Organic-inorganic composite binder and lithium ion battery negative pole piece

By using organic and inorganic composite adhesives in the negative electrode material of lithium-ion battery, using boron-containing inorganic substances and basic adhesives to form a three-dimensional structure, the problem of volume expansion of silicon-carbon composite materials during charging and discharging is solved, and the circulation performance is improved and safety, achieving efficient electrochemical performance improvement.

CN118879239APending Publication Date: 2024-11-01NINGBO HANGCHANG METAL MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411035347.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The graphite capacity of the negative electrode material of lithium-ion batteries is low and the safety performance is poor. The volume expansion of silicon-carbon composite materials during charging and discharging leads to poor circulation performance. The existing adhesive cannot effectively alleviate structural damage.

Method used

The organic and inorganic composite adhesive is used to form a three-dimensional elastic mesh structure through boron-containing inorganic substances and base adhesives, which alleviates the volume expansion and stress changes of silicon, and improves the adhesion between the negative electrode material and the current collector through B-OH bonds. Promotes stable SEI layer formation.

Benefits of technology

It significantly improves the circulation performance of lithium-ion batteries, enhances the bonding and electrochemical properties of the negative electrode materials, and reduces the production cost and production complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879239A_ABST
    Figure CN118879239A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of secondary batteries, and particularly relates to an organic-inorganic composite binder and a lithium ion battery negative pole piece. The organic-inorganic composite binder comprises the following components in parts by weight: 8.0 to 9.5 parts of a basic binder, 0.5 to 2.0 parts of a boron-containing inorganic substance and 80 to 100 parts of water, the basic binder is a binder containing carboxyl or hydroxyl, and the boron-containing inorganic matter is boric acid containing-B-O-bonds or borate containing no heavy metal ions; the lithium ion battery negative pole piece comprises a silicon carbon material, a conductive agent and the organic-inorganic composite binder. The boron-containing inorganic matter is used for modifying the basic binder, the composite binder with excellent binding performance is finally obtained, and the composite binder is used for the lithium ion battery negative pole piece, so that the volume expansion and stress change of silicon can be relieved, and the cycle performance of the lithium ion battery is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of secondary batteries, and in particular relates to an organic-inorganic composite binder and a negative electrode sheet of a lithium-ion battery. Background Art

[0002] Lithium-ion batteries (LIBs) are currently the most mainstream chemical energy storage power source due to their high specific energy and good cycle performance. However, the commercial negative electrode material - graphite, has low capacity and poor safety performance, and can no longer meet people's needs for high energy density and good safety performance of lithium-ion batteries. Therefore, it is urgent to develop some new lithium-ion battery negative electrode materials with high capacity, low cost and high safety performance. Elemental silicon has a high theoretical specific capacity (4200mAh / g) and low cost, making it the most promising negative electrode material. However, the silicon negative electrode will produce a large volume expansion (up to 300%) during the charging and discharging process, which brings a series of problems such as powder shedding, unstable SEI layer (Solid Electrolyte Interface) and particle pulverization, resulting in poor cycle performance of the negative electrode material and cannot be well applied to lithium-ion batteries. Therefore, silicon-carbon composite materials, which also have high capacity and better cycle performance, have become relatively good substitutes.

[0003] Although the carbon material in the silicon-carbon negative electrode material can alleviate the negative impact of silicon volume expansion to a certain extent, making the silicon-carbon negative electrode have better cycle performance than pure silicon materials, this mitigation effect is limited, and it is still necessary to further improve the electrochemical performance of the silicon-carbon negative electrode through various modifications. Among them, the negative impact of silicon volume expansion can also be effectively alleviated by reasonable design of the binder. Commonly used binders such as polyvinylidene fluoride (PVDF), sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), etc., the molecules themselves are linear structures, the main skeleton structure is soft, and chain slippage will occur during the volume expansion of silicon particles, thereby destroying the structure of the binder in the electrode. Therefore, it is urgent to develop a binder that can fully alleviate the volume expansion of silicon and will not change the structure, thereby effectively improving the cycle performance of the silicon-carbon negative electrode. Summary of the invention

[0004] The purpose of the present invention is to provide an organic-inorganic composite binder to address the above technical problems. The base binder is modified with a boron-containing inorganic substance to obtain a composite binder with excellent bonding properties. The composite binder is used for the negative electrode of a lithium-ion battery and can effectively improve the cycle performance of the lithium-ion battery.

[0005] The organic-inorganic composite binder in the technical solution of the present invention comprises the following components in parts by weight: 8.0 to 9.5 parts of a basic binder, 0.5 to 2.0 parts of a boron-containing inorganic substance and 80 to 100 parts of water.

