PET (Polyethylene Terephthalate) composite material as well as preparation method and application thereof

By modifying PET with modified copper powder, PET composite materials with improved impact resistance and friction reduction and wear resistance were prepared, which solved the problem of insufficient performance of polyethylene terephthalate in tribological applications, and achieved Higher notch-free impact strength and lower friction coefficient.

CN118879040APending Publication Date: 2024-11-01WUHAN RES INST OF MATERIALS PROTECTION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410980891.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The application of polyethylene terephthalate in the field of tribology is limited by poor impact resistance and limited friction and wear resistance, resulting in limited use in friction pair materials.

Method used

The PET composite material obtained by modifying PET by modifying modified copper powder is improved by mechanical blending, intensive refining and injection molding using a combination of polyethylene terephthalate and modified copper powder. The material's notch-free impact strength and friction-reducing wear resistance.

Benefits of technology

While improving impact resistance, the friction coefficient and wear rate of PET composite materials are reduced, the lubricating layer formation and molecular chain flexibility during the friction process are enhanced, and the friction stability and impact resistance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879040A_ABST
    Figure CN118879040A_ABST
Patent Text Reader

Abstract

The invention discloses a PET (polyethylene terephthalate) composite material as well as a preparation method and application thereof, and relates to the field of antifriction and wear-resistant materials, and the PET composite material is prepared from the following components in parts by weight: 89-91 parts of polyethylene glycol terephthalate; and 9-11 parts of modified copper powder. According to the PET composite material prepared by modifying the PET through the modified copper powder, the friction coefficient and the wear rate of the PET composite material can be reduced, and meanwhile, the unnotched impact strength of the PET composite material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of friction-reducing and wear-resistant materials, and in particular to a PET composite material and a preparation method and application thereof. Background Art

[0002] About 30% of human primary energy is consumed due to friction, and about 60% of mechanical parts fail due to various types of wear. How to effectively control and reduce the energy consumed by friction and wear is of great significance to the development of the country's green economy. Polymer materials have high elasticity, low density, high toughness, corrosion resistance, excellent self-lubrication and machining properties. As friction pair materials, they can effectively extend the service life of mechanical equipment and reduce energy consumption and economic losses.

[0003] At present, polyethylene terephthalate (PET) is a milky white, highly solidified and crystalline polymer with a highly symmetrical structure, extremely high rigidity and hardness, excellent wear resistance and dimensional stability. At the same time, as a thermoplastic engineering plastic with a linear structure, it has good self-lubrication, chemical inertness and good mechanical properties, and is therefore often used as a friction pair component.

[0004] However, the application of polyethylene terephthalate in the field of tribology is limited due to its poor impact resistance and limited friction and wear resistance. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned related technologies, the present application provides a PET composite material and a preparation method and application thereof. The present application modifies PET by modified copper powder to obtain a PET composite material, which can reduce the friction coefficient and wear rate of the PET composite material while improving the unnotched impact strength of the PET composite material.

[0006] In the first aspect, the present application provides a PET composite material adopting the following technical solution: A PET composite material is prepared from the following components in parts by weight: 89-91 parts of polyethylene terephthalate and 9-11 parts of modified copper powder.

[0007] Preferably, it is prepared from the following components in parts by weight: 90 parts of polyethylene terephthalate; 10 parts of modified copper powder Preferably, the modified copper powder is obtained by modifying copper powder with a silane coupling agent.

[0008] Preferably, the modified copper powder is prepared by the following steps: copper powder, water, silane coupling agent and ethanol are mixed and dispersed, reacted at 20-30° C. for 2-3 hours, centrifuged, washed and dried to obtain the modified copper powder.

[0009] Preferably, the modified copper powder is prepared by the following steps: mixing and dispersing copper powder, water, a silane coupling agent and ethanol, reacting at 25° C. for 2.5 hours, centrifuging, washing and drying to obtain the modified copper powder.

[0010] Preferably, the weight ratio of the copper powder to the silane coupling agent is 10:1-3.

[0011] Preferably, the weight ratio of the copper powder to the silane coupling agent is 5:1.

[0012] Preferably, the silane coupling agent is KH-560 silane coupling agent Preferably, the copper powder has a particle size of 1-15 μm.

[0013] In the second aspect, the present application provides a method for preparing a PET composite material using the following technical solution: A preparation method of a PET composite material comprises the following steps: mechanically blending modified copper powder and polyethylene terephthalate powder to obtain blended powder, internally kneading the blended powder and then crushing it to obtain mixed particles, and injection molding the mixed particles to obtain the PET composite material.

[0014] Preferably, the mechanical blending comprises: ball milling for 1-2 hours.

[0015] Preferably, the mechanical blending comprises: ball milling for 1.5 hours.

[0016] Preferably, the parameters of the banburying are: melting temperature 250-270° C., rotor frequency 15-25 Hz, and banburying time 7-9 min.

