Heat-conducting liquid crystal polymer composite material and preparation method thereof
By using a pretreatment method for thermally conductive fillers and nanofibers, combined with melt blending, injection molding, and heat treatment, the problems of uneven filler dispersion and poor interfacial compatibility in thermally conductive liquid crystal polymer composites were solved, achieving high thermal conductivity, high mechanical properties, and stability of the material.
Patent Information
- Application Number
- CN202410908483.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
Existing thermally conductive liquid crystal polymer composites suffer from problems such as uneven filler dispersion, poor interfacial compatibility, and decreased mechanical properties, which limit their performance improvement.
By pretreating thermally conductive fillers and nanofibers, and combining the steps of melt blending, injection molding, and heat treatment, thermally conductive liquid crystal polymer composite materials are prepared to ensure uniform dispersion of thermally conductive fillers in the matrix and enhanced interfacial bonding.
It improves the thermal conductivity, tensile strength, and flexural strength of the material, enhances its mechanical properties and thermal stability, ensures its density and uniformity, and extends its service life.
Smart Images

Figure BDA0004932849010000051 
Figure BDA0004932849010000061 
Figure BDA0004932849010000071
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of liquid crystal polymers, and in particular relates to a thermally conductive liquid crystal polymer composite material and a preparation method thereof. Background Art
[0002] Liquid crystal polymer (LCP) has become an important choice for high-performance materials due to its unique molecular structure, excellent mechanical properties, chemical stability and thermal stability. However, the thermal conductivity of LCP itself is not ideal, which limits its application in the field of high thermal conductivity. Therefore, preparing composite materials by introducing thermal conductive fillers into the LCP matrix has become an effective way to improve its thermal conductivity.
[0003] In the prior art, the preparation method of thermally conductive liquid crystal polymer composite materials has problems such as uneven filler dispersion, poor interface compatibility, and decreased mechanical properties, which restricts the further improvement of its performance. Therefore, it is necessary to develop a new thermally conductive liquid crystal polymer composite material and its preparation method to overcome the shortcomings of the prior art. Summary of the invention
[0004] The purpose of the present invention is to provide a thermally conductive liquid crystal polymer composite material and a preparation method thereof. The composite material prepared by the present invention has good thermal conductivity.
[0005] In order to achieve the above-mentioned object and other related objects, the present invention provides the following technical solutions:
[0006] The present invention provides a thermally conductive liquid crystal polymer composite material, and a preparation method thereof comprises the following steps:
[0007] Pretreating a thermally conductive filler to obtain a pretreated thermally conductive filler, wherein the thermally conductive filler includes at least one of gallium nitride, gallium nitride nanomaterials, molybdenum disulfide, and molybdenum disulfide materials;
[0008] pretreating the nanofibers to obtain pretreated nanofibers;
[0009] Mixing a liquid crystal polymer, a pretreated thermal conductive filler, a grafting modifier, an interface treatment agent, pretreated nanofibers, an antioxidant, a plasticizer, and a toughening agent to obtain a mixed raw material;
[0010] Melting and blending the mixed raw materials to obtain a composite material;
[0011] injection molding the composite material to obtain a modified composite material;
[0012] The modified composite material is heat treated to obtain a thermally conductive liquid crystal polymer composite material.
[0013] Preferably, the nanofibers include polyimide nanofibers.
[0014] Preferably, the liquid crystal polymer comprises LCP.
[0015] Preferably, the graft modifier includes PP-g-MAH.
[0016] Preferably, the interface treatment agent includes a silane coupling agent, and the silane coupling agent includes KH-550.
[0017] Preferably, the antioxidant includes antioxidant 1035.
[0018] Preferably, the plasticizer comprises perfluoropolyether.
[0019] Preferably, the toughening agent comprises a polyetheramide elastomer.