[0006] The organic-inorganic composite binder obtained by the present invention forms a three-dimensional elastic network structure through the action of a large number of hydrogen bonds and covalent bonds in the basic binder, the boron-containing inorganic substance and water, and can effectively alleviate the volume expansion and stress change of silicon during the charging and discharging process; the boron-containing inorganic substance itself has a small molecule and a simple structure, and is more likely to release a -BO- group, so it is easier to achieve connection between molecular chains and play an ion conduction and electron conduction role; at the same time, the B-OH bond can chemically react with the negative electrode material on its surface, thereby improving the adhesion between the negative electrode material and the current collector; the boron element itself can also participate in the formation of the SEI layer, which is helpful to form a stable SEI layer.

[0007] Furthermore, the base binder is a binder containing carboxyl groups or hydroxyl groups.

[0008] Furthermore, the basic binder is one or more of polyacrylic acid, sodium carboxymethyl cellulose, and sodium alginate.

[0009] Furthermore, the boron-containing inorganic substance is boric acid containing a -BO- bond or a borate containing no heavy metal ions.

[0010] Furthermore, the boron-containing inorganic substance is one or more of boric acid, lithium borate and sodium borate.

[0011] Furthermore, the mass ratio of the base binder to the boron-containing inorganic substance is 4 to 12:1.

[0012] The method for preparing the organic-inorganic composite binder comprises the following steps: adding the base binder into water, mixing and stirring, adding the boron-containing inorganic substance, and heating and mixing.

[0013] Furthermore, the temperature during heating and mixing is 40 to 60°C.

[0014] The present invention also provides a lithium ion battery negative electrode plate, comprising a silicon-carbon material, a conductive agent and the above-mentioned organic-inorganic composite binder.

[0015] Furthermore, the amounts of silicon-carbon material, conductive agent and organic-inorganic composite binder in the negative electrode sheet of the lithium-ion battery are 7.0-9.0 parts, 0.5-2.0 parts and 0.5-2.0 parts respectively.

[0016] The method for preparing the negative electrode sheet of the lithium-ion battery comprises the following steps: uniformly mixing the silicon-carbon material, the conductive agent and the organic-inorganic composite binder, coating the mixture on the current collector, and performing stamping after vacuum drying.

[0017] The conductive agent in the negative electrode plate of the lithium ion battery of the present invention is not limited, and any conductive agent that can be applied to lithium ion batteries can be used. The conductive agent can be listed as one or more of conductive carbon black, conductive graphite, carbon fiber, and carbon nanotubes.

[0018] Preferably, the current collector is copper foil.

[0019] Furthermore, the drying temperature is 80-120° C., and the drying time is 6-12 hours.

[0020] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0021] (1) The basic binder is modified with a boron-containing inorganic substance to obtain a composite binder with excellent bonding performance, which can be used for the negative electrode of lithium-ion batteries to alleviate the volume expansion and stress change of silicon and effectively improve the cycle performance of lithium-ion batteries;

[0022] (2) Boron-containing inorganic substances have small molecules and simple structures, and are more likely to release -BO- groups, thus achieving connections between molecular chains and playing the role of ion and electron conduction. At the same time, the B-OH bond can react chemically with the negative electrode material on its surface, thus improving the bonding between the negative electrode material and the current collector.

[0023] (3) The boron element in boron-containing inorganic substances can also participate in the formation of the SEI layer, which helps to form a stable SEI layer;

[0024] (4) The obtained organic-inorganic composite binder forms a three-dimensional elastic network structure by a large number of hydrogen bonds and covalent bonds in the base binder, boron-containing inorganic substances and water, which can alleviate the volume expansion and stress changes of silicon during the charge and discharge process;

[0025] (5) The preparation method of the organic-inorganic composite binder uses water as the solvent throughout the process, the conditions are mild, the cost is low, the preparation process is simple, and it can be mass-produced. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The AC impedance spectra of the lithium ion batteries obtained in Example 1 and Comparative Examples 4-5 are shown;

[0027] Figure 2 The graph is a cycle performance diagram of the lithium ion batteries obtained in Example 1 and Comparative Examples 4-5 at a rate of 0.2C. DETAILED DESCRIPTION

[0028] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosed content of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0029] Example 1

[0030] The preparation method of the organic-inorganic composite binder of this embodiment comprises the following steps: adding 9.0 parts of polyacrylic acid to 90 parts of water, stirring magnetically until the solution is clear and transparent, adding 1.0 parts of boric acid, heating to 60° C., and continuing stirring until the organic-inorganic composite binder is completely dissolved;

[0031] The silicon-carbon material, super carbon black and organic-inorganic composite binder were uniformly mixed in a mass ratio of 8:1:1, coated on a copper foil, vacuum dried at 100° C. for 8 hours, and then stamped to obtain a negative electrode sheet for a lithium-ion battery.

