin, 30-50 parts of magnesium hydroxide, 5-10 parts of manganese compound, 30-50 parts of plasticizer and 1-5 parts of stabilizer.
[0008] Preferably, the manganese compound includes one or more of manganese monoxide, manganese dioxide, manganese trioxide, manganese hydroxide, manganese sulfate, manganese chloride and manganese nitrate.
[0009] Preferably, the plasticizer comprises phthalate.
[0010] Preferably, the stabilizer includes one or more of zinc stearate, cadmium stearate, calcium stearate, dibutyltin dilaurate, dibutyltin dimaleate and hydrotalcite calcium zinc stabilizer.
[0011] The present invention provides a method for preparing the self-extinguishing low-smoke polyvinyl chloride composite material described in the above technical solution, comprising the following steps:
[0012] Mixing magnesium hydroxide, a manganese compound and an activator to perform an activation reaction to obtain an activated product;
[0013] The activated product, polyvinyl chloride resin, plasticizer and stabilizer are mixed and grafted and plasticized to obtain a self-extinguishing low-smoke polyvinyl chloride composite material.
[0014] Preferably, the activator comprises one of ethanol, methanol, propanol or ethylene glycol; the mass of the activator is 10-15% of the total mass of the magnesium hydroxide and the manganese compound.
[0015] Preferably, the activation reaction is carried out at a temperature of 70 to 130° C. and for a time of 10 to 120 min.
[0016] Preferably, the temperature of the grafting and plasticizing is 30 to 180° C., and the time is 10 to 90 minutes.
[0017] The present invention also provides the use of the self-extinguishing low-smoke polyvinyl chloride composite material described in the above technical solution or the self-extinguishing low-smoke polyvinyl chloride composite material prepared by the preparation method described in the above technical solution in fireproof materials.
[0018] Beneficial effects of the present invention:
[0019] The invention improves the flame retardant property and smoke suppression ability of the polyvinyl chloride composite material by adding manganese compound and magnesium hydroxide to the traditional PVC resin; wherein the manganese ion can catalyze the oxidation of PVC alkane side chains to form oxidized functional groups such as hydroxyl or carboxyl, and form organic bonds with the hydroxyl groups on the magnesium hydroxide; meanwhile, the magnesium oxide generated by the thermal decomposition of the magnesium hydroxide itself also has a certain physical adsorption effect; the two synergistically promote the combustion part of the PVC to be firmly combined on the surface of the unburned PVC composite material in the form of a condensed phase residual carbon layer, forming a stable carbon layer, inhibiting further combustion of the flame by isolating the combustibles, greatly reducing the dissipation of solid particles of part of the combustion smoke in the air, and improving the smoke suppression ability of the composite material; meanwhile, the significant increase in the mass of the condensed phase residual carbon layer can also form an effective physical barrier, greatly improving the flame retardant property of the composite material to a certain extent.
[0020] The self-extinguishing low-smoke polyvinyl chloride composite material prepared by the present invention has excellent smoke suppression ability and flame retardant performance, with a maximum smoke density of ≤45.00, a smoke density grade of ≤38.46, a limiting oxygen index of ≥30.8, and a carbon residue rate of ≥60.4%; at the same time, the manganese compound has a greater price advantage than traditional flame retardants such as antimony trioxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a TGA graph of the pyrolysis of the condensed phase residual carbon layer of the self-extinguishing low-smoke polyvinyl chloride composite material in Example 1 and Comparative Example 1 and Comparative Example 2 in an air atmosphere;
[0022] Figure 2 This is a SEM image of the condensed phase residual carbon layer of the self-extinguishing low-smoke polyvinyl chloride composite material of Comparative Example 1;
[0023] Figure 3 This is a SEM image of the condensed phase residual carbon layer of the self-extinguishing low-smoke polyvinyl chloride composite material of Comparative Example 2;
[0024] Figure 4 This is a SEM image of the condensed phase residual carbon layer of the self-extinguishing low-smoke polyvinyl chloride composite material of Example 1;
[0025] Figure 5 It is a schematic diagram showing the difference between the flame retardant modes of the self-extinguishing low-smoke polyvinyl chloride composite material of the present invention and conventional polyvinyl chloride materials. DETAILED DESCRIPTION
[0026] The present invention provides a self-extinguishing low-smoke polyvinyl chloride composite material, comprising the following raw materials in parts by weight:
[0027] 150-200 parts of polyvinyl chloride resin, 30-50 parts of magnesium hydroxide, 5-10 parts of manganese compound, 30-50 parts of plasticizer and 1-5 parts of stabilizer.