[0020] In more detail, the steps include:
[0021] Pre-treating the thermal conductive filler: dispersing the thermal conductive filler in an organic solvent, adding an interface treatment agent, stirring in a water bath, filtering, washing, and drying to obtain a pre-treated thermal conductive filler;
[0022] Pre-treating the nanofibers: adding an interface treatment agent and nanofibers to an organic solvent, ultrasonically dispersing, filtering after dispersion, and drying to obtain pre-treated nanofibers;
[0023] Mixing the liquid crystal polymer, the pretreated thermal conductive filler, the grafting modifier, the interface treatment agent, the pretreated nanofiber, the antioxidant, the plasticizer, and the toughening agent at a stirring speed of 800 to 2000 rpm for 10 to 60 minutes to obtain a mixed raw material;
[0024] The mixed raw materials are melt blended, the extrusion temperature is set to 250-280°C, the screw aspect ratio is 20-40:1, the extrusion speed is set to 30-60rpm, and the shear rate is controlled at 100-300s -1 , obtaining a composite material;
[0025] The composite material is injection molded, the injection temperature is controlled at 240-270° C., the mold temperature is set at 90-110° C., the injection pressure is set at 60-90 MPa, and the injection time is 10-60 seconds to obtain a modified composite material;
[0026] The modified composite material is heat-treated at a temperature of 100 to 200° C. for 1 to 5 hours, and then cooled to obtain a thermally conductive liquid crystal polymer composite material.
[0027] Furthermore, the pretreated thermal conductive filler includes at least one of pretreated gallium nitride nanoparticles and pretreated molybdenum disulfide nanosheets; the weight ratio of the pretreated gallium nitride nanoparticles to the pretreated gallium nitride nanoparticles is 0.5 to 2:1.
[0028] The beneficial effects of the present invention are:
[0029] (1) The formula of the present invention has a reasonable composition. 1) The melting point and other physicochemical information of each component are different. The proportion of the components, the selection of ingredients, the pretreatment and the layer-by-layer treatment (first melt blending, then injection molding, and finally heat treatment) balance the physicochemical properties of each component, and successfully prepare a thermally conductive liquid crystal polymer composite material with better thermal conductivity, tensile strength and bending strength. 2) Generally speaking, the more the amount of thermal conductive filler added, the better the thermal conductivity performance. However, the present invention finds that in the method of the present invention, appropriately reducing the thermal conductive filler can improve the final performance. In terms of weight, in Example 1, the ratio of pretreated gallium nitride nanoparticles to pretreated molybdenum disulfide nanosheets is 1.2:1, in Example 2, the ratio of pretreated gallium nitride nanoparticles to pretreated molybdenum disulfide nanosheets is 1.5:1, and in Example 3, the ratio of pretreated gallium nitride nanoparticles to pretreated molybdenum disulfide nanosheets is 1:1; at the same time, compared with Example 1, Example 3 reduces the amount of thermal conductive filler added, and compared with Example 1, all the properties of Example 3 are improved.
[0030] (2) In the preparation process of the present invention, melt blending is first performed, followed by injection molding, and finally heat treatment. During melt blending, the thermally conductive filler and the LCP matrix are melt blended at high temperature and high shear, so that the thermally conductive filler can be initially and evenly dispersed in the matrix. The reasons for the preparation of the present invention are as follows: 1) Improving the uniformity and density of the material: During the melt blending process, there may be some local filler aggregation or uneven dispersion. In order to avoid the occurrence of this problem, the extruded composite material is further subjected to injection molding, which can make the material fully flow under high temperature and high pressure conditions, further break the aggregation area of the filler, and achieve a more uniform dispersion of the filler in the matrix, thereby improving the density and uniformity of the material. 2) Improving the mechanical properties of the material: High pressure molding during the injection molding process helps to eliminate voids and defects inside the material, thereby improving the mechanical properties of the material, such as tensile strength, bending strength and impact strength. The heat treatment process can release the residual stress inside the material, promote the interface bonding between the matrix and the filler, and improve the comprehensive mechanical properties of the material. 3) Enhanced interface bonding and thermal conductivity: Through injection molding, the LCP matrix can be fully infiltrated with thermal conductive fillers under high pressure, enhancing the interface bonding between the matrix and the filler, reducing the interface thermal resistance, and improving the thermal conduction efficiency. During the heat treatment process, the chemical bonding between the filler and the matrix is further strengthened, and the chemical reaction between the treatment agent on the surface of the filler and the matrix is fully carried out, further improving the interface bonding and thermal conductivity. 4) Stabilize the size and shape of the material: Injection molding can accurately control the size and shape of the product, ensure the dimensional stability of the product after cooling, and can manufacture products of complex shapes according to actual needs. The heat treatment process can stabilize the internal structure of the material, reduce the stress concentration that may occur during the cooling process, and prevent the material from changing size or deforming during use. 5) Improve the thermal stability and durability of the material: Through injection molding, the density and uniformity of the material can be improved, and internal defects can be reduced, thereby improving the thermal stability of the material. Heat treatment can further stabilize the internal structure of the material, improve the durability and stability of the material in a high temperature environment, and extend the service life of the material.