[0032] Example 2

[0033] The preparation method of the organic-inorganic composite binder of this embodiment comprises the following steps: adding 9.0 parts of sodium carboxymethyl cellulose to 95 parts of water, stirring with a magnetic stirrer until the solution is clear and transparent, adding 1.0 parts of lithium borate, heating to 55° C., and continuing stirring until the organic-inorganic composite binder is completely dissolved;

[0034] The silicon-carbon material, super carbon black and organic-inorganic composite binder were uniformly mixed in a mass ratio of 7.5:1.0:1.5, coated on a copper foil, vacuum dried at 110° C. for 8 h, and then stamped to obtain a negative electrode sheet for a lithium-ion battery.

[0035] Example 3

[0036] The preparation method of the organic-inorganic composite binder of this embodiment comprises the following steps: adding 9.0 parts of sodium alginate to 100 parts of water, stirring magnetically until the solution is clear and transparent, adding 1.0 parts of sodium borate, heating to 50° C., and continuing stirring until the organic-inorganic composite binder is completely dissolved;

[0037] The silicon-carbon material, super carbon black and organic-inorganic composite binder were uniformly mixed in a mass ratio of 7.5:1.5:1.0, coated on a copper foil, vacuum dried at 90° C. for 10 h, and then stamped to obtain a negative electrode sheet for a lithium-ion battery.

[0038] Example 4

[0039] The difference between this embodiment and embodiment 1 is that 8.5 parts of polyacrylic acid are added to 90 parts of water, magnetically stirred until the solution is clear and transparent, 1.5 parts of boric acid are added, heated to 60° C., and stirred continuously until the organic-inorganic composite binder is completely dissolved.

[0040] Example 5

[0041] The difference between this embodiment and embodiment 1 is that 8.0 parts of polyacrylic acid are added to 90 parts of water, magnetically stirred until the solution is clear and transparent, 2.0 parts of boric acid are added, heated to 60° C., and stirred continuously until the organic-inorganic composite binder is completely dissolved.

[0042] Comparative Example 1

[0043] The difference between this comparative example and Example 1 is that 9.0 parts of polyacrylic acid are added to 90 parts of water, magnetically stirred until the solution is clear and transparent, 2.5 parts of boric acid are added, heated to 60° C., and stirred continuously until the organic-inorganic composite binder is completely dissolved.

[0044] Comparative Example 2

[0045] The difference between this comparative example and Example 1 is that 9.0 parts of polyacrylic acid are added to 90 parts of water, magnetically stirred until the solution is clear and transparent, 0.4 parts of boric acid are added, heated to 60° C., and stirred continuously until the organic-inorganic composite binder is completely dissolved.

[0046] Comparative Example 3

[0047] The difference between this comparative example and Example 1 is that 9.0 parts of polyacrylic acid are added to 90 parts of water, magnetically stirred until the solution is clear and transparent, 1.0 part of triethanolamine borate is added, heated to 60° C., and stirred continuously until the organic-inorganic composite binder is completely dissolved.

[0048] Comparative Example 4

[0049] The binder used in this comparative example is obtained by adding 10.0 parts of polyacrylic acid to 90 parts of water and stirring with a magnetic stirrer until the solution is clear and transparent;

[0050] The silicon-carbon material, super carbon black and the obtained binder were uniformly mixed in a mass ratio of 8:1:1, coated on a copper foil, vacuum dried at 100° C. for 8 hours and then stamped to obtain a negative electrode sheet for a lithium-ion battery.

[0051] Comparative Example 5

[0052] The binder used in this comparative example is obtained by adding 10.0 parts of polyvinylidene fluoride to 90 parts of water and stirring with a magnetic stirrer until the solution is clear and transparent;

[0053] The silicon-carbon material, super carbon black and the obtained binder were uniformly mixed in a mass ratio of 8:1:1, coated on a copper foil, vacuum dried at 100° C. for 8 hours and then stamped to obtain a negative electrode sheet for a lithium-ion battery.

[0054] Comparative Example 6

[0055] The preparation method of the negative electrode plate of the lithium-ion battery in this comparative example comprises the following steps: mixing silicon-carbon material, super carbon black, 9% polyacrylic acid solution and boric acid in a mass ratio of 8:1:0.99:0.01, coating the mixture on copper foil, and performing stamping after vacuum drying at 100°C for 8 hours.

[0056] The negative electrode of the lithium-ion battery obtained in the embodiment and the comparative example is used as the electrode, the metal lithium is used as the counter electrode, and the electrolyte is LiPF6 / DMC:EC (V:V=7:3) with a concentration of 1 mol / L containing 5% FEC electrolyte additive. The button cell is assembled in a glove box protected by an argon atmosphere. The battery tester of Wuhan Blue Electric Electronics Co., Ltd. is used for electrochemical performance testing, the charge and discharge voltage range is 0.01V~1.5V (vs.Li+ / Li), and the test temperature is 30°C. At the same time, the impedance test is carried out using the French Biologic VMP-3E electrochemical workstation, and the test frequency is 100mHz~100kHz.

