Anti-counterfeiting material for inducing RTP through boron-nitrogen coordination bond effect and preparation method of anti-counterfeiting material

Through the method of induction of boron and nitrogen coordination bonds, the problems of environmental pollution and non-recyclable in existing anti-counterfeiting materials are solved, and recyclable room temperature phosphorescent materials are realized, with long afterglow emission and dual afterglow adjustment functions, showing Excellent anti-counterfeiting performance and sustainability.

CN118879061APending Publication Date: 2024-11-01SOUTHWEST UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410771920.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-15
Publication Date
2024-11-01

Smart Images

  • Figure CN118879061A_ABST
    Figure CN118879061A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of an anti-counterfeiting material for inducing RTP through boron-nitrogen coordination bond action. The preparation method comprises the following steps: S1, synthesizing boron-nitrogen coordination micromolecules (NCBW-X); s2, a waterproof polyurethane elastomer (PCL-IPDI-ADH-NCBW-X) containing a boron and nitrogen coordination bond is synthesized; s3, adding a bactericide with the mass fraction of 0.1-1% and an antioxidant with the mass fraction of 0.1-1% into the waterproof polyurethane elastomer prepared in the step S2 to obtain the anti-counterfeiting material for inducing RTP through the boron-nitrogen coordination bond action, the anti-counterfeiting material prepared by the method has the characteristics of EX-De (excitation dependence), can generate different colors of afterglow at room temperature through excitation of different wavelengths to achieve the anti-counterfeiting effect, is a recyclable and reusable anti-counterfeiting material, and has good potential in the aspect of anti-counterfeiting packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of anti-counterfeiting packaging elastomers in new materials, and relates to a non-covalent bond dynamic reversible system material formed by coordination bonds and a preparation method thereof, and in particular to an anti-counterfeiting material inducing RTP by boron-nitrogen coordination bonds and a preparation method thereof. Background Art

[0002] Room temperature phosphorescent (RTP) materials can produce long-life luminescence after light excitation, and have broad application prospects in the fields of anti-counterfeiting, smart sensing, data encryption, etc., so they have attracted widespread attention. However, the difficulty is that most RTP small molecules may have a specific electronic configuration in the free state, which enables them to emit light after absorbing light energy. When these molecules are embedded or chemically grafted onto polyurethane chains, their electronic environment may change, thereby affecting their ability to emit light. Compared with traditional heavy element small molecule phosphorescent systems, RTP polymers have the advantages of light weight, low toxicity, good flexibility, and easy processing, and have attracted widespread attention in recent years. RTP is a radiative transition from molecular triplet excitons at room temperature, and its lifetime is usually on the order of microseconds or even longer. Most reported RTP luminophores contain heavy atoms, otherwise the efficiency of these spin-forbidden transitions is very low. In this case, non-radiative decay caused by molecular motion and intermolecular collisions becomes dominant. Therefore, organic molecules lacking heavy atoms hardly emit phosphorescence at room temperature. Metals, such as platinum (Pt) and iridium (Ir), can effectively enhance spin-orbit coupling, thereby improving the intersystem crossing (ISC) and triplet radiative emission rates. However, the development of high-performance pure RTP emitting materials remains a major challenge because of the large energy gap (ΔEST) between the lowest singlet (S1) and lowest triplet (T1) excited states and the weak spin-orbit coupling between the singlet and triplet states in these RTP materials.

[0003] To date, the most popular design paradigms for organic RTPs mainly follow two strategies: 1) improving ISC by, for example, introducing carbonyls and / or halogens into the molecule; 2) suppressing triplet non-radiative processes by, for example, crystallization, supramolecular assembly, or matrix hardening. It is worth noting that most RTP emitters usually obey the Kasha rule, where phosphorescence comes from T1, but multiple phosphorescence can be observed in a single molecule, which violates the Kasha rule and is rarely reported.

[0004] The study found that polyurethane materials without BN coordination bonds do not have the RTP effect, but the addition of BN coordination bonds causes the material to exhibit room temperature phosphorescence.

