Anti-yellowing oxidation PVC (polyvinyl chloride) film and preparation method thereof
By using modified talc powder and almond shell powder, combined with appropriate formulation and processing technology, the yellowing problem of PVC film under photothermal effects was solved, and the yellowing resistance and tensile strength were improved.
Patent Information
- Application Number
- CN202411201091.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-29
AI Technical Summary
PVC film is susceptible to yellowing due to light and heat during use, and current technology has not been able to completely solve this problem.
Modified talc and almond shell powder are used as the main components. Through reasonable formulation design and processing technology, the surface of modified talc is coated with an organic coupling agent, and almond shell powder contains phenolic substances that provide antioxidant effects. Combined with appropriate plasticizers and antioxidants, the yellowing resistance of PVC film is improved.
It effectively slows down the yellowing process of PVC film, maintains excellent physical properties, and improves the yellowing resistance and tensile strength of PVC film.
Smart Images

Figure BDA0005017860960000061 
Figure BDA0005017860960000071
Abstract
Description
Technical Field
[0001] The invention relates to the field of PVC films, in particular to a yellowing oxidation-resistant PVC film and a preparation method thereof. Background Art
[0002] PVC (polyvinyl chloride) is a widely used plastic material, which is widely used in various industries due to its low price, durability and easy processing.
[0003] However, PVC film is easily affected by light and heat during use, causing yellowing and oxidation, which seriously affects the appearance and quality of the product. In order to solve this problem, industry insiders have made many attempts, but the existing technology has not been able to completely solve the yellowing problem of PVC. Summary of the invention
[0004] In order to improve the yellowing resistance of PVC film, the present application provides a yellowing-resistant oxidation PVC film and a preparation method thereof.
[0005] In the first aspect, the present application provides a yellowing oxidation-resistant PVC film adopting the following technical solution: A yellowing oxidation-resistant PVC film comprises the following raw materials in parts by weight: 60-90 parts of PVC; 20-60 parts of a plasticizer; 2-8 parts of calcium stearate; 10-30 parts of modified talcum powder; 1-3 parts of an antioxidant; and 5-15 parts of almond shell powder. The modified talcum powder is prepared by modifying the following raw materials: talcum powder, ethanol, 3-mercaptopropyltrimethoxysilane, cupric chloride and polypropylene.
[0006] By adopting the above technical scheme, PVC is used as the main component of the film, and the modified talc has better dispersibility and compatibility, thereby reducing the yellowing caused by filler aggregation. Almond shell powder, as a natural filler, has a certain antioxidant effect due to the phenolic substances it contains, which helps to improve the yellowing resistance of the PVC film. The comprehensive effect of each component can improve the yellowing resistance of the PVC film. Through reasonable formula design and processing technology, it is possible to slow down the yellowing process while maintaining the excellent physical properties of the PVC film.
[0007] Preferably, the preparation method of the modified talc powder is: 10-20 parts by weight of talc powder and 50-150 parts by weight of ethanol are mixed and stirred, 5-15 parts by weight of 3-mercaptopropyltrimethoxysilane, 1-5 parts by weight of cupric chloride and 5-10 parts by weight of polypropylene are added and mixed and stirred after ultrasonic treatment, and then filtered, washed and dried to obtain the modified talc powder.
[0008] By adopting the above technical scheme, the present application modifies talcum powder; the surface of 3-mercaptopropyltrimethoxysilane has a hydrophilic group and a hydrophobic group, which reacts with the surface of talcum powder to coat the surface of talcum powder with a layer of organic coupling agent; cupric chloride chelates with the mercapto group and hydroxyl functional groups of 3-mercaptopropyltrimethoxysilane to form a stable complex, thereby improving the stability and yellowing resistance of the PVC film.
[0009] Preferably, the weight ratio of talc, 3-mercaptopropyltrimethoxysilane, cupric chloride and polypropylene is (1.6-1.8):1:(0.15-0.23):(0.6-0.7).
[0010] By adopting the above technical scheme, talcum powder, 3-mercaptopropyltrimethoxysilane, cupric chloride and polypropylene are combined together, and 3-mercaptopropyltrimethoxysilane can be grafted on PVC to improve the compatibility of PVC and polypropylene, thereby further improving the tensile strength of the PVC film.
[0011] Preferably, the almond shell powder is modified almond shell powder, and the preparation method of the modified almond shell powder is: 3-9 parts by weight of sodium alginate is mixed with 10-30 parts by weight of water, and then 10-20 parts by weight of almond shell powder and 5-10 parts by weight of polyethylene glycol are added, mixed, ultrasonically dispersed, filtered, dried and then ground to obtain the modified almond shell powder.
