Negative electrode binder, negative electrode plate and battery

By using a binder composition of hydroxyl or carboxylation modified liquid metal with a variety of structural units in lithium-ion batteries, the problem of both rigidity and flexibility of the adhesive is solved, significantly reducing the battery impedance and improving the lithium-ion battery performance.

CN118879245AInactive Publication Date: 2024-11-01SHENZHEN HAODYNE TECH CO LTD

Patent Information

Application Number
CN202411383308.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing lithium-ion battery adhesives cannot take into account both rigidity and flexibility, cannot effectively reduce battery impedance, and cannot meet the high-performance needs of high-volume-changing negative electrode materials during charging and discharging.

Method used

Using a binder composition containing a liquid metal material with hydroxyl or carboxylation modification and a binder group, hydroxyl, nitrile, and acrylate structural units, a new negative electrode binder is formed by blending, thereby improving conductivity and taking into account the adhesive. The mechanical properties of the assembled agent reduce the internal resistance of the battery.

Benefits of technology

It significantly improves the conductivity and mechanical properties of the negative electrode adhesive, enhances the capacity and peel strength of the battery, solves the mechanical stress release problem caused by changes in the negative electrode volume, and improves the overall performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a negative electrode binder, a negative electrode plate and a battery. The negative electrode binder comprises a binder composition and a liquid metal material, the binder composition comprises a polymer, and the polymer comprises a carboxyl structural unit, a hydroxyl structural unit, a nitrile structural unit and an acrylate structural unit; the liquid metal material is a hydroxyl or carboxylation modified liquid metal material. According to the invention, the hydroxyl or carboxylation modified liquid metal material and the binder composition containing the carboxyl structural unit, the hydroxyl structural unit, the nitrile structural unit and the acrylate structural unit are blended to form the new negative electrode binder; by adding the hydroxyl or carboxylation modified liquid metal, the conductivity of the negative electrode binder is greatly improved, the binder has a unique response mechanism to current, the rigidity and flexibility of the binder can be considered, and the mechanical property of the binder is comprehensively improved; the internal resistance of the battery is greatly reduced, and the capacity is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a negative electrode binder, a negative electrode sheet and a battery. Background Art

[0002] Lithium-ion batteries have the advantages of high operating voltage, wide operating temperature range, high energy density, high output power, no memory effect and long cycle life. They have been widely used not only in the field of 3C digital products such as mobile phones and laptops, but also in the field of new energy vehicles and large-scale energy storage. Lithium-ion batteries are generally composed of positive electrodes, negative electrodes, separators and electrolytes; the negative electrode includes a negative electrode active material layer, which is obtained by coating the negative electrode slurry on the surface of the negative electrode current collector, drying, rolling and cutting. The negative electrode slurry includes negative electrode active material, conductive agent and negative electrode binder. Binder is an auxiliary additive in electrode materials. Its main function is to bind active materials with active materials, active materials with conductive agents, and active materials with current collectors to form an electrode as a whole. At the same time, the binder will also help to form a stable SEI layer to a certain extent. As a component in the electrode material, although the binder is used in very small amounts, it plays a very important role in maintaining the mechanical integrity and conductive network integrity of the electrode. Research on binders in the prior art is also increasing.

[0003] The Chinese invention patent with publication number CN111430712A discloses a method for preparing a silicon-based negative electrode binder for lithium-ion batteries. An acrylic monomer, a crosslinking agent, and an initiator are mixed, and crosslinked and polymerized under heat initiation to form a crosslinked PAA; a grafting modifier is added to the crosslinked PAA, and the mixture is stirred and heated. The binder prepared by this method is easily soluble in water and ethanol, and exists in the form of a hydrogel, which is environmentally friendly. Electrochemical tests have shown that the binder has excellent cycle performance as a lithium-ion silicon-based negative electrode binder. However, the above technology only emphasizes the improvement of the negative electrode performance by the mechanical strength of the material, and does not pay attention to the role of improving the conductive properties of the binder in reducing battery impedance.

[0004] The Chinese invention patent with publication number CN117050679A discloses a silicon negative electrode binder with a chemical / ionic / hydrogen bond triple cross-linked network and a preparation method. The hydroxyl groups of β-CD and the hydroxyl groups on the Si surface react with each other, and a hydrogen bond cross-linked network is formed by the reaction between β-CD, CA, ALG, active material Si and copper current collector. The in-situ esterification reaction occurs between β-CD, CA, ALG and the Si surface to form a chemical cross-linked network, and the carboxyl groups generated by the hydrolysis of the cross-linked ester groups react with the carboxyl groups of CA and the CuO formed by partial oxidation on the copper current collector to form a carboxylate copper complex and diffuse to the electrode to form an ionic cross-linked network, thereby forming a triple cross-linked binder with a three-dimensional network structure. However, the above technology cannot take into account both the rigidity and flexibility of the binder, and cannot meet the demand for high-performance negative electrode binders for high-volume-change negative electrode materials during the charge and discharge process.