[0005] Therefore, it is necessary to design a new method to synergistically construct RTP anti-counterfeiting materials by dynamic borate esters and BN coordination bonds to solve the environmental pollution problem of existing anti-counterfeiting materials requiring heavy atoms to produce RTP effect and the problem that the lack of dynamics makes them non-recyclable and non-recyclable. Summary of the invention

[0006] In view of this, in order to solve the environmental pollution problem of the existing anti-counterfeiting materials requiring heavy atoms to produce the RTP effect and the problem that the lack of dynamics makes them non-recyclable and non-recyclable, the present invention provides an anti-counterfeiting material that induces RTP through boron-nitrogen coordination bonds and a preparation method thereof. The anti-counterfeiting material prepared by this method has the characteristics of EX-De (excitation dependence), and can produce afterglow of different colors through excitation of different wavelengths at room temperature to achieve the anti-counterfeiting effect. It is a recyclable and reusable anti-counterfeiting material, and has good potential in anti-counterfeiting packaging.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] A method for preparing an anti-counterfeiting material inducing RTP by boron-nitrogen coordination bonding, comprising the following steps:

[0009] S1. Synthesis of boron-nitrogen coordination small molecules: dissolving and reacting 1,4-phenylenediboronic acid and triolamine compounds at room temperature through a solution reaction to form a boron-nitrogen coordination small molecule (NCBW-X);

[0010] S2, synthesizing a waterproof polyurethane elastomer: reacting polycaprolactone and isophorone diisocyanate in a dry solvent, using a catalyst dibutyltin dilaurate, reacting at 80° C. to form a capped prepolymer, adding adipic acid dihydrazide (ADH) to the obtained prepolymer, controlling the reaction temperature to 40-70° C. and the reaction time to 1-4 hours, further adding (NCBW-X) prepared in step S1, controlling the reaction temperature to 80° C. and the reaction time to 4-10 hours, to obtain a waterproof polyurethane elastomer containing boron-nitrogen coordination bonds (PCL-IPDI-ADH-NCBW-X);

[0011] During the preparation of isocyanate-terminated prepolymers, the control of temperature and time is crucial to the mechanical properties and self-healing characteristics of the final material; adjusting the temperature to 40°C can ensure that ADH will not agglomerate due to high temperature, and further increasing the temperature allows NCBW-X to fully react and the unreacted isocyanate groups to be completely consumed to form the expected polyurethane network structure.

[0012] S3. Add 0.1-1% by mass of a bactericide and 0.1-1% by mass of an antioxidant to the waterproof polyurethane elastomer prepared in step S2, stir evenly to make the bactericide and antioxidant fully dispersed in the prepolymer, pour into a mold after the polymerization reaction is completed, dry and solidify at 70°C to obtain an anti-counterfeiting material with RTP induced by boron-nitrogen coordination bonds.

[0013] The anti-counterfeiting polyurethane elastomer material is produced by the action of boron-nitrogen coordination bonds, in which the dynamic covalent boron-nitrogen coordination bonds are composed of ligands such as borate esters and nitrogen-containing electron donors; due to the dynamic nature of borate esters, it is recyclable and reusable, and due to the presence of boron-nitrogen coordination bonds, the RTP effect is significantly improved, and it can produce a long afterglow of up to 6 seconds at 298K with 254nm excitation. The room temperature phosphorescence of the material is realized under room temperature conditions, and it exhibits dual phosphorescence emission at 77K, benefiting from excellent afterglow emission and Ex-De behavior. The dual afterglow emission can be turned on / off by adjusting the excitation wavelength or temperature. Based on this behavior, we successfully demonstrated quadruple anti-counterfeiting information encryption using fluorescence and phosphorescence patterns. This strategy is simple in concept and synthesis, and provides valuable insights into the basic design principles for constructing long-lifetime RTP emission and Ex-De.

