Preparation method of lithium ion silicon negative electrode battery biopolymer binder
The lithium-ion silicon negative electrode battery biopolymer binder prepared by soap-free emulsion polymerization uses the dual functional groups of guar gum and gum arabic to solve the problem of poor volume expansion and flexibility of silicon negative electrode, significantly improving the electricity of lithium-ion batteries Chemical performance stability.
Patent Information
- Application Number
- CN202411117798.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-01
AI Technical Summary
The huge volume expansion of the silicon negative electrode during charging and discharging of lithium-ion batteries leads to excessive growth of the electrode solid electrolyte membrane and the shedding of active substances, reducing the battery capacity and cycle life. At the same time, existing ion polymer-type binders lead to lithium-ion negative electrodes The flexibility is poor and it is prone to charge and discharge cracking.
The lithium-ion silicon negative electrode battery biopolymer binder was prepared by soap-free emulsion polymerization method, and the reaction was initiated by ammonium persulfate under heating conditions. A binder containing dual functional groups was prepared to enhance the bond strength and mechanical properties of the silicon negative electrode.
Through hydrogen bonds and chemical bonds of dual functional groups, the integrity of the silicon negative electrode is maintained, the shedding and pulverization are prevented, flexibility is improved, and the volume changes during the charging and discharge process is overcome, which significantly improves the electrochemical performance stability of lithium-ion batteries.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lithium ion batteries, and in particular to a method for preparing a biopolymer binder for lithium ion silicon negative electrode batteries. Background Art
[0002] Among the many negative electrode materials for lithium-ion batteries under research, silicon negative electrode undoubtedly has obvious advantages. It has a theoretical specific capacity of up to 4200mAh / g, which is much higher than the theoretical specific capacity of graphite negative electrode of 3700mAh / g. In addition, silicon is environmentally friendly, abundant in resources, has a low lithium insertion potential, and its operating voltage is close to that of graphite. Therefore, it is considered to be the most promising negative electrode material. However, the huge volume expansion (>400%) of silicon negative electrode during charging and discharging will lead to excessive growth of electrode solid electrolyte membrane (SEI) and shedding of active materials, resulting in rapid attenuation of battery capacity and shortened cycle life. Therefore, how to improve the defects of silicon negative electrode to improve the electrochemical performance of lithium-ion batteries has become a problem that needs to be solved urgently.
[0003] In addition, water-based binders have an important influence on the performance of lithium-ion battery electrodes and have become an important direction for the development of lithium battery electrode binders, among which ion polymer binders are one of the important research directions of water-based binders. However, the current ion polymer binders still have a high addition amount, which leads to poor flexibility of lithium-ion negative electrodes, and thus easily causes cracking of electrodes during charging and discharging.
[0004] According to the above situation, the inventors of the present invention conducted a comprehensive study on this, and finally prepared a lithium-ion silicon negative electrode battery biopolymer binder by a soap-free emulsion polymerization method, which can improve the defect of poor flexibility of the lithium-ion negative electrode. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a biopolymer binder for lithium-ion silicon negative electrode batteries to solve the problems raised in the above background technology.
[0006] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing a biopolymer binder for a lithium-ion silicon negative electrode battery comprises the following steps: adding guar gum, gum arabic, polyacrylic acid and deionized water into a reaction kettle in a certain proportion, stirring at a speed of 150-250 r / min for 20-30 min, heating to 60-75° C., adding ammonium persulfate to initiate a reaction for 6-12 h, and preparing the biopolymer binder for a lithium-ion silicon negative electrode battery.
[0007] Furthermore, the amount of ammonium persulfate added is 0.5% of the total mass of the raw materials.
[0008] Furthermore, the lithium-ion silicon negative electrode battery biopolymer binder includes the following component raw materials: by mass percentage, 0-30% guar gum, 0-30% gum arabic, 40-50% polyacrylic acid, and 20-30% deionized water.
[0009] Furthermore, in an embodiment of the present invention, the lithium-ion silicon negative electrode battery biopolymer binder includes the following component raw materials: by mass percentage, 10% guar gum, 10% gum arabic, 50% polyacrylic acid, and 30% deionized water.
[0010] Furthermore, in an embodiment of the present invention, the lithium-ion silicon negative electrode battery biopolymer binder includes the following component raw materials: 20% guar gum, 20% gum arabic, 40% polyacrylic acid, and 20% deionized water in percentage by mass.