[0012] By adopting the above technical scheme, sodium alginate is used as a stabilizer to reduce the thermal degradation of PVC during processing and use. Almond shell powder contains phenolic substances and has a certain antioxidant effect, which helps to delay the yellowing of PVC. Almond shell powder and sodium alginate are blended and then mixed with polyethylene glycol to improve the mechanical strength of almond shell powder, thereby improving the mechanical strength of PVC filled with almond shell powder as a filler.
[0013] Preferably, the weight ratio of the almond shell powder, polyethylene glycol and sodium alginate is (2.4-3.2):(1.2-1.4):1.
[0014] By adopting the above technical scheme, when almond shell powder, polyethylene glycol and sodium alginate are in a specific weight ratio, a large number of hydroxyl groups and carboxyl groups exist in the molecular weight of ammonium alginate, which forms a hydrogel with polyethylene glycol and covers the almond shell powder. The almond shell powder is evenly dispersed in PVC, which helps to reduce the yellowing phenomenon caused by heat or light in PVC, and at the same time, the PVC has excellent tensile strength.
[0015] Preferably, the degree of polymerization of the PVC is 1000-1100.
[0016] By adopting the above technical solution and selecting a suitable degree of polymerization, the tensile strength and yellowing resistance of PVC can be effectively improved.
[0017] Preferably, the weight ratio of the modified talc powder, PVC and modified almond shell powder is 1:(3.8-4.2):(0.55-0.65).
[0018] By adopting the above technical scheme, the modified talcum powder improves the dispersibility and compatibility in PVC after surface treatment, and further improves the tensile strength of PVC, while the modified almond shell powder can further improve the thermal stability of PVC, thereby helping to reduce the yellowing phenomenon caused by filler aggregation; the combined use of modified talcum powder and modified almond shell powder can enhance the tensile strength of PVC while improving the yellowing resistance of PVC.
[0019] The plasticizer is one of dioctyl phthalate and diisooctyl phthalate.
[0020] Preferably, the antioxidant is one of antioxidant 168 and antioxidant 1010.
[0021] By adopting the above technical solution and selecting suitable plasticizers and antioxidants, the yellowing resistance of the PVC film can be effectively improved.
[0022] In the second aspect, the present application provides a method for preparing a yellowing-resistant PVC film using the following technical solution: A method for preparing a yellowing-resistant PVC film comprises the following steps: mixing PVC, a plasticizer, calcium stearate, modified talcum powder, an antioxidant and almond shell powder, continuing to stir after cooling, calendering and drying to obtain the yellowing-resistant oxidation PVC film.
[0023] By adopting the above technical scheme, the raw materials for preparing the PVC film are processed in steps, so that various raw materials are mixed more evenly, thereby obtaining a yellowing-resistant PVC film.
[0024] In summary, this application has the following beneficial technical effects: 1. PVC is the main component of the film, and the modified talc has better dispersibility and compatibility, thereby reducing the yellowing caused by filler aggregation. Almond shell powder, as a natural filler, has a certain antioxidant effect due to the phenolic substances it contains, which helps to improve the yellowing resistance of PVC film. The comprehensive effect of each component can improve the yellowing resistance of PVC film. Through reasonable formula design and processing technology, it is possible to slow down the yellowing process while maintaining the excellent physical properties of PVC film.
[0025] 2. The present application modifies talcum powder. The surface of 3-mercaptopropyltrimethoxysilane has hydrophilic groups and hydrophobic groups, which react with the surface of talcum powder to coat the surface of talcum powder with a layer of organic coupling agent; cupric chloride chelates with the mercapto and hydroxyl functional groups of 3-mercaptopropyltrimethoxysilane to form a stable complex, thereby improving the stability and yellowing resistance of the PVC film. DETAILED DESCRIPTION
[0026] The present application is further described in detail below in conjunction with embodiments and comparative examples. Example
[0027] Example 1 A method for preparing a yellowing resistant oxidation PVC film comprises the following steps: 60g PVC, 20g plasticizer, 2g calcium stearate, 10g modified talc, 1g antioxidant and 5g almond shell powder are put into a stirrer and mixed and stirred for 30min at a temperature of 80°C and a rotation speed of 800r / min, and then stirred for 10min after cooling to 60°C, and then rolled by a calender and dried for 2h at a temperature of 100°C to obtain a yellowing resistant oxidation PVC film. The polymerization degree of PVC is 1000, the brand is SG-5, and it is purchased from Sichuan Jinlu Resin Co., Ltd. The antioxidant is antioxidant 1010, and the plasticizer is dioctyl phthalate.