[0014] The principle and beneficial effect of this basic scheme are: the material is mainly composed of polycaprolactone (PCL) and isophorone diisocyanate (IPDI) to form a prepolymer, and the prepolymer, adipic acid dihydrazide (ADH) and boron nitrogen coordination small molecules (NCBW-X) constitute the final elastomer. By adding ADH and NCBW-X to the prepolymer, a network structure containing both hydrogen bonds and coordination effects is formed. Such a design not only enhances the anti-counterfeiting performance of polyurethane materials, but also the RTP anti-counterfeiting effect of elastomers. Among them, polycaprolactone (PCL) and isophorone diisocyanate (IPDI) provide the basic polymer skeleton and physical properties of soft segments and hard segments respectively; adipic acid dihydrazide (ADH), as the main source of hydrogen bonds, forms strong hydrogen bonds with the amino acid residues of the polymer chain, enhances the cohesion of the material and promotes phase separation; boron nitrogen coordination small molecules (NCBW-X) form coordination bonds with electron-rich nitrogen atoms and boron atoms with empty orbitals in the polymer, providing additional mechanical performance enhancement and dynamic self-healing mechanisms.

[0015] Furthermore, in step S1, the triolamine compound is triethanolamine, and the boron-nitrogen coordination small molecule formed is NCBW-1.

[0016] Further, the synthesis of NCBW-1 in step S1 specifically includes the following steps: at room temperature, 1,4-phenylenediboronic acid and triethanolamine are dissolved in methanol respectively, then the triethanolamine solution is transferred to a single-necked flask, and then the methanol solution of 1,4-dihydroxyborophene is added dropwise, and a white precipitate begins to form within 1 minute after the addition, and the reaction stops after 5 minutes without further heating. Finally, the precipitate is filtered and washed with ethanol two to three times.

[0017] Further, step S2 is the synthesis of a polyurethane prepolymer containing a boron-nitrogen coordinated small molecule NCBW-1, which specifically includes the following steps: under nitrogen protection, polycaprolactone is dissolved in a three-necked flask, isophorone diisocyanate is added through a syringe, IPDI is added and mixed evenly, and then dibutyltin dilaurate accounting for 0.1wt% of the mass of IPDI / PCL-2000 is added as a catalyst, and stirred in a nitrogen atmosphere at 80°C for 3h to obtain an isocyanate-terminated prepolymer; after cooling to about 50°C, adipic acid dihydrazide is added and the temperature is raised to 80°C and the reaction is continued for 2h, and then the NCBW-1 prepared in step S1 is added thereto, and the reaction is continued for 6h to obtain a polyurethane prepolymer containing a boron-nitrogen coordination bond, which is recorded as PCL-IPDI-ADH-NCBW-1.

[0018] Furthermore, in step S3, the bactericide is dodecyltrimethylammonium chloride, and the antioxidant is one of butylated hydroxytoluene (BHT), triphenyl phosphite (TPP) or butylated hydroxyanisole (BHA).

[0019] By adding these ingredients, the various properties of anti-counterfeiting materials can be further improved, making them more suitable for practical applications and anti-counterfeiting needs.

[0020] The anti-counterfeiting material is prepared by the method for preparing the anti-counterfeiting material inducing RTP by the boron-nitrogen coordination bond.

[0021] Furthermore, the anti-counterfeiting packaging material has the characteristic of Ex-De (excitation dependence), and shows blue emission when irradiated with excitation wavelengths of 254nmUV and 365nmUV light at 298K. After removing the light source, high-brightness green RTP afterglow emission was captured under 254nm excitation for about 6s. In addition, when switching to 365nm UV irradiation, there was no afterglow emission light in the target area. However, when irradiated with excitation wavelengths of 254nm UV and 365nmUV light at 77K, there was still bright blue emission. The difference is that after removing the light source under 254nm UV, the afterglow color changed from green at 298K to blue.

[0022] Furthermore, the anti-counterfeiting packaging material has a green afterglow when excited at 254nm at room temperature 298K, and has no afterglow when excited at 365nm. It has a blue afterglow when excited at 254nm at 77K, and has a green afterglow when excited at 365nm.

[0023] Furthermore, the reversible behavior of the formation and breaking of boron-nitrogen coordination bonds endows the anti-counterfeiting material with the characteristics of being recyclable and reusable.