[0011] Furthermore, in an embodiment of the present invention, the lithium-ion silicon negative electrode battery biopolymer binder includes the following component raw materials: 30% guar gum, 50% polyacrylic acid, and 20% deionized water in percentage by mass.
[0012] Furthermore, in an embodiment of the present invention, the biopolymer binder for lithium-ion silicon negative electrode batteries includes the following raw materials: 30% gum arabic, 50% polyacrylic acid, and 20% deionized water in percentage by mass.
[0013] Furthermore, the lithium-ion silicon negative electrode battery biopolymer binder is used in the silicon negative electrode.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the biopolymer guar gum and gum arabic are binders composed of polysaccharides and glycoproteins and have dual functional groups, and their molecular segments contain a large number of functional groups (-OH, -COOH, -NH2). Among them, -COOH and -NH2 can form hydrogen bonds with the hydroxylated silicon surface and anchor on the silicon surface, which is conducive to maintaining the integrity of the silicon negative electrode, avoiding the shedding and separation of silicon, and preventing the silicon negative electrode from pulverizing and breaking during the lithium ion embedding / ejection process; -OH can improve the bonding strength and mechanical properties of the silicon negative electrode and inhibit the volume change of the silicon negative electrode. In addition, the dual functional groups of guar gum and gum arabic can maintain a strong chemical bond to give the silicon negative electrode excellent flexibility, thereby overcoming the expansion of the silicon negative electrode during the charging and discharging process, and achieving the effect of maintaining the stable electrochemical performance of the lithium ion battery for a long time. DETAILED DESCRIPTION
[0015] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] It should be noted that the purchasers of all raw materials involved in the present invention include, without any special restrictions, the following examples: Guar gum was purchased from Qingdao Wanyuanshan Biotechnology Co., Ltd.; Gum arabic was purchased from Shandong Kuoyi Biotechnology Co., Ltd.; Silicon nanoparticles were purchased from Shenzhen Better New Energy Materials Co., Ltd.
[0017] Conductive agent Super-p was purchased from Tianjin Youmeng Chemical Technology Co., Ltd.; Catechol was purchased from Hunan Daochen Technology Co., Ltd.; Ammonium persulfate, analytical grade, was purchased from Alfa Aesar (China) Chemical Co., Ltd.
[0018] Example 1: A method for preparing a biopolymer binder for lithium-ion silicon negative electrode batteries: 10 parts of guar gum, 10 parts of gum arabic, 50 parts of polyacrylic acid and 30 parts of deionized water were added into a reactor, stirred at a speed of 200 r / min for 30 minutes, heated to 70°C, and then 0.5 parts of ammonium persulfate were added to initiate the reaction for 9 hours to prepare a biopolymer binder for lithium-ion silicon negative electrode batteries.
[0019] Based on Example 1, Examples 2 to 4 and Comparative Examples 1 to 2 are provided: Among them, except for the different amounts of guar gum, gum arabic, polyacrylic acid and deionized water in Examples 2 to 4, other processes remain unchanged; in Comparative Example 1, guar gum and gum arabic are not added, and only polyacrylic acid is used as a binder; in Comparative Example 2, guar gum and gum arabic are not added, and catechol is used instead, and other processes remain unchanged.