[0031] (3) The mechanism of the present invention: 1) The uniform distribution of thermally conductive fillers and nanofibers in the LCP matrix together constitutes multiple thermal conductive channels, forming an efficient heat conduction network and improving the thermal conductivity of the material. 2) Through the use of interface treatment agents, the bonding force between the thermally conductive fillers and nanofibers and the matrix is enhanced respectively, reducing the interface thermal resistance. 3) Liquid crystal polymer, pretreated thermally conductive filler, grafting modifier, interface treatment agent, pretreated nanofibers, antioxidant, plasticizer, and toughening agent are mixed and used, and each component complements each other and synergistically improves the overall thermal conductivity. For example, the interface treatment agent forms chemical bonds at the interface between other components and the matrix, significantly improving the interface bonding force and thermal conduction efficiency, ensuring high thermal conductivity and high mechanical properties. The multi-level structure formed by polyimide nanofibers is embedded in the matrix, which improves the overall strength and toughness of the material and further improves thermal stability. After preparation, the components of the present invention can be arranged in an orderly manner, especially the layered structure of the thermal conductive filler and the nanofibers. The layered structures can also confine each other. The filling or embedding of other components can make up for the inherent defects of the layered structure, such as uneven distribution, irregular morphology, internal disorder, and poor stability. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] Unless otherwise specified, the equipment and materials used in the examples can be easily obtained from commercial companies.
[0034] The partial addition amounts in the present invention are calculated in parts by weight, and the total number of parts by weight does not need to be equal to 100 parts, which does not violate the basic formulation principle.
[0035] Example 1
[0036] Thermally conductive liquid crystal polymer composite material and preparation method thereof, the steps are as follows:
[0037] 1. Pre-treat thermal conductive filler
[0038] (1) Weigh 12 g of gallium nitride nanoparticles (Article No.: 103818, Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.), disperse them in 100 ml of ethanol solution, add 1 g of interface treatment agent, stir in a 60°C water bath for 2 hours, filter after reaction, wash three times, and dry in a vacuum drying oven at 80°C for 24 hours to obtain pretreated gallium nitride nanoparticles.
[0039] (2) Weigh 12 g of molybdenum disulfide nanosheets (article number AM-MoS2-N-02, Zhejiang Yamei Nanotechnology Co., Ltd.), disperse them in 100 ml of ethanol solution, add 1 g of interface treatment agent, stir in a 60 ° C water bath for 2 hours, after the reaction, filter, wash three times, and dry in a vacuum drying oven at 80 ° C for 24 hours to obtain pretreated molybdenum disulfide nanosheets.
[0040] 2. Pretreatment of Nanofibers
[0041] Add 2g of interface treatment agent to 100ml of ethanol, then add 7g of polyimide nanofiber (polyimide PI nano short fiber-ordinary type, Jiangxi Xiancai Nanofiber Technology Co., Ltd.), use ultrasonic processing equipment to disperse at a frequency of 40kHz for 60 minutes, filter after dispersion, and then put it in a vacuum drying oven at 80°C for 12 hours to obtain pretreated nanofibers.
[0042] 3. Mix
[0043] Referring to Table 1, LCP, pretreated gallium nitride nanoparticles, pretreated molybdenum disulfide nanosheets, polypropylene grafted with methacrylic acid, an interface treatment agent, pretreated nanofibers, an antioxidant, perfluoropolyether, and polyetheramide elastomer were added into a high-speed mixer, and the stirring speed was set to 1200 rpm and the stirring time was 30 minutes to obtain a mixed raw material.
[0044] Table 1
[0045]
[0046] 4. Melt blending
[0047] The mixed raw materials were melt blended through a twin-screw extruder. The extrusion temperature was set to 250°C, the screw aspect ratio was 36:1, the extrusion speed was set to 50 rpm, and the shear rate was controlled at 300 s -1 After extrusion, the material is quickly cooled and formed through a cooling water bath to obtain a composite material.