[0024] The beneficial effects of the present invention are:

[0025] 1. The anti-counterfeiting material disclosed in the present invention induces RTP through the action of boron-nitrogen coordination bonds. Boron-nitrogen coordination small molecules are introduced into the main chain through chain extension reaction. Through molecular design, borate esters and nitrogen-containing electron donors that can form coordination are introduced into the polyurethane main chain respectively to prepare thermoplastic polyurethane elastomer materials based on the synergistic action of dynamic borate esters and BN coordination bonds. BN coordination bonds construct intramolecular and intermolecular supramolecular effects in polyurethane elastomers: intermolecular BN coordination bonds promote the folding of polymer chains, giving the material ultra-high mechanical properties; intermolecular BN coordination bonds act as physical cross-linking points, significantly improving the mechanical strength of the material. At the same time, the introduction of BN coordination bonds in polyurethane elastomers has an RTP effect. In addition, the high reversibility of borate esters and BN coordination bonds gives polyurethane elastomers excellent recyclability and recyclability.

[0026] 2. The anti-counterfeiting material of boron-nitrogen coordination bond induced RTP disclosed in the present invention is mainly composed of polycaprolactone (PCL) and isophorone diisocyanate (IPDI) as prepolymers, adipic acid dihydrazide (ADH) and boron-nitrogen coordination small molecules (NCBW-X) as the final elastomer. By adding ADH and NCBW-X to the prepolymer, a network structure containing both hydrogen bonds and coordination effects is formed. Such a design not only enhances the mechanical properties of the polyurethane material, but also gives it excellent anti-counterfeiting properties and recyclable and recyclable properties.

[0027] 3. The anti-counterfeiting material for inducing RTP by boron-nitrogen coordination bond disclosed in the present invention, wherein the functional small molecule containing boron-nitrogen coordination is constructed by the nucleophilic addition reaction of 1,4-phenylenediboronic acid, 2-hydroxymethyl-1,3-propanediol and triethanolamine, wherein the small molecule is characterized by containing an 8-membered ring of boron-nitrogen coordination, and the material is composed of a main chain consisting of a polycaprolactone (PCL) substrate and isophorone diisocyanate (IPDI), wherein PCL is composed of a long-chain polyester with a molecular weight of about 2000; the material is formed by introducing adipic acid dihydrazide (ADH) and a boron-nitrogen coordination small molecule NCBW-X into the main chain to form an RTP material by boron-nitrogen coordination bond, and the material has the characteristics of Ex-De (excitation dependence);

[0028] The polyurethane anti-counterfeiting material constructed as above is recyclable and reusable, and has RTP properties at room temperature; the special design of the boron-nitrogen coordination bonds in the material allows the coordination bonds to break and reorganize quickly after mechanical damage, thus having green and sustainable performance; the material preparation process is carried out in a water-free and oxygen-free environment to ensure the integrity and stability of the formed polyurethane network structure.

[0029] 4. In the anti-counterfeiting material of the boron-nitrogen coordination bond induced RTP disclosed in the present invention, adipic acid dihydrazide provides a multiple hydrogen bond system for the composite material, and the boron-nitrogen small molecule compound containing the coordination bond structure attacks the boron atom in the boric acid molecule through the secondary amino group as a nucleophilic reagent to form a new boron-nitrogen coordination bond. Its advantage is that the eight-ring borate ester elastomer system formed by boron-nitrogen coordination can retain its RTP characteristics in the polyurethane elastomer segment, and the high dynamics of borate ester can achieve the advantages of recyclability and reusability. Based on the above advantages, the elastomer can realize the dynamic reversible system of non-covalent bonds formed by hydrogen bonds and coordination bonds. First, the terminal hydroxyl polycaprolactone and diisocyanate are first prepolymerized, and then the chain extender containing multiple hydrogen bond systems and the chain extender containing boron-nitrogen with coordination bond structure are added respectively for chain extension to obtain two terminal hydroxyl polymers containing different chain extenders, and the chain extender ratio in the two terminal hydroxyl polymers containing different chain extenders is adjusted. Furthermore, the construction of a non-covalent dynamic reversible system with the synergistic effect of hydrogen bonds and coordination bonds is conducive to the generation of the RTP effect, which lasts up to 6 seconds at room temperature, solving the problem of short afterglow of anti-counterfeiting polyester elastomer materials.

[0030] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:

[0032] Figure 1 The synthetic route of the boron-nitrogen coordination small molecule (NCBW-1) in the embodiment of the present invention is shown in FIG.