[0028] The preparation method of the modified talc powder is as follows: 10g of talc powder and 50g of 95% ethanol are mixed and stirred for 2 minutes, and then 5g of 3-mercaptopropyltrimethoxysilane, 1g of copper chloride and 5g of polypropylene are added and mixed and stirred for 10 minutes after ultrasonic treatment in an ultrasonic cleaner, and then filtered, washed with anhydrous ethanol and dried in an oven at a temperature of 55°C for 2 hours to obtain the modified talc powder. The polypropylene is selected from SABIC, and the grade is 8511E.
[0029] Example 2 A method for preparing a yellowing resistant oxidation PVC film comprises the following steps: 90g PVC, 60g plasticizer, 8g calcium stearate, 30g modified talc, 3g antioxidant and 15g almond shell powder are put into a stirrer and mixed and stirred for 30min at a temperature of 80°C and a rotation speed of 800r / min, and then stirred for 10min after cooling to 60°C, and then rolled by a calender and dried for 2h at a temperature of 100°C to obtain a yellowing resistant oxidation PVC film. The polymerization degree of PVC is 1000, the brand is SG-5, and it is purchased from Sichuan Jinlu Resin Co., Ltd. The antioxidant is antioxidant 168, and the plasticizer is diisooctyl phthalate.
[0030] The preparation method of the modified talc powder is as follows: 10g of talc powder and 50g of 95% ethanol are mixed and stirred for 2 minutes, and then 5g of 3-mercaptopropyltrimethoxysilane, 1g of copper chloride and 5g of polypropylene are added and mixed and stirred for 10 minutes after ultrasonic treatment in an ultrasonic cleaner, and then filtered, washed with anhydrous ethanol and dried in an oven at a temperature of 55°C for 2 hours to obtain the modified talc powder. The polypropylene is selected from SABIC, and the grade is 8511E.
[0031] Example 3 A method for preparing a yellowing resistant oxidation PVC film comprises the following steps: 75g PVC, 40g plasticizer, 5g calcium stearate, 20g modified talc, 2g antioxidant and 10g almond shell powder are put into a stirrer, mixed and stirred for 30min at a temperature of 80°C and a rotation speed of 800r / min, and stirred for 10min after cooling to 60°C, and rolled by a calender, and dried for 2h at a temperature of 100°C to obtain a yellowing resistant oxidation PVC film. The polymerization degree of PVC is 1000, the brand is SG-5, and it is purchased from Sichuan Jinlu Resin Co., Ltd. The antioxidant is antioxidant 1010, and the plasticizer is dioctyl phthalate.
[0032] The preparation method of the modified talc powder is as follows: 10g of talc powder and 50g of 95% ethanol are mixed and stirred for 2 minutes, and then 5g of 3-mercaptopropyltrimethoxysilane, 1g of copper chloride and 5g of polypropylene are added and mixed and stirred for 10 minutes after ultrasonic treatment in an ultrasonic cleaner, and then filtered, washed with anhydrous ethanol and dried in an oven at a temperature of 55°C for 2 hours to obtain the modified talc powder. The polypropylene is selected from SABIC, and the grade is 8511E.
[0033] Example 4 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 3 in that: the preparation method of modified talcum powder is as follows: 20g of talcum powder and 150g of 95% ethanol are mixed and stirred for 2 minutes, ultrasonically treated in an ultrasonic cleaner for 15 minutes, and then 15g of 3-mercaptopropyltrimethoxysilane, 5g of copper chloride and 10g of polypropylene are added and mixed and stirred for 10 minutes, and then filtered, washed with anhydrous ethanol, and dried in an oven at a temperature of 55°C for 2 hours to obtain modified talcum powder. The polypropylene is selected from SABIC, and the grade is 8511E.
[0034] Example 5 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 3 in that, in the process of preparing modified talcum powder, the input amount of talcum powder is 16g, the input amount of 3-mercaptopropyltrimethoxysilane is 10g, the input amount of cupric chloride is 1.5g, and the input amount of polypropylene is 6g.
[0035] Example 6 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 3 in that, in the process of preparing modified talcum powder, the input amount of talcum powder is 18g, the input amount of 3-mercaptopropyltrimethoxysilane is 10g, the input amount of cupric chloride is 2.3g, and the input amount of polypropylene is 7g.