[0028] In the present invention, unless otherwise specified, the required raw materials for preparation are all commercially available products well known to those skilled in the art.
[0029] In the present invention, the mass fraction of the polyvinyl chloride resin is preferably 150 to 200 parts, more preferably 160 to 200 parts, and more preferably 170 to 200 parts; the present invention has no special limitation on the source of the polyvinyl chloride resin, and any commercially available product known in the art can be used; in an embodiment of the present invention, the polyvinyl chloride resin is preferably derived from the products of Gansu Yinda Chemical Co., Ltd.
[0030] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the magnesium hydroxide of the present invention is preferably 30 to 50 parts, more preferably 30 to 45 parts, and more preferably 30 to 42 parts; the magnesium hydroxide of the present invention is preferably ultrafine magnesium hydroxide, and the mesh number of the ultrafine magnesium hydroxide is preferably ≥2000 mesh, and more preferably 6000 mesh; the ultrafine magnesium hydroxide is preferably derived from Jiangxi Guangyuan Chemical Group, and the product number is GY-6000; the magnesium hydroxide of the present invention is an ultra-high mesh magnesium hydroxide product produced by crushing the original ore, has strong hydrophilicity, a large contact area with polyvinyl chloride, and a good modification effect on polyvinyl chloride.
[0031] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the manganese compound of the present invention is preferably 5 to 10 parts, and more preferably 5 to 8 parts; the manganese compound preferably includes one or more of manganese monoxide, manganese dioxide, manganese trioxide, manganese hydroxide, manganese sulfate, manganese chloride and manganese nitrate, and more preferably includes one or more of manganese monoxide, manganese dioxide, manganese trioxide, manganese sulfate, manganese chloride and manganese nitrate; manganese ions can catalyze the oxidation of PVC alkane side chains to form oxidized functional groups such as hydroxyl or carboxyl. When the alkane molecular chain is catalytically oxidized, the obtained combustion product can quickly combine with magnesium hydroxide to drive the aggregation of the surrounding PVC composite materials. The rapid aggregation of a large number of PVC composite materials will cause the oxygen required for combustion to be "scarce" in a short time, thereby achieving a quenching effect and realizing self-extinguishing flame retardancy.
[0032] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the plasticizer is preferably 30 to 50 parts, and more preferably 30 to 40 parts; the present invention has no special limitation on the type of the plasticizer, and any plasticizer commonly used in the art can be used; in an embodiment of the present invention, the plasticizer is preferably a phthalate, and the phthalate is sourced from Shanghai McLean Biochemical Technology Co., Ltd.
[0033] Based on the mass fraction of the polyvinyl chloride resin, the mass fraction of the stabilizer is preferably 1 to 5 parts, and more preferably 2 to 5 parts; the stabilizer preferably includes one or more of zinc stearate, cadmium stearate, calcium stearate, dibutyl tin dilaurate, dibutyl tin dimaleate and hydrotalcite calcium zinc stabilizer, and more preferably includes one or more of zinc stearate, cadmium stearate, calcium stearate and hydrotalcite calcium zinc stabilizer.
[0034] The present invention provides a method for preparing the self-extinguishing low-smoke polyvinyl chloride composite material described in the above technical solution, comprising the following steps:
[0035] Mixing magnesium hydroxide, a manganese compound and an activator to perform an activation reaction to obtain an activated product;
[0036] The activated product, polyvinyl chloride resin, plasticizer and stabilizer are mixed and grafted and plasticized to obtain a self-extinguishing low-smoke polyvinyl chloride composite material.
[0037] In the present invention, the activator preferably includes one of ethanol, methanol, propanol or ethylene glycol; the mass of the activator is preferably 10-15% of the total mass of the magnesium hydroxide and the manganese compound, and more preferably 10-12%.
[0038] In the present invention, the activation reaction temperature is preferably 70-130°C, more preferably 80-120°C, more preferably 90-120°C; the activation reaction time is preferably 10-120 min, more preferably 10-110 min, more preferably 10-100 min.
[0039] In the present invention, the temperature of the grafting and plasticization is preferably 30 to 180° C., more preferably 40 to 180° C., and more preferably 60 to 180° C.; the time is preferably 10 to 90 min, more preferably 10 to 75 min, and more preferably 10 to 55 min.