[0017] Preferably, the banburying parameters are: melting temperature 260° C., rotor frequency 20 Hz, and banburying time 8 min.

[0018] Preferably, the injection molding parameters are: injection temperature 270-290°C, injection pressure 55-65MPa, injection time 28-32s, cooling time 9-11s, and mold temperature 75-85°C.

[0019] Preferably, the injection molding parameters are: injection temperature 280°C, injection pressure 60MPa, injection time 30s, cooling time 10s, and mold temperature 80°C.

[0020] In the third aspect, the application of a PET composite material provided by the present application adopts the following technical solution: An application of a PET composite material, wherein the PET composite material is used for making a friction element.

[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. Polyethylene terephthalate is modified by modified copper powder to obtain a polyethylene terephthalate composite material. On the one hand, the friction coefficient of polyethylene terephthalate is reduced, and on the other hand, the unnotched impact strength of polyethylene terephthalate is improved. Therefore, the anti-friction and wear-resistant properties are improved while the impact resistance is improved; 2. By adjusting the content of modified copper powder, during the friction process of polyethylene terephthalate composite material, copper powder will accumulate on the wear surface to form a lubricating layer, and the friction coefficient of the friction surface is reduced through the effect of interlayer sliding. A lower or higher content of copper powder is not conducive to the formation of a surface lubricating layer, and at the same time will aggravate the plastic deformation of PET, thereby increasing the friction coefficient; 3. By adjusting the content of modified copper powder, the molecular interaction between the polyethylene terephthalate macromolecular chains is reduced, the chain activity is enhanced, the flexibility of the molecular chain is increased, and more elastic deformation can occur when impacted, thereby enhancing the unnotched impact strength. When the content of modified copper powder increases to a certain extent, its dispersion uniformity will be reduced, agglomeration will occur, and the movement of polyethylene terephthalate macromolecular chain segments will be hindered. When the content of modified copper powder is low, it is less dispersed and unevenly distributed in polyethylene terephthalate, and it is less connected to the polyethylene terephthalate molecular chain, resulting in a lower unnotched impact strength; 4. By adjusting the content of modified copper powder, the compatibility of each component in the polyethylene terephthalate composite material is improved, thereby improving the stability of the friction coefficient of the polyethylene terephthalate composite material during continuous friction. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a scanning electron microscope image of the copper powder used in this application.

[0023] Figure 2 It is a comparison chart of the friction coefficient curves of the PET composite materials provided in Examples 1-3 and Comparative Examples 1-5 of the present application. DETAILED DESCRIPTION

[0024] The present application is further described in detail below in conjunction with examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention.

[0025] The raw materials used in the examples and comparative examples can all be obtained commercially.

[0026] Preparation Example The present invention provides a modified copper powder, which is prepared by the following steps: Copper powder is put into a three-necked flask, deionized water is added and the copper powder is dispersed by ultrasonic and mechanical stirring; KH-560 silane coupling agent dispersed in anhydrous ethanol is added into the three-necked flask, the weight ratio of KH-560 silane coupling agent to copper powder is 1:5, ultrasonic and mechanical stirring are performed at 25°C for 2.5 hours to obtain a mixed solution, the mixed solution is allowed to stand, and then centrifuged and washed with anhydrous ethanol to obtain a solid product, and the solid product is vacuum dried at 70°C for 11 hours to obtain modified copper powder.

[0027] Example 1 Example 1 of the present application provides a PET composite material, which is prepared by the following steps: weighing polyethylene terephthalate powder and modified copper powder with a weight ratio of 91:9, placing them in a planetary ball mill for mechanical grinding and blending for 1.5 hours, and then drying them at 70°C for 3 hours to obtain a blended powder. Then the blended powder is placed in a mixer and melt-mixed and crushed under the parameters of a melting temperature of 260°C, a rotor frequency of 20Hz, and a mixing time of 8min to obtain mixed particles. Finally, the mixed particles are molded by an injection molding machine under the parameters of an injection molding temperature of 280°C, an injection pressure of 60MPa, an injection molding time of 30s, a cooling time of 10s, and a mold heating and insulation of 80°C during injection molding, and the PET composite material is obtained after demolding at room temperature and natural cooling.

[0028] Example 2 Example 2 of the present application provides a PET composite material. The difference between Example 2 and Example 1 is that the weight ratio of polyethylene terephthalate powder and modified copper powder weighed during the preparation process of the PET composite material of Example 2 is 90:10.

[0029] Example 3 Example 3 of the present application provides a PET composite material. The difference between Example 3 and Example 1 is that the weight ratio of polyethylene terephthalate powder and modified copper powder weighed during the preparation process of the PET composite material of Example 3 is 89:11.