[0057] The conductivity of the negative electrode sheet of the lithium ion battery obtained in Example 1 is 3.096 S / cm, the conductivity of the negative electrode sheet of the lithium ion battery obtained in Comparative Example 4 is 2.019 S / cm, and the conductivity of the negative electrode sheet of the lithium ion battery obtained in Comparative Example 5 is 1.739 S / cm, indicating that the organic-inorganic composite binder cross-linked with boric acid is more conducive to the conduction of electrons; Figure 1 It can be seen that after CV cycles, the SEI impedance value of the lithium ion battery obtained in Example 1 is significantly smaller, indicating that the boron-containing inorganic substance helps to form a stable SEI layer and has good ion conduction and electron conduction effects.

[0058] Table 1 Electrochemical performance data of lithium ion batteries obtained in Examples and Comparative Examples

[0059]

[0060]

[0061] From Table 1 and Figure 2It can be obtained that the lithium ion battery obtained in Example 1 has a high initial capacity and good cycle performance; the lithium ion batteries obtained in Examples 2-5 also have good cycle performance; in Example 1, too much boric acid is added, so that the proportion of carboxyl groups that play a bonding role in the composite binder is reduced, resulting in poor overall bonding performance, reduced initial coulomb efficiency, and poor cycle performance; in Example 2, too little boric acid is added, and only a small amount of polyacrylic acid chain segments are cross-linked, the cross-linked network structure is reduced, the improvement of the bonding performance of the binder and the improvement of the stability of the SEI layer are reduced, and the cycle performance of the lithium ion battery is poor; in Example 3, polyacrylic acid is modified using an organic borate to obtain a binder, and triethanolamine borate separates the BO3 group The difficulty of crosslinking is greater, and the steric hindrance is slightly larger, the degree of crosslinking with the carboxylic acid group of polyacrylic acid is reduced, the bonding effect of the binder is deteriorated, and the cycle performance of the lithium ion battery is reduced; Comparative Examples 4 and 5 use polyacrylic acid and polyvinylidene fluoride as binders respectively, without adding boron-containing inorganic substances, the bonding effect between the silicon-carbon material and the current collector is greatly reduced, and the resulting lithium ion battery cycle performance is deteriorated; Comparative Example 6 is to directly add polyacrylic acid solution and boric acid in the process of preparing the negative electrode sheet of the lithium ion battery. When the negative electrode slurry is stirred, the boric acid is not completely combined with the polyacrylic acid. When the electrode sheet is dried, a part of the boric acid powder will be combined with the polyacrylic acid and will not play a role, resulting in poor bonding effect and reduced lithium ion battery cycle performance.

[0062] Finally, it should be noted that the specific embodiments described herein are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make various modifications or supplements to the described embodiments or replace them in similar ways. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. An organic-inorganic composite binder, characterized in that: The invention comprises the following components in parts by weight: 8.0 to 9.5 parts of a basic binder, 0.5 to 2.0 parts of a boron-containing inorganic substance and 80 to 100 parts of water.

2. The organic-inorganic composite binder according to claim 1, characterized in that: The base binder is a binder containing carboxyl groups or hydroxyl groups.

3. The organic-inorganic composite binder according to claim 2, characterized in that: The basic binder is one or more of polyacrylic acid, sodium carboxymethyl cellulose and sodium alginate.

4. The organic-inorganic composite binder according to claim 1, characterized in that: The boron-containing inorganic substance is boric acid containing a -BO- bond or a borate containing no heavy metal ions.

5. The organic-inorganic composite binder according to claim 4, characterized in that: The boron-containing inorganic substance is one or more of boric acid, lithium borate and sodium borate.

6. The organic-inorganic composite binder according to claim 1, characterized in that: The mass ratio of the basic binder to the boron-containing inorganic substance is 4 to 12:

1.

7. A method for preparing the organic-inorganic composite binder according to claim 1, characterized in that: The method comprises the following steps: adding a basic binder into water, mixing and stirring, adding a boron-containing inorganic substance, and heating and mixing.

8. The preparation method according to claim 7, characterized in that: The temperature during heating and mixing is 40 to 60°C.

9. A negative electrode plate for a lithium ion battery, characterized in that: The invention comprises a silicon-carbon material, a conductive agent and the organic-inorganic composite binder according to claim 1.

10. The negative electrode plate of a lithium-ion battery according to claim 9, characterized in that: The usage of silicon-carbon material, conductive agent and organic-inorganic composite binder are 7.0-9.0 parts, 0.5-2.0 parts and 0.5-2.0 parts respectively.