[0040] In the present invention, the activation reaction and the graft polymerization reaction are preferably carried out under stirring conditions, and the stirring speed is independently preferably 400 to 1200 rpm, more preferably 500 to 1100 rpm, and even more preferably 600 to 1000 rpm.
[0041] The present invention also provides the use of the self-extinguishing low-smoke polyvinyl chloride composite material described in the above technical solution or the self-extinguishing low-smoke polyvinyl chloride composite material prepared by the preparation method described in the above technical solution in fireproof materials.
[0042] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0043] The polyvinyl chloride resin used in Examples 1 to 15 of the present invention and Comparative Examples 1 to 2 is sourced from Gansu Yinda Chemical Co., Ltd.; the mesh size of the magnesium hydroxide used is 6000 mesh, sourced from Jiangxi Guangyuan Chemical Group, and the product number is GY-6000; the phthalate used is sourced from Shanghai McLean Biochemical Technology Co., Ltd.
[0044] The manganese compounds and stabilizers used in Examples 1 to 15 of the present invention and Comparative Examples 1 to 2 are all commercially available products, and there is no specific requirement for their sources.
[0045] Example 1
[0046] 50 g of magnesium hydroxide, 5 g of manganese dioxide and 15 mL of ethanol were mixed, and an activation reaction was carried out at 120° C. for 10 min under stirring conditions of 800 rpm to obtain an activated product;
[0047] The activated product was mixed with 200 g of PVC resin, 30 g of phthalate and 2 g of hydrotalcite calcium zinc stabilizer, and heated to react at 170° C. for 15 min under stirring at 800 rpm to obtain the self-extinguishing low-smoke polyvinyl chloride composite material of Example 1.
[0048] Example 2
[0049] The only difference from Example 1 is:
[0050] The manganese compound used is manganese monoxide;
[0051] The stabilizer used was zinc stearate;
[0052] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 2 was obtained.
[0053] Example 3
[0054] The only difference from Example 1 is:
[0055] The manganese compound used is manganese trioxide;
[0056] The stabilizer used was cadmium stearate;
[0057] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 3 was obtained.
[0058] Example 4
[0059] The only difference from Example 1 is:
[0060] The manganese compound used is manganese nitrate;
[0061] The stabilizer used was calcium stearate;
[0062] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 4 was obtained.
[0063] Example 5
[0064] The only difference from Example 1 is:
[0065] The manganese compound used was manganese chloride;
[0066] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 5 was obtained.
[0067] Example 6
[0068] The only difference from Example 1 is:
[0069] The activation reaction temperature was 90°C and the time was 30 min;
[0070] The temperature of graft polymerization reaction was 150°C and the time was 25 min;
[0071] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 6 was obtained.
[0072] Example 7
[0073] The only difference from Example 2 is that:
[0074] The activation reaction temperature was 90°C and the time was 30 min;
[0075] The temperature of graft polymerization reaction was 150°C and the time was 25 min;
[0076] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 7 was obtained.
[0077] Example 8
[0078] The only difference from Example 3 is that:
[0079] The activation reaction temperature was 90°C and the time was 30 min;
[0080] The temperature of graft polymerization reaction was 150°C and the time was 25 min;
[0081] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 8 was obtained.
[0082] Example 9
[0083] The only difference from Example 4 is that:
[0084] The activation reaction temperature was 90°C and the time was 30 min;
[0085] The temperature of graft polymerization reaction was 150°C and the time was 25 min;
[0086] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 9 was obtained.
[0087] Example 10
[0088] The only difference from Example 5 is:
[0089] The activation reaction temperature was 90°C and the time was 30 min;
[0090] The temperature of graft polymerization reaction was 150°C and the time was 25 min;
[0091] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 10 was obtained.
[0092] Embodiment 11
[0093] The only difference from Example 1 is:
[0094] The activation reaction time was 30 min;
[0095] The graft polymerization reaction time was 25 min;
[0096] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 11 was obtained.
[0097] Example 12
[0098] The only difference from Example 2 is that:
[0099] The activation reaction time was 30 min;
[0100] The graft polymerization reaction time was 25 min;
[0101] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 12 was obtained.
[0102] Embodiment 13
[0103] The only difference from Example 3 is that:
[0104] The activation reaction time was 30 min;
[0105] The graft polymerization reaction time was 25 min;
[0106] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 13 was obtained.
[0107] Embodiment 14
[0108] The only difference from Example 4 is that:
[0109] The activation reaction time was 30 min;
[0110] The graft polymerization reaction time was 25 min;
[0111] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 14 was obtained.