[0048] 5. Injection molding
[0049] The composite material was added into the hopper of the injection molding machine, the injection temperature was controlled at 250° C., the mold temperature was set to 100° C., the injection pressure was set to 85 MPa, and the injection time was 30 seconds to obtain a modified composite material.
[0050] 6. Heat treatment
[0051] The modified composite material was placed in a constant temperature oven, the temperature was controlled at 150° C., and heat treated for 3 hours. After the heat treatment, the composite material was naturally cooled to room temperature to obtain a thermally conductive liquid crystal polymer composite material.
[0052] Example 2
[0053] Thermally conductive liquid crystal polymer composite material and preparation method thereof, in this embodiment, different from embodiments 1 and 3.
[0054] Referring to Table 2, LCP, pretreated gallium nitride nanoparticles, pretreated molybdenum disulfide nanosheets, polypropylene grafted with methacrylic acid, an interface treatment agent, pretreated nanofibers, an antioxidant, perfluoropolyether, and polyetheramide elastomer were added to a high-speed mixer, and the stirring speed was set to 1200 rpm and the stirring time was 30 minutes to obtain a mixed raw material.
[0055] Table 2
[0056]
[0057] The rest is the same as Example 1.
[0058] Example 3
[0059] Thermally conductive liquid crystal polymer composite material and preparation method thereof, in this embodiment, different from embodiments 1 and 3.
[0060] Referring to Table 3, LCP, pretreated gallium nitride nanoparticles, pretreated molybdenum disulfide nanosheets, polypropylene grafted with methacrylic acid, an interface treatment agent, pretreated nanofibers, an antioxidant, perfluoropolyether, and polyetheramide elastomer were added to a high-speed mixer, the stirring speed was set to 1200 rpm, the stirring time was set to 28 minutes, and a mixed raw material was obtained.
[0061] Table 3
[0062]
[0063] The rest is the same as Example 1.
[0064] Comparative Example 1
[0065] Liquid crystal polymer composite material and preparation method thereof, without adding thermal conductive filler and nanofiber, the steps are as follows:
[0066] 1. Mix
[0067] Referring to Table 4, LCP, polypropylene grafted with methacrylic acid, interface treatment agent, antioxidant, perfluoropolyether, and polyetheramide elastomer were added into a high-speed mixer, and the stirring speed was set to 1200 rpm and the stirring time was set to 30 minutes to obtain a mixed raw material.
[0068] Table 4
[0069]
[0070] 2. Melt blending
[0071] The mixed raw materials were melt blended through a twin-screw extruder. The extrusion temperature was set at 280 °C, the screw aspect ratio was 36:1, the extrusion speed was set at 50 rpm, and the shear rate was controlled at 300 s -1 After extrusion, the material is quickly cooled and formed through a cooling water bath to obtain a composite material.
[0072] 3. Injection molding
[0073] The composite material was added into the hopper of the injection molding machine, the injection temperature was controlled at 270°C, the mold temperature was set to 110°C, the injection pressure was set to 85 MPa, and the injection time was 30 seconds to obtain a modified composite material.
[0074] 4. Heat treatment
[0075] The modified composite material was placed in a constant temperature oven, the temperature was controlled at 150° C., and heat treated for 3 hours. After the heat treatment, the composite material was naturally cooled to room temperature to obtain a liquid crystal polymer composite material.
[0076] Comparative Example 2
[0077] A thermally conductive liquid crystal polymer composite material and a preparation method thereof, without pre-treating the thermally conductive filler and the nanofiber, comprises the following steps:
[0078] 1. Mix
[0079] Referring to Table 5, LCP, gallium nitride nanoparticles, molybdenum disulfide nanosheets, polypropylene grafted with methacrylic acid, an interface treatment agent, polyimide nanofibers, an antioxidant, perfluoropolyether, and polyetheramide elastomer are added to a high-speed mixer, the stirring speed is set to 1200 rpm, the stirring time is 30 minutes, and a mixed raw material is obtained.