[0030] Comparative Example 1 Comparative Example 1 provides a PET composite material. The difference between Comparative Example 1 and Example 2 is that no modified copper powder is added to the PET composite material of Comparative Example 1 during the preparation process.

[0031] Comparative Example 2 Comparative Example 2 provides a PET composite material. The difference between Comparative Example 2 and Example 2 is that the weight ratio of the polyethylene terephthalate powder and the modified copper powder weighed during the preparation of the PET composite material of Comparative Example 2 is 95:5.

[0032] Comparative Example 3 Comparative Example 3 provides a PET composite material. The difference between Comparative Example 3 and Example 2 is that the weight ratio of the polyethylene terephthalate powder and the modified copper powder weighed during the preparation process of the PET composite material of Comparative Example 3 is 85:15.

[0033] Comparative Example 4 Comparative Example 4 provides a PET composite material. The difference between Comparative Example 4 and Example 2 is that the weight ratio of the polyethylene terephthalate powder and the modified copper powder weighed during the preparation process of the PET composite material of Comparative Example 4 is 92:8.

[0034] Comparative Example 5 Comparative Example 5 provides a PET composite material. The difference between Comparative Example 5 and Example 2 is that the weight ratio of the polyethylene terephthalate powder and the modified copper powder weighed during the preparation of the PET composite material of Comparative Example 5 is 88:12.

[0035] Test and Inspection (1) Scanning electron microscope imaging of copper powder, the results are as follows Figure 1 As shown, the copper powder particle size is 1-15 μm.

[0036] (2) The PET composite materials provided in Examples 1-3 and Comparative Examples 1-5 were subjected to unnotched impact strength tests on an Izod impact tester according to ISO 180:2000. The sample size was 80×10×4 mm. The test results are shown in Table 1 below.

[0037] (3) The PET composite materials provided in Examples 1-3 and Comparative Examples 1-5 were subjected to tribological tests under dry friction conditions on an Rtec friction and wear tester. The mating member of the kinematic pair was a φ6.35 mm ball made of GCr15 bearing steel, the working load was 20 N, the linear speed was 80 mm / s, and the working time was 30 min. The comparison of the friction coefficient curves of the PET composite materials obtained in Examples 1-3 and Comparative Examples 1-5 is shown in FIG. Figure 2 As shown, the average friction coefficient and wear rate are shown in Table 1 below.

[0038] Table 1:

[0039] Results Analysis The following combination Figure 1The experimental data provided in Table 1 are used to explain this application in detail.

[0040] Referring to Comparative Example 1, according to Examples 1-3 and Figure 2 It can be seen that the unnotched impact strength of the PET composite materials provided by Examples 1-3 is higher than the unnotched impact strength of Comparative Example 1 without adding copper powder, and the average friction coefficient and wear rate of the PET composite materials provided by Examples 1-3 are lower than the average friction coefficient and wear rate of Comparative Example 1 without adding copper powder. It shows that the addition of modified copper powder is beneficial to improving the friction reduction and wear resistance of the PET composite material while improving the impact resistance of the PET composite material. In particular, in Example 2, when the weight ratio of modified copper powder to polyethylene terephthalate is 1:9, the unnotched impact strength of the PET composite material is increased by 20.44% compared with the unnotched impact strength of the sample without adding modified copper powder, and the average friction coefficient is reduced by 31.11%, and the wear rate is reduced by 28.79%. The reason for the analysis is that: on the one hand, the addition of appropriate content of micron-sized copper powder particles can serve as the center of stress concentration, induce silver streaks and shear bands in the polyethylene terephthalate matrix, and inhibit the silver streaks from developing into cracks. The toughening of polyethylene terephthalate improves the unnotched impact strength of the PET composite material, and is also beneficial for the copper powder to accumulate on the wear surface of the friction part of the PET composite material during the friction process to form a lubricating layer to reduce the friction coefficient; on the other hand, the addition of copper powder is beneficial to the dispersion and loss of heat in the friction part of the PET composite material during the friction process, reducing the negative impact on the unnotched impact strength and friction coefficient of the PET composite material caused by the plastic deformation of polyethylene terephthalate. Under the combined effect, the friction reduction and wear resistance of the PET composite material are improved while the impact resistance of the PET composite material is improved.

[0041] Referring to Examples 1-3 and Comparative Examples 4-5, it can be seen that the content of modified copper powder in the PET composite material increases in the order of Comparative Example 4, Example 1, Example 2, Example 3, and Comparative Example 5. As the content of modified copper powder increases, the average friction coefficient of the PET composite material shows a trend of first decreasing and then increasing. When the weight ratio of modified copper powder to polyethylene terephthalate is 1:9, the average friction coefficient of the PET composite material reaches the lowest. Analysis shows that the copper powder modified by the coupling agent will be connected with the molecular chain of polyethylene terephthalate, which improves the adhesion of the two materials and the strength of the composite material. During the friction process, the copper powder will accumulate on the wear surface to form a lubricating layer, and the friction coefficient of the friction surface is reduced by the effect of its interlayer sliding. The copper powder with a lower or higher content is not conducive to the formation of the surface lubricating layer, and at the same time, it will aggravate the plastic deformation of polyethylene terephthalate, thereby increasing the friction coefficient.