[0036] Example 7 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 6 in that an equal amount of almond shell powder is replaced with modified almond shell powder, wherein the preparation method of the modified almond shell powder is as follows: 3g of sodium alginate and 10g of water are mixed and stirred for 2min, and then 10g of almond shell powder and 5g of polyethylene glycol are added and mixed and stirred for 10min, and then ultrasonically dispersed in an ultrasonic cleaner for 30min, filtered and transferred to an oven, dried at 70°C for 2h, and then ground to obtain modified almond shell powder. The polyethylene glycol is Saudi PEG400, with a brand of CY-040.
[0037] Example 8 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 6 in that an equal amount of almond shell powder is replaced with modified almond shell powder, wherein the preparation method of the modified almond shell powder is as follows: 9g of sodium alginate and 30g of water are mixed and stirred for 2min, and then 20g of almond shell powder and 10g of polyethylene glycol are added and mixed and stirred for 10min, and then ultrasonically dispersed in an ultrasonic cleaner for 30min, filtered and transferred to an oven, dried at 70°C for 2h, and then ground to obtain modified almond shell powder. The polyethylene glycol is Saudi PEG400, with a brand name of CY-040.
[0038] Example 9 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 8 in that: in the process of preparing the modified almond shell powder, the input amount of almond shell powder is 12g, the input amount of polyethylene glycol is 6g, and the input amount of sodium alginate is 5g.
[0039] Example 10 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 8 in that: in the process of preparing the modified almond shell powder, the input amount of almond shell powder is 16g, the input amount of polyethylene glycol is 7g, and the input amount of sodium alginate is 5g.
[0040] Embodiment 11 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 10 in that the input amount of modified talcum powder is 20 g, the input amount of PVC is 76 g, and the input amount of modified almond shell powder is 11 g.
[0041] Example 12 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 10 in that the input amount of modified talcum powder is 20 g, the input amount of PVC is 84 g, and the input amount of modified almond shell powder is 13 g.
[0042] Comparative Example Comparative Example 1 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 3 in that an equal amount of modified talcum powder is replaced with talcum powder.
[0043] Comparative Example 2 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 3 in that an equal amount of modified talc is replaced with titanium dioxide.
[0044] Comparative Example 3 A method for preparing a yellowing-resistant oxidation PVC film, which is different from Example 3 in that an equal amount of almond shell powder is replaced with titanium dioxide.
[0045] Comparative Example 4 A method for preparing a yellowing-resistant oxidation PVC film, which is different from that of Example 3 in that an equal amount of almond shell powder is replaced with coconut shell powder.
[0046] Performance testing: Yellowing resistance test: Aging was performed using 420nm ultraviolet rays in a hot air oven with high temperature and high humidity. The corresponding test samples were taken out of the oven after 250 hours, cooled to room temperature and packaged in aluminum lined bags for testing. The yellowness index of the samples was obtained by testing Examples 1-12 and Comparative Examples 1-4.
[0047] Tensile strength: The mechanical properties of the PVC films prepared in Examples 1-12 and Comparative Examples 1-4 were tested according to GB / T 1040.3-2006, and the tensile strength of the aged PVC films was also tested.
[0048] According to the data comparison of Examples 1-3 and Comparative Examples 1-4, it can be obtained that PVC is the main component of the film, and the modified talc has better dispersibility and compatibility, thereby reducing the yellowing caused by filler aggregation. Almond shell powder, as a natural filler, has a certain antioxidant effect due to the phenolic substances it contains, which helps to improve the yellowing resistance of the PVC film. The comprehensive effect of each component can improve the yellowing resistance of the PVC film. Through reasonable formula design and processing technology, it is possible to achieve the yellowing process while maintaining the excellent physical properties of the PVC film.
[0049] According to the data comparison of Examples 3-6, it can be obtained that talcum powder, 3-mercaptopropyltrimethoxysilane, cupric chloride and polypropylene are combined together, and 3-mercaptopropyltrimethoxysilane can be grafted on PVC to improve the compatibility of PVC and polypropylene, thereby further improving the tensile strength of the PVC film.
[0050] According to the data comparison of Examples 6-8, sodium alginate, as a stabilizer, reduces the thermal degradation of PVC during processing and use. Almond shell powder contains phenolic substances, which has a certain antioxidant effect and helps to delay the yellowing of PVC. The mechanical strength of almond shell powder is improved by blending almond shell powder and sodium alginate and then mixing with polyethylene glycol, thereby improving the mechanical strength of PVC filled with almond shell powder as a filler.