[0033] Figure 2 The synthetic route of the waterproof polyurethane elastomer (PCL-IPDI-ADH NCBW-X) containing boron-nitrogen coordination bonds in the examples and comparative examples of the present invention;

[0034] Figure 3is the boron-nitrogen coordination small molecule (NCBW-1) in the embodiment of the present invention 1 H-NMR and 13 C-NMR spectrum, where Figure 3 (a) is a boron-nitrogen coordinated small molecule (NCBW-1) 1 H-NMR spectrum, Figure 3 (b) is a boron-nitrogen coordinated small molecule (NCBW-1) 13 C-NMR spectrum;

[0035] Figure 4 The synthetic route of the boron-nitrogen coordinated small molecule (NCBW-3) in the comparative example of the present invention;

[0036] Figure 5 is the boron nitrogen coordination small molecule (NCBW-3) in the comparative example of the present invention 1 H-NMR and 13 C-NMR (b), where Figure 5 (a) is a boron-nitrogen coordinated small molecule (NCBW-3) 1 H-NMR spectrum, Figure 5 (b) is a boron-nitrogen coordinated small molecule (NCBW-3) 13 C-NMR spectrum;

[0037] Figure 6 This is a dual excitation spectrum of the anti-counterfeiting polyurethane elastomer material (PCL-IPDI-ADH-NCBW-1) prepared in an embodiment of the present invention;

[0038] Figure 7 The fluorescence emission spectrum of the anti-counterfeiting polyurethane elastomer material (PCL-IPDI-ADH-NCBW-1) prepared in an embodiment of the present invention;

[0039] Figure 8 This is a phosphorescence emission spectrum of the waterproof polyurethane elastomer material (PCL-IPDI-ADH-NCBW-1) according to an embodiment of the present invention;

[0040] Fig. 9 (a) shows different afterglow images obtained from PCL-IPDI-ADH-NCBW-1 prepared in the embodiment of the present invention when excited at 254 nm and 365 nm at 77 K and 298 K, respectively; Fig. 9 (b) shows the luminescence of the PCL-IPDI-ADH-NCBW-1 elastomer prepared in the embodiment of the present invention after being dissolved and filled into the mold of the QR code and Chinese characters; Fig. 9 (c) Anti-counterfeiting application of the anti-counterfeiting material prepared according to the embodiment of the present invention. DETAILED DESCRIPTION

[0041] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0042] Anti-counterfeiting performance means that the material can show blue emission when irradiated with excitation wavelengths of 254nm UV and 365nm UV light at 298K, wherein the boron-nitrogen coordination causes energy level structure changes and associated anti-Kasha rule luminescence, thereby inducing phosphorescence emission at room temperature. After removing the light source, high-brightness green RTP afterglow emission was captured under 254nm excitation for about 6s. In addition, when switching to 365nmUV irradiation, there was no afterglow emission in the target area. However, when irradiated with excitation wavelengths of 254nmUV and 365nmUV light at 77K, there was still bright blue emission. The difference is that after the light source was removed under 254nm UV, the afterglow color changed from green at 298K to blue, demonstrating excellent chemical stability and anti-counterfeiting capabilities.

[0043] Example

[0044] like Figure 1 , Figure 2 The method for preparing the anti-counterfeiting material of boron-nitrogen coordination bond-induced RTP comprises the following steps:

[0045] S1, such as Figure 1 Synthesis of boron-nitrogen coordination small molecule (NCBW-1) as shown: 1,4-phenylenediboronic acid (10 g, 0.06 mol) and triethanolamine (12.7 g, 0.12 mol) were dissolved in methanol (about 75 ml) at room temperature. Subsequently, the triethanolamine solution was transferred to a 250 ml single-necked flask. Then the methanol solution of 1,4-dihydroxyboronphenyl was added dropwise. A white precipitate began to form within 1 minute after the addition. The reaction stopped after 5 minutes without further heating. Finally, the precipitate was filtered and washed with ethanol two to three times. This procedure gave a white solid product with a yield of 95%; Figure 3 is the boron-nitrogen coordination small molecule (NCBW-1) of this embodiment. 1 H-NMR and 13 C-NMR spectrum, where Figure 3 (a) is a boron-nitrogen coordinated small molecule (NCBW-1) 1 H-NMR spectrum, Figure 3 (b) is a boron-nitrogen coordinated small molecule (NCBW-1) 13 C-NMR spectrum.