[0080] Table 5
[0081]
[0082] 2. Melt blending
[0083] The mixed raw materials were melt blended through a twin-screw extruder. The extrusion temperature was set to 250°C, the screw aspect ratio was 36:1, the extrusion speed was set to 50 rpm, and the shear rate was controlled at 300 s -1 After extrusion, the material is quickly cooled and formed through a cooling water bath to obtain a composite material.
[0084] 3. Injection molding
[0085] The composite material was added into the hopper of the injection molding machine, the injection temperature was controlled at 250° C., the mold temperature was set to 100° C., the injection pressure was set to 85 MPa, and the injection time was 30 seconds to obtain a modified composite material.
[0086] 4. Heat treatment
[0087] The modified composite material was placed in a constant temperature oven, the temperature was controlled at 150° C., and heat treated for 3 hours. After the heat treatment, the composite material was naturally cooled to room temperature to obtain a thermally conductive liquid crystal polymer composite material.
[0088] Comparative Example 3
[0089] A thermally conductive liquid crystal polymer composite material and a preparation method thereof, without heat treatment, comprises the following steps:
[0090] 1. Pre-treat thermal conductive filler
[0091] (1) Weigh 12 g of gallium nitride nanoparticles (Article No.: 103818, Jiangsu Xianfeng Nanomaterial Technology Co., Ltd.), disperse them in 100 ml of ethanol solution, add 1 g of interface treatment agent, stir in a 60°C water bath for 2 hours, filter after reaction, wash three times, and dry in a vacuum drying oven at 80°C for 24 hours to obtain pretreated gallium nitride nanoparticles.
[0092] (2) Weigh 12 g of molybdenum disulfide nanosheets (article number AM-MoS2-N-02, Zhejiang Yamei Nanotechnology Co., Ltd.), disperse them in 100 ml of ethanol solution, add 1 g of interface treatment agent, stir in a 60 ° C water bath for 2 hours, after the reaction, filter, wash three times, and dry in a vacuum drying oven at 80 ° C for 24 hours to obtain pretreated molybdenum disulfide nanosheets.
[0093] 2. Pretreatment of Nanofibers
[0094] Add 2g of interface treatment agent to 100ml of ethanol, then add 7g of polyimide nanofiber (polyimide PI nano short fiber-ordinary type, Jiangxi Xiancai Nanofiber Technology Co., Ltd.), use ultrasonic processing equipment to disperse at a frequency of 40kHz for 60 minutes, filter after dispersion, and then put it in a vacuum drying oven at 80°C for 12 hours to obtain pretreated nanofibers.
[0095] 3. Mix
[0096] Referring to Table 1, LCP, pretreated gallium nitride nanoparticles, pretreated molybdenum disulfide nanosheets, polypropylene grafted with methacrylic acid, an interface treatment agent, pretreated nanofibers, an antioxidant, perfluoropolyether, and polyetheramide elastomer were added into a high-speed mixer, and the stirring speed was set to 1200 rpm and the stirring time was 30 minutes to obtain a mixed raw material.
[0097] 4. Melt blending
[0098] The mixed raw materials were melt blended through a twin-screw extruder. The extrusion temperature was set to 250°C, the screw aspect ratio was 36:1, the extrusion speed was set to 50 rpm, and the shear rate was controlled at 300 s -1 After extrusion, the material is quickly cooled and formed through a cooling water bath to obtain a composite material.
[0099] 5. Injection molding
[0100] The composite material was added into the hopper of the injection molding machine, the injection temperature was controlled at 250° C., the mold temperature was set to 100° C., the injection pressure was set to 85 MPa, and the injection time was 30 seconds to obtain a thermally conductive liquid crystal polymer composite material.
[0101] Detection:
[0102] Sampling: Samples with a diameter of 10 mm and a thickness of 2 mm were cut out from the finished products of Examples 1 to 3 and Comparative Examples 1 to 3, respectively.
[0103] Thermal conductivity, tensile strength, and flexural strength refer to the method of patent application publication number CN109161225A
[0104] The results are shown in Table 6 below.
[0105] Table 6
[0106]
[0107] Result analysis:
[0108] Referring to Table 6, Examples 1 to 3 are compared with Comparative Examples 1 to 3:
[0109] In Comparative Example 1, no thermal conductive filler and nanofibers were added, and the thermal conductivity was significantly reduced. The thermal conductivity of Example 2 was 4 times that of Comparative Example 1, and the tensile strength and flexural strength were also the worst.