[0051] According to the data comparison of Examples 8-10, when almond shell powder, polyethylene glycol and sodium alginate are in a specific weight ratio, there are a large number of hydroxyl groups and carboxyl groups in the molecular weight of ammonium alginate, which forms a hydrogel with polyethylene glycol and covers the almond shell powder. The almond shell powder is evenly dispersed in PVC, which helps to reduce the yellowing phenomenon caused by heat or light in PVC, and at the same time, the PVC has excellent tensile strength.
[0052] According to the data comparison of Examples 10-12, the modified talcum powder improves the dispersibility and compatibility in PVC after surface treatment, further improving the tensile strength of PVC, and the modified almond shell powder can further improve the thermal stability of PVC, thereby helping to reduce the yellowing phenomenon caused by filler aggregation; the combined use of modified talcum powder and modified almond shell powder can improve the yellowing resistance of PVC while enhancing its tensile strength.
[0053] The specific embodiments are merely explanations of the present application and are not limitations of the present application. After reading this specification, those skilled in the art may make modifications to the embodiments without any creative contribution as needed. However, as long as they are within the scope of the claims of the present application, they are protected by the patent law.
Claims
1. A yellowing oxidation resistant PVC film, characterized in that: The composition comprises the following raw materials in parts by weight: 60-90 parts of PVC; Plasticizer 20-60 parts; 2-8 parts of calcium stearate; 10-30 parts of modified talc; 1-3 parts of antioxidant; 5-15 parts of almond shell powder; the modified talc is prepared by modifying the following raw materials: talc, ethanol, 3-mercaptopropyltrimethoxysilane, cupric chloride and polypropylene.
2. The yellowing-resistant oxidation PVC film according to claim 1, characterized in that: The preparation method of the modified talcum powder comprises: mixing 10-20 parts by weight of talcum powder and 50-150 parts by weight of ethanol, adding 5-15 parts by weight of 3-mercaptopropyltrimethoxysilane, 1-5 parts by weight of cupric chloride and 5-10 parts by weight of polypropylene after ultrasonic treatment, mixing and stirring, filtering, washing and drying to obtain the modified talcum powder.
3. The yellowing-resistant oxidation PVC film according to claim 2, characterized in that: The weight ratio of the talc powder, 3-mercaptopropyltrimethoxysilane, cupric chloride and polypropylene is (1.6-1.8):1:(0.15-0.23):(0.6-0.7).
4. The yellowing-resistant oxidation PVC film according to claim 1, characterized in that: The almond shell powder is modified almond shell powder. The preparation method of the modified almond shell powder is: 3-9 weight parts of sodium alginate and 10-30 weight parts of water are mixed, and then 10-20 weight parts of almond shell powder and 5-10 weight parts of polyethylene glycol are added, mixed, ultrasonically dispersed, filtered, dried and then ground to obtain the modified almond shell powder.
5. The yellowing-resistant oxidation PVC film according to claim 4, characterized in that: The weight ratio of the almond shell powder, polyethylene glycol and sodium alginate is (2.4-3.2): (1.2-1.4):
1.
6. The yellowing-resistant oxidation PVC film according to claim 1, characterized in that: The polymerization degree of the PVC is 1000-1100.
7. The yellowing-resistant oxidation PVC film according to claim 4, characterized in that: The weight ratio of the modified talcum powder, PVC and modified almond shell powder is 1: (3.8-4.2): (0.55-0.65).
8. The yellowing-resistant oxidation PVC film according to claim 1, characterized in that: The plasticizer is one of dioctyl phthalate and diisooctyl phthalate.
9. The yellowing-resistant oxidation PVC film according to claim 1, characterized in that: The antioxidant is A method for preparing a yellowing-resistant oxidation PVC film, characterized in that: The method for preparing a yellowing-resistant oxidation PVC film according to any one of claims 1 to 9 comprises the following steps: mixing PVC, plasticizer, calcium stearate, modified talcum powder, antioxidant and almond shell powder, continuing to stir after cooling, calendering and drying to obtain the yellowing-resistant oxidation PVC film.
Citation Information
Patent Citations
Yellowing-resistant wool powder and preparation method thereof
CN115521610A
Yellowing-resistant antioxidant PVC (polyvinyl chloride) film
CN116790076A
Roofing membrane with PVC cap and core
US20230139071A1