[0020] The raw material component parameters of the binders obtained in Examples 1 to 4 and Comparative Examples 1 to 2 are shown in Table 1 below: Table 1
[0021] Performance test: The performance test was performed on the binders prepared in Examples 1 to 4 and Comparative Examples 1 to 2. The specific test method was as follows: silicon nanoparticles and conductive agent Super-p were mixed with the binders prepared in Examples 1 to 4 and Comparative Examples 1 to 2 in a mass ratio of 3:1:1, and stirred in a homogenizer for 10 minutes to obtain slurry; (2) the slurry corresponding to each example was coated on a copper foil of the same specification with a coating thickness of 100 μm, and dried at 60°C for 24 hours to obtain a silicon negative electrode sheet, ensuring that the average loading amount of the active substance in the silicon negative electrode sheet was 0.8 mg / cm 2 ; (3) The silicon negative electrode sheet was cut into a circular silicon negative electrode sheet with a diameter of 14 nm by a punching machine, and the silicon negative electrode sheet and the lithium iron phosphate positive electrode sheet were assembled into a button half-cell, and a LiPF6 electrolyte with a concentration of 1.08 mol / kg was injected into the button half-cell to obtain a button battery. Finally, at 25°C, a peeling force test, a swelling rate test, and a charge and discharge cycle test of 100 cycles at a current density of 4A / g were performed. The specific test methods are as follows: 1. Peel force test: (1) Stick one side of the 3M-VHB double-sided tape on the negative electrode of the button battery and the other side on the stainless steel plate. The three are integrated into one. (2) Fix the whole onto the two fixtures of the peel force tester and perform a 180° peel test at a speed of 10 mm / min until the negative electrode sheet is completely peeled off. 2. Swelling rate test: (1) Use a micrometer to measure the thickness of the button battery and record it as h0; (2) Fully charge the button battery, place it in a constant temperature box, charge and discharge it 500 times at a current density of 4A / g, take it out and measure its thickness with a micrometer and record it as h1; (3) Calculate the swelling rate of the battery after 500 cycles of charge and discharge according to the formula: swelling rate = (h1-h0) / h1×100%.
[0022] The specific test results are shown in Table 2 below: Table 2
[0023] Result analysis: It can be seen from Examples 3 to 4 in Table 2 above that guar gum and gum arabic can have a positive effect on the biopolymer binder for lithium-ion silicon negative electrode batteries, and can significantly improve the peeling force, swelling rate and capacity of the battery; compared with Examples 1 to 2, it can be seen that the lithium-ion silicon negative electrode battery biopolymer binder prepared by adding two components at the same time has a better effect on improving battery performance than the biopolymer binder prepared by adding a certain component alone; in particular, when the mass ratio of guar gum, gum arabic, polyacrylic acid and deionized water is 1:1:5:3, the electrochemical performance of the battery reaches the best (ie, Example 1 is the best example). Compared with the embodiments, guar gum and gum arabic were not added in Comparative Examples 1 and 2, and the electrochemical performance of the finally assembled battery was much worse, especially in Comparative Example 1, only polyacrylic acid was used as a binder, and the electrochemical performance of the final battery was the worst; in Comparative Example 2, after polyacrylic acid was mixed with catechol, the catechol formed hydrogen bonds with silicon nanoparticles and oxygen-containing functional groups or oxide layers on the surface of the copper foil, and the battery capacity was significantly improved, but the peeling force and swelling rate were not significantly improved.
[0024] In summary, the biopolymer binder for lithium-ion silicon negative electrode batteries prepared by the present invention can improve and enhance the flexibility of the silicon negative electrode, thereby overcoming the volume expansion of the silicon negative electrode during the charge and discharge process, thereby achieving the effect of maintaining the stability of the electrochemical performance of the lithium-ion battery for a long time.
[0025] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a biopolymer binder for a lithium-ion silicon negative electrode battery, characterized in that: The lithium-ion silicon negative electrode battery biopolymer binder comprises the following raw materials: by mass percentage, 0-30% guar gum, 0-30% gum arabic, 40-50% polyacrylic acid, and 20-30% deionized water.
2. The method for preparing a biopolymer binder for lithium-ion silicon negative electrode batteries according to claim 1, characterized in that: The lithium-ion silicon negative electrode battery biopolymer binder comprises the following component raw materials: 10% guar gum, 10% gum arabic, 50% polyacrylic acid, and 30% deionized water, calculated by mass percentage.
3. The method for preparing a biopolymer binder for lithium-ion silicon negative electrode batteries according to claim 1, characterized in that: Specifically, guar gum, gum arabic, polyacrylic acid and deionized water are added into a reactor, heated to 60-75°C, and ammonium persulfate is added to initiate the reaction for 6-12 hours to prepare a biopolymer binder for lithium-ion silicon negative electrode batteries.
4. A biopolymer binder for lithium-ion silicon negative electrode batteries prepared according to the method for preparing a biopolymer binder for lithium-ion silicon negative electrode batteries according to any one of claims 1 to 3.
5. Use of the biopolymer binder for lithium-ion silicon negative electrode batteries according to claim 4 in silicon negative electrodes.
Citation Information
Cited By
Lithium ion battery silicon negative electrode binder and preparation method and application thereof
CN120041111A
Cross-linked silicon-based negative electrode binder and method for preparing the same
CN122958953A