[0042] Especially in Comparative Examples 2 and 3, when the content of modified copper powder is too low or too high, the friction coefficient curve shows a sharp fluctuation over time. Analysis shows that it is caused by uneven distribution or agglomeration of copper powder. At this time, the compatibility of each component in the PET composite material dominates the impact resistance and friction reduction and wear resistance of the PET composite material. It shows that adjusting the content of modified copper powder to a suitable range is conducive to improving the stability of the friction coefficient of the PET composite material during continuous friction.

[0043] With reference to Examples 1-3 and Comparative Examples 4-5, it can be seen that the content of modified copper powder in the PET composite material increases in the order of Comparative Example 4, Example 1, Example 2, Example 3, and Comparative Example 5. As the content of modified copper powder increases, the unnotched impact strength of the PET composite material increases first and then decreases. When the weight ratio of modified copper powder to polyethylene terephthalate is 1:9, the unnotched impact strength of the PET composite material reaches the highest. The analysis is that the copper powder treated with a coupling agent reduces the molecular force between the polyethylene terephthalate macromolecular chains, enhances the activity of the chains, increases the flexibility of the molecular chains, and can undergo more elastic deformation when impacted, which increases the unnotched impact strength. When the content of modified copper powder increases to a certain extent, the uniformity of its dispersion will be reduced, agglomeration will occur, and the movement of the polyethylene terephthalate macromolecular chain segments will be hindered, resulting in a lower unnotched impact strength. When the content of modified copper powder is low, the dispersion in polyethylene terephthalate is less and the distribution is uneven, and there are fewer connections with the polyethylene terephthalate molecular chain, resulting in lower unnotched impact strength.

[0044] In summary, with comparative example 1 as a control, the unnotched impact strength of the PET composite materials provided by comparative examples 2-5 all decreased, indicating that in general, adding modified copper powder to the polyethylene terephthalate matrix will cause the unnotched impact strength of the prepared PET composite materials to decrease. However, it was unexpectedly found that the unnotched impact strength of the PET composite materials provided by Examples 1-3 was restored to be equivalent to or even slightly improved to the unnotched impact strength of pure polyethylene terephthalate, wherein the unnotched impact strength improvement rate of the PET composite material provided by Example 2 reached 20.44%. In combination with the average friction coefficient of the PET composite materials provided by Examples 1-3, it was reduced by 11.85-31.11%, and the wear rate was reduced by 9.09-28.79%, indicating that when the weight fraction of the modified copper powder was 9-11%, the average friction coefficient and wear rate of the PET composite materials were reduced while the unnotched impact strength of the PET composite materials was also improved, achieving the effect of improving the multiple performances of the friction reduction, wear resistance and impact resistance of the PET composite materials.

[0045] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A PET composite material, characterized in that: The invention is prepared from the following components in parts by weight: 89-91 parts of polyethylene terephthalate and 9-11 parts of modified copper powder.

2. A PET composite material according to claim 1, characterized in that: The modified copper powder is obtained by modifying copper powder with a silane coupling agent.

3. A PET composite material according to claim 2, characterized in that: The modified copper powder is prepared by the following steps: copper powder, water, silane coupling agent and ethanol are mixed and dispersed, reacted at 20-30° C. for 2-3 hours, centrifuged, washed and dried to obtain the modified copper powder.

4. A PET composite material according to claim 3, characterized in that: The weight ratio of the copper powder to the silane coupling agent is 10:1-3.

5. A PET composite material according to claim 2, characterized in that: The copper powder has a particle size of 1-15 μm.

6. A method for preparing the PET composite material according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mechanically blending modified copper powder and polyethylene terephthalate powder to obtain blended powder, internally kneading the blended powder and then crushing it to obtain mixed particles, and injection molding the mixed particles to obtain the PET composite material.

7. The method for preparing a PET composite material according to claim 6, characterized in that: The mechanical blending includes: ball milling for 1-2 hours.

8. The method for preparing a PET composite material according to claim 6, characterized in that: The parameters of the banburying are: melting temperature 250-270° C., rotor frequency 15-25 Hz, and banburying time 7-9 min.

9. The method for preparing a PET composite material according to claim 6, characterized in that: The injection molding parameters are: injection temperature 270-290°C, injection pressure 55-65MPa, injection time 28-32s, cooling time 9-11s, and mold temperature 75-85°C.

10. An application of the PET composite material according to any one of claims 1 to 5, characterized in that: The PET composite material is used for making friction elements.