[0046] S2. Synthesize waterproof polyurethane elastomer containing synergistic hydrogen bonds and coordination bonds: Figure 2 As shown in the figure, under nitrogen protection, 20.0g of polycaprolactone (PCL-2000, 0.01mol) was weighed into a 250mL three-necked flask, and 6.67g of isophorone diisocyanate (IPDI, 0.03mol, dissolved in a small amount of DMF) was added through a syringe. After adding IPDI and mixing evenly, 0.1wt% of dibutyltin dilaurate was added as a catalyst, accounting for the mass of IPDI / PCL-2000. Nitrogen was added at 80°C. The mixture was stirred in an atmosphere for 3 hours to obtain an isocyanate-terminated prepolymer; after cooling to about 40°C, 1.74 g of adipic acid dihydrazide (ADH, 0.01 mol) was added, the temperature was raised to 80°C, and the reaction was continued for 2 hours, and then 3.92 g of the boron-nitrogen coordination small molecule (NCBW, 0.01 mol) prepared in step S1 was added thereto, and the reaction was continued for 6 hours to obtain a waterproof polyurethane elastomer containing boron-nitrogen coordination bonds (PCL-IPDI-ADH-NCBW-1);

[0047] S3. Add a bactericide and an antioxidant to the waterproof polyurethane elastomer prepared in step S2, pour the solution into a polytetrafluoroethylene mold, and dry at 70° C. to obtain an anti-counterfeiting material with RTP induced by boron-nitrogen coordination bonds.

[0048] Comparative Example

[0049] The difference between the comparative example and the embodiment is that in step S1, 1,4-phenylenediboronic acid and 2-hydroxymethyl-1,3-propanediol are dissolved and reacted at room temperature by solution reaction to form a boron-nitrogen coordination small molecule (NCBW-3); specifically, the steps are as follows:

[0050] S1, such as Figure 4 Synthesis of boron-nitrogen coordination small molecule (NCBW-3) as shown: 1,4-phenylenediboronic acid (10 g, 0.06 mol) and 2-hydroxymethyl-1,3-propanediol (12.7 g, 0.12 mol) were dissolved in ethanol (about 75 ml) at room temperature. Subsequently, the solution of 2-hydroxymethyl-1,3-propanediol was transferred to a 250 ml single-necked flask. Then the ethanol solution of 1,4-dihydroxyboronphenyl was added dropwise. A white precipitate began to form within 1 minute after the addition. The reaction stopped after 5 minutes without further heating. Finally, the precipitate was filtered and washed with ethanol two to three times. This procedure gave a white solid product with a yield of 95%; Figure 5 is the boron-nitrogen coordination small molecule (NCBW-3) in the comparative example 1 H-NMR and 13 C-NMR (b), where Figure 5 (a) is a boron-nitrogen coordinated small molecule (NCBW-3) 1 H-NMR spectrum, Figure 5(b) is a boron-nitrogen coordinated small molecule (NCBW-3) 13 C-NMR spectrum.

[0051] S2. Synthesis of waterproof polyurethane elastomer containing synergistic hydrogen bonds and coordination bonds: Under nitrogen protection, 20.0 g of polycaprolactone (PCL-2000, 0.01 mol) was weighed into a 250 mL three-necked flask, and 6.67 g of isophorone diisocyanate (IPDI, 0.03 mol, dissolved in a small amount of DMF) was added through a syringe. After adding IPDI and mixing evenly, dibutyltin dilaurate accounting for 0.1 wt% of the mass of IPDI / PCL-2000 and 0.1 wt% was added as a solvent. Catalyst, stirred at 80°C in a nitrogen atmosphere for 3h to obtain an isocyanate-terminated prepolymer; after cooling to about 40°C, 1.74g of adipic acid dihydrazide (ADH, 0.01mol) was added, the temperature was raised to 80°C and the reaction was continued for 2h, and then 3.92g of the boron-nitrogen coordination small molecule (NCBW-3, 0.01mol) prepared in step S1 was added thereto, and the reaction was continued for 6h to obtain a waterproof polyurethane elastomer containing boron-nitrogen coordination bonds (PCL-IPDI-ADH-NCBW-3);

[0052] S3. Add a bactericide and an antioxidant to the waterproof polyurethane elastomer prepared in step S2, pour the solution into a polytetrafluoroethylene mold, and dry at 70° C. to obtain an anti-counterfeiting material with RTP induced by boron-nitrogen coordination bonds.