[0112] Embodiment 15
[0113] The only difference from Example 5 is:
[0114] The activation reaction time was 30 min;
[0115] The graft polymerization reaction time was 25 min;
[0116] The self-extinguishing low-smoke polyvinyl chloride composite material of Example 15 was obtained.
[0117] Comparative Example 1
[0118] The only difference from Example 1 is:
[0119] No manganese dioxide was added;
[0120] The self-extinguishing low-smoke polyvinyl chloride composite material of Comparative Example 1 was obtained.
[0121] Comparative Example 2
[0122] The only difference from Example 1 is:
[0123] No magnesium hydroxide was added;
[0124] The self-extinguishing low-smoke polyvinyl chloride composite material of Comparative Example 2 was obtained.
[0125] Performance Testing
[0126] The composite materials prepared in the above Examples 1 to 15 and Comparative Examples 1 to 2 were subjected to performance tests, and the test results are recorded in Table 1:
[0127] (1) Maximum smoke density and smoke density level test: Tested in accordance with GB / T8627-2007 standard;
[0128] (2) Limiting oxygen index test: Tested in accordance with GB / T2406.2-2009 standard;
[0129] (3) Determination of residual carbon rate: Take the standard sample in (1) and weigh it before combustion. After the combustion test, weigh the remaining mass. The residual carbon rate is calculated by the ratio of the remaining mass to the initial mass.
[0130] Table 1 Test results of composite materials obtained in Examples 1 to 15 and Comparative Examples 1 to 2
[0131]
[0132]
[0133] From the results of Example 1, Comparative Example 1 and Comparative Example 2, it can be seen that in the absence of either magnesium hydroxide or manganese compound, the flame retardant properties and smoke suppression capabilities of the PVC composite material are significantly different, indicating that there is an obvious coordinated flame retardant effect between magnesium hydroxide and manganese compounds, and the manganese compound needs to be combined with magnesium hydroxide to show an obvious flame retardant effect, indicating that the catalytic flame retardant effect of the manganese compound is synergistic flame retardant, and magnesium hydroxide is the main flame retardant. When magnesium hydroxide and manganese compounds are added, the flame retardant properties and smoke suppression capabilities of the PVC composite material are significantly enhanced, and the limiting oxygen index, maximum smoke density and smoke density level are significantly improved.
[0134] After the smoke density level and maximum smoke density of the sample were tested, the condensed phase residual carbon layer of the sample was collected. In an air atmosphere, the mass changes of the condensed phase residual carbon layer of the self-extinguishing low-smoke polyvinyl chloride composite material prepared by magnesium hydroxide and manganese compound in Example 1, magnesium hydroxide only in Comparative Example 1, and manganese compound only in Comparative Example 2 at different temperatures were measured by a thermogravimetric analyzer, and the results were obtained. Figure 1 .from Figure 1 It can be seen that there are differences in the pyrolysis curves of the three. The pyrolysis curves of only adding one of them as a flame retardant are similar, and the decomposition temperature is low, and the condensed phase residual carbon layer is not stable enough. On the contrary, the pyrolysis temperature of the condensed phase residual carbon layer of the composite material with magnesium hydroxide and manganese compounds added is significantly increased, indicating that its condensed phase residual carbon layer is more stable.
[0135] The condensed phase residual carbon layer of the self-extinguishing low-smoke polyvinyl chloride composite material of Comparative Examples 1 to 2 and Example 1 was observed by scanning electron microscope, and the Figures 2 to 4 .from Figure 2 , Figure 3 and Figure 4It can be seen that the surface of the PVC composite material with only magnesium hydroxide added is relatively dense, but the physical adsorption capacity of magnesium oxide generated by its decomposition is limited, and the condensed phase residual carbon layer of the composite material is still not stable and strong enough; while the condensed phase residual carbon layer of the PVC composite material with only manganese compounds added can obviously see that the condensed phase residual carbon layer is tighter, and the difference can also be clearly observed from the residual carbon rate. This is due to the catalytic flame retardant effect of manganese ions, which can concentrate the surrounding PVC alkane molecular chains in a large range in a short period of time, making oxygen "scarce" phenomenon instantaneously, achieving the quenching effect, but this also causes the secondary combustion to be more intense, so its limiting oxygen index is low. However, when magnesium hydroxide and manganese compounds are added at the same time, the condensed phase residual carbon layer of the PVC composite material is firm and dense, and magnesium hydroxide and manganese compounds synergistically flame retardant each other, quenching in a short time, and forming a series of physical barriers with magnesium oxide as the main body to prevent the continuous spread of combustion. Compared with traditional flame retardants such as antimony trioxide, manganese compounds are environmentally friendly and more price-friendly while maintaining excellent flame retardant properties and smoke suppression capabilities. It can broaden the application of manganese compound catalytic flame retardant, and further obtain PVC composite materials with better flame retardant properties and smoke suppression capabilities.