[0110] In Comparative Example 2, the thermal conductive filler and nanofibers are not pretreated, and the performance is also significantly reduced, but it is better than Comparative Example 1. The thermal conductivity of Example 2 can reach 1.4 times that of Comparative Example 2.
[0111] In Comparative Example 3, no heat treatment is performed and various properties also decrease, but it is better than Comparative Example 1 and Comparative Example 2. The thermal conductivity of Example 2 can reach 1.25 times that of Comparative Example 3.
[0112] Compare Examples 1 to 3:
[0113] Example 2 adjusts the addition ratio of pretreated gallium nitride nanoparticles and pretreated molybdenum disulfide nanosheets, increases the total addition amount of thermal conductive filler, increases the addition amount of nanofibers, and reduces the addition amount of plasticizer. Compared with Example 1, various properties of Example 2 are improved.
[0114] Compared with Example 1, Example 3 reduces the amount of thermally conductive filler added, and compared with Example 1, various properties of Example 3 are improved.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a thermally conductive liquid crystal polymer composite material, characterized in that: The steps include: Pretreating a thermally conductive filler to obtain a pretreated thermally conductive filler, wherein the thermally conductive filler includes at least one of gallium nitride, gallium nitride nanomaterials, molybdenum disulfide, and molybdenum disulfide materials; pretreating the nanofibers to obtain pretreated nanofibers; Mixing a liquid crystal polymer, a pretreated thermal conductive filler, a grafting modifier, an interface treatment agent, pretreated nanofibers, an antioxidant, a plasticizer, and a toughening agent to obtain a mixed raw material; Melting and blending the mixed raw materials to obtain a composite material; injection molding the composite material to obtain a modified composite material; The modified composite material is heat treated to obtain a thermally conductive liquid crystal polymer composite material.
2. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The nanofibers include polyimide nanofibers.
3. The method for preparing the thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The liquid crystal polymer includes LCP.
4. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The graft modifier includes PP-g-MAH.
5. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The interface treatment agent includes a silane coupling agent, and the silane coupling agent includes KH-550.
6. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The antioxidant includes antioxidant 1035.
7. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The plasticizer includes perfluoropolyether.
8. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The toughening agent includes a polyetheramide elastomer.
9. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The steps include: Pre-treating the thermal conductive filler: dispersing the thermal conductive filler in an organic solvent, adding an interface treatment agent, stirring in a water bath, filtering, washing, and drying to obtain a pre-treated thermal conductive filler; Pre-treating the nanofibers: adding an interface treatment agent and nanofibers to an organic solvent, ultrasonically dispersing, filtering after dispersion, and drying to obtain pre-treated nanofibers; Mixing the liquid crystal polymer, the pretreated thermal conductive filler, the grafting modifier, the interface treatment agent, the pretreated nanofiber, the antioxidant, the plasticizer, and the toughening agent at a stirring speed of 800 to 2000 rpm for 10 to 60 minutes to obtain a mixed raw material; The mixed raw materials are melt blended, the extrusion temperature is set to 250-280°C, the screw aspect ratio is 20-40:1, the extrusion speed is set to 30-60rpm, and the shear rate is controlled at 100-300s -1 , obtaining a composite material; The composite material is injection molded, the injection temperature is controlled at 240-270° C., the mold temperature is set at 90-110° C., the injection pressure is set at 60-90 MPa, and the injection time is 10-60 seconds to obtain a modified composite material; The modified composite material is heat-treated at a temperature of 100 to 200° C. for 1 to 5 hours, and then cooled to obtain a thermally conductive liquid crystal polymer composite material.
10. The method for preparing a thermally conductive liquid crystal polymer composite material according to claim 1, characterized in that: The pretreated thermal conductive filler includes at least one of pretreated gallium nitride nanoparticles and pretreated molybdenum disulfide nanosheets; the weight ratio of the pretreated gallium nitride nanoparticles to the pretreated gallium nitride nanoparticles is 0.5 to 2:1.
Citation Information
Cited By
Rubber composition for tire shoulder pad rubber and preparation method thereof
CN121851483A