[0053] Figure 6 This is a dual excitation spectrum of the anti-counterfeiting polyurethane elastomer material (PCL-IPDI-ADH-NCBW-1) of the embodiment. It can be seen from the excitation spectrum of PCL-IPDI-ADH-NCBW-1 that regardless of Em=402nm or Em=432nm, it can be measured that PCL-IPDI-ADH-NCBW-1 has two fluorescence excitation wavelengths, Ex=269nm and Ex=350nm, which just corresponds to the blue emission fluorescence that can be seen at 254nm and 365nm.

[0054] Figure 7 This is the fluorescence emission spectrum of the anti-counterfeiting polyurethane elastomer material (PCL-IPDI-ADH-NCBW-1) of the embodiment. When excited at 269nm at 298K, the emission peak is at 432nm; when excited at 350nm, the emission peak is at 402nm. When excited at 269nm at 77K, the emission peak is at 452nm; and when excited at 350nm, the emission peak is at 402nm.

[0055] Figure 8The phosphorescence emission spectrum of the waterproof polyurethane elastomer material (PCL-IPDI-ADH-NCBW-1) of the embodiment is shown in Figure 1. When excited at 277nm at 298K, the emission peak is at 488nm; when excited at 365nm, the emission peak is at 542nm but there is no obvious phosphorescence emission; when excited at 269nm at 77K, the emission peak is at 416nm; and when excited at 365nm, the emission peak is at 534nm.

[0056] Fig. 9 (a) shows the different afterglow images obtained by exciting PCL-IPDI-ADH-NCB W-1 at 254nm and 365nm at 77K and 298K, respectively. The blue afterglow of 254nm at 77K is as long as more than 34s, while the green afterglow of 365nm at 77K is as long as more than 4.8s, showing the phenomenon of Ex-De dual phosphorescence. Fig. 9 (b) shows the luminescence of the molds of the two-dimensional code and Chinese characters filled with PCL-IPDI-ADH-N CBW-1 elastomer after dissolving, from top to bottom: sunlight, fluorescence, phosphorescence, Fig. 9 (c) A simple anti-counterfeiting application was simulated. PCL-IPDI-ADH-NC BW-1 was dissolved in a mold engraved with 961217 and the four numbers 9627 were filled in. Then, the two numbers 1 were filled in with the dissolved PCL-IPDI-ADH-NCBW-3. After the filling was completed, a layer of rice paper printed with 970125 was covered on the top of the mold. Under sunlight, only the words on the rice paper were displayed, which was the first layer of anti-counterfeiting. When irradiated with ultraviolet 254nm and 365nm, fluorescent 961217 was displayed, which was the second layer of anti-counterfeiting. After turning off the 254nm irradiation, only the four numbers 9627 were displayed in the form of afterglow, while 365nm did not display any numbers, which was the third layer of anti-counterfeiting. In addition, when 254nm and 365nm were turned off at 77K, the six numbers 961217 were displayed in the form of blue and green afterglow respectively, which was the fourth layer of anti-counterfeiting in the form of changing temperature.

[0057] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.

Claims

1. A method for preparing an anti-counterfeiting material with boron-nitrogen coordination bond-induced RTP, characterized in that: The following steps are involved: S1. Synthesis of boron-nitrogen coordination small molecules: dissolving and reacting 1,4-phenylenediboronic acid and triolamine compounds at room temperature through a solution reaction to form a boron-nitrogen coordination small molecule (NCBW-X); S2, synthesizing a waterproof polyurethane elastomer: reacting polycaprolactone and isophorone diisocyanate in a dry solvent, using a catalyst dibutyltin dilaurate, reacting at 80° C. to form a capped prepolymer, adding adipic acid dihydrazide (ADH) to the obtained prepolymer, controlling the reaction temperature to 40-70° C. and the reaction time to 1-4 hours, further adding (NCBW-X) prepared in step S1, controlling the reaction temperature to 80° C. and the reaction time to 4-10 hours, to obtain a waterproof polyurethane elastomer containing boron-nitrogen coordination bonds (PCL-IPDI-ADH-NCBW-X); S3. Add 0.1-1% by mass of a bactericide and 0.1-1% by mass of an antioxidant to the waterproof polyurethane elastomer prepared in step S2, stir evenly to make the bactericide and antioxidant fully dispersed in the prepolymer, pour into a mold after the polymerization reaction is completed, dry and solidify at 70°C to obtain an anti-counterfeiting material with RTP induced by boron-nitrogen coordination bonds.