[0136] The difference between the flame retardant mode of the self-extinguishing low-smoke polyvinyl chloride composite material of the present invention and the conventional polyvinyl chloride material is further explained. Figure 5 As shown, conventional polyvinyl chloride materials contain magnesium hydroxide flame retardants and additives, which will release CO2, CO and HCl during the combustion process. Only adding magnesium hydroxide flame retardants cannot effectively curb the spread of combustion; while the composite material of the present invention uses magnesium hydroxide and manganese compounds as flame retardants. During the combustion process, the polyvinyl chloride in the combustion area is firmly covered on the surface of the unburned material in the form of a condensed phase residual carbon layer, forming a solid protective barrier, which greatly reduces the escape of some solid particles of combustion smoke in the air, inhibits further combustion of the flame by isolating combustibles, significantly slows down the spread of the fire, and greatly reduces gas emissions during combustion, thereby improving the flame retardancy and smoke suppression properties of the composite material to a certain extent.
[0137] It can be seen from the above Examples 1 to 15 and Comparative Examples 1 to 2 that the self-extinguishing low-smoke polyvinyl chloride composite material prepared by the present invention has a maximum smoke density of ≤45.00, a smoke density grade of ≤38.46, a limiting oxygen index of ≥30.8, and a carbon residue rate of ≥60.4%, which makes it have high added value and further expands the application field of the polyvinyl chloride composite material.
[0138] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A self-extinguishing low-smoke polyvinyl chloride composite material, characterized in that: The preparation comprises the following raw materials in parts by weight: 150-200 parts of polyvinyl chloride resin, 30-50 parts of magnesium hydroxide, 5-10 parts of manganese compound, 30-50 parts of plasticizer and 1-5 parts of stabilizer.
2. The self-extinguishing low-smoke polyvinyl chloride composite material according to claim 1, characterized in that: The manganese compound includes one or more of manganese monoxide, manganese dioxide, manganese trioxide, manganese hydroxide, manganese sulfate, manganese chloride and manganese nitrate.
3. The self-extinguishing low-smoke polyvinyl chloride composite material according to claim 1, characterized in that: The plasticizers include phthalates.
4. The self-extinguishing low-smoke polyvinyl chloride composite material according to claim 1, characterized in that: The stabilizer includes one or more of zinc stearate, cadmium stearate, calcium stearate, dibutyltin dilaurate, dibutyltin dimaleate and hydrotalcite calcium zinc stabilizer.
5. The method for preparing the self-extinguishing low-smoke polyvinyl chloride composite material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Mixing magnesium hydroxide, a manganese compound and an activator to perform an activation reaction to obtain an activated product; The activated product, polyvinyl chloride resin, plasticizer and stabilizer are mixed and grafted and plasticized to obtain a self-extinguishing low-smoke polyvinyl chloride composite material.
6. The preparation method according to claim 5, characterized in that: The activator comprises one of ethanol, methanol, propanol or ethylene glycol; the mass of the activator is 10-15% of the total mass of the magnesium hydroxide and the manganese compound.
7. The preparation method according to claim 5, characterized in that: The activation reaction is carried out at a temperature of 70 to 130° C. and for a time of 10 to 120 minutes.
8. The preparation method according to claim 5, characterized in that: The temperature of the grafting and plasticizing is 30 to 180° C., and the time is 10 to 90 minutes.
9. Use of the self-extinguishing low-smoke polyvinyl chloride composite material according to any one of claims 1 to 4 or the self-extinguishing low-smoke polyvinyl chloride composite material prepared by the preparation method according to any one of claims 5 to 8 in fireproof materials.
Citation Information
Patent Citations
Method for preparing serpentine-magnesium hydroxide-manganese borate composite flame retardant
CN109608692A
ABS resin material and preparation method thereof
CN110105703A
Efficient flame-retardant ecological floor and preparation method thereof
CN113388212A
Composite flame-retardant smoke-suppression type polyvinyl chloride membrane material
CN114685912A
Degradable flame retardant and preparation method thereof
CN117603566A