2. The method for preparing the anti-counterfeiting polyurethane elastomer material according to claim 1, characterized in that: In step S1, the triolamine compound is triethanolamine, and the formed boron-nitrogen coordination small molecule is NCBW-1.

3. The method for preparing the anti-counterfeiting polyurethane elastomer material according to claim 2, characterized in that: The synthesis of NCBW-1 in step S1 is as follows: The method comprises the following steps: at room temperature, 1,4-phenylenediboronic acid and triethanolamine are dissolved in methanol respectively, the triethanolamine solution is then transferred to a single-necked flask, and then a methanol solution of 1,4-dihydroxyborophene is added dropwise, a white precipitate begins to form within 1 minute after the addition, the reaction stops after 5 minutes, no further heating is required, and finally the precipitate is filtered and washed with ethanol two to three times.

4. The method for preparing the anti-counterfeiting polyurethane elastomer material according to claim 2, characterized in that: Step S2 is the synthesis of a polyurethane prepolymer containing a small molecule NCBW-1 with boron-nitrogen coordination, which specifically includes the following steps: under nitrogen protection, polycaprolactone is dissolved in a three-necked flask, isophorone diisocyanate is added through a syringe, IPDI is added and mixed evenly, and then 0.1wt% of dibutyltin dilaurate is added as a catalyst, which is accounted for the mass of IPDI / PCL-2000 and stirred for 3 hours in a nitrogen atmosphere at 80°C to obtain an isocyanate-terminated prepolymer; after cooling to about 50°C, adipic acid dihydrazide is added, the temperature is raised to 80°C, and the reaction is continued for 2 hours, and then the NCBW-1 prepared in step S1 is added thereto, and the reaction is continued for 6 hours to obtain a polyurethane prepolymer containing a boron-nitrogen coordination bond, which is recorded as PCL-IPDI-ADH-NCBW-1.

5. The method for preparing the anti-counterfeiting polyurethane elastomer material according to claim 3, characterized in that: In step S3, the bactericide is dodecyltrimethylammonium chloride, and the antioxidant is one of butylated hydroxytoluene (BHT), triphenyl phosphite (TPP) or butylated hydroxyanisole (BHA).

6. An anti-counterfeiting material prepared by the method for preparing an anti-counterfeiting material inducing RTP by boron-nitrogen coordination bonding as claimed in any one of claims 1 to 5.

7. The anti-counterfeiting material according to claim 6, characterized in that: It has the characteristics of excitation dependence. When irradiated with the excitation wavelengths of 254nm UV and 365nm UV light at 298K, it shows blue emission. After the light source is removed, there is high-brightness green RTP afterglow emission under 254nm excitation. When switched to 365nm UV irradiation, it still has high-brightness blue emission when irradiated with the excitation wavelengths of 254nm UV and 365nm UV light at 77K. After the light source is removed under 254nm UV, the afterglow color changes from green at 298K to blue.

8. The anti-counterfeiting material according to claim 6, characterized in that: At room temperature 298K, 254nm excitation has a green afterglow, and 365nm excitation has no afterglow. At 77K, 254nm excitation has a blue afterglow, and 365nm excitation has a green afterglow.

9. The anti-counterfeiting material according to claim 6, characterized in that: The reversible behavior of the formation and breaking of boron-nitrogen coordination bonds makes the anti-counterfeiting material recyclable and reusable.

Citation Information

Cited By

  • Cardanol-based room-temperature phosphorescent shape memory polymer as well as preparation method and application thereof

    CN120209259A