[0005] Therefore, it is of great significance to develop an adhesive that can take into account both the rigidity and flexibility of the adhesive and can effectively reduce the battery impedance. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a negative electrode binder, a negative electrode material and a battery.

[0007] The present invention adopts the following technical solutions: In a first aspect, the present invention provides a negative electrode binder, comprising a binder composition and a liquid metal material, wherein the binder composition comprises a polymer, and the polymer comprises a carboxyl structural unit, a hydroxyl structural unit, a nitrile structural unit, and an acrylate structural unit; and the liquid metal material is a hydroxyl or carboxyl modified liquid metal material.

[0008] Furthermore, the mass ratio of the binder composition to the liquid metal material is 1:(0.2-0.6).

[0009] Furthermore, the weight average molecular weight of the polymer is 10w-800w, and the PDI is 0.5-3.

[0010] Furthermore, in the polymer, the mass ratio of the carboxyl structural unit, the hydroxyl structural unit, the nitrile structural unit, and the acrylate structural unit is 1:(0.2-0.8):(0.05-0.4):(0.05-0.4).

[0011] Furthermore, the carboxyl structural unit includes one or more of an acrylic acid structural unit, a maleic anhydride structural unit, an itaconic acid structural unit, and a methacrylic acid structural unit; The hydroxyl structural unit includes one or more of a polyvinyl alcohol structural unit, a dopamine structural unit, a methacryloyl dopamine structural unit, a trimethylol methacrylamide structural unit, a phenyl glycidyl ether acrylic acid structural unit, a 2-hydroxy-3-phenoxypropyl acrylate structural unit, a polyethylene glycol monomethacrylate structural unit, and a hydroxyethyl methacrylate structural unit; The nitrile structural unit includes one or more of an acrylonitrile structural unit, a styrene nitrile structural unit, a methacrylonitrile structural unit, a 2-cyano-3-ethoxyethyl acrylate structural unit, an ethyl cyanoacrylate structural unit, a tetrakis(4-cyanophenyl)ethylene structural unit, a 2-cyano-5-norbornene structural unit, and a benzylmalononitrile structural unit; The acrylic acid ester structural unit includes one or more of a methacrylate structural unit, a methyl acrylate structural unit, an ethyl acrylate structural unit, a propyl acrylate structural unit, a butyl acrylate structural unit, an isooctyl acrylate structural unit, a hydroxypropyl acrylate structural unit, a 3,3-ethyl dimethacrylate structural unit, an ethylene glycol dimethacrylate structural unit, and a polyethylene glycol dimethacrylate structural unit.

[0012] Furthermore, the volume average particle size of the liquid metal material is less than 200 nm.

[0013] Furthermore, the liquid metal material includes at least one of a gallium-indium alloy and a gallium-indium-tin alloy; the mass ratio of gallium to indium in the gallium-indium alloy is (0.85-0.9):(0.1-0.15); the mass ratio of gallium, indium and tin in the gallium-indium-tin alloy is (0.6-0.7):(0.2-0.25):(0.1-0.15).

[0014] Furthermore, the weight percentage of hydroxyl groups or carboxyl groups in the liquid metal material is 0.01‰-0.1‰.

[0015] In a second aspect, the present invention provides a negative electrode sheet, comprising the negative electrode binder.

[0016] In a third aspect, the present invention provides a battery, comprising the negative electrode sheet described above.

[0017] The negative electrode binder of the present invention is formed by blending a hydroxyl or carboxyl modified liquid metal material with a binder composition comprising a carboxyl structural unit, a hydroxyl structural unit, a nitrile structural unit, and an acrylate structural unit. The addition of the hydroxyl or carboxyl modified liquid metal greatly improves the conductivity of the negative electrode binder, and the binder has a unique response mechanism to current, which can take into account the rigidity and flexibility of the binder and comprehensively improve the mechanical properties of the binder; the internal resistance of the battery is greatly reduced, and the capacity is improved. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.

[0019] The present invention provides a negative electrode binder, comprising a binder composition and a liquid metal material, wherein the binder composition comprises a polymer, and the polymer comprises a carboxyl structural unit, a hydroxyl structural unit, a nitrile structural unit, and an acrylate structural unit; and the liquid metal material is a hydroxyl or carboxyl modified liquid metal material.

[0020] As is well known in the art, the above-mentioned carboxyl structural units are obtained by polymerizing monomers containing carboxyl functional groups. Similarly, hydroxyl structural units are obtained by polymerizing monomers containing hydroxyl functional groups, nitrile structural units are obtained by polymerizing monomers containing cyano functional groups, and acrylate structural units are obtained by polymerizing monomers containing acrylate functional groups. Similarly, in the polymer, the mass ratio of carboxyl structural units, hydroxyl structural units, nitrile structural units, and acrylate structural units is the ratio of the added amounts of monomers containing carboxyl functional groups, monomers containing hydroxyl functional groups, monomers containing cyano functional groups, and monomers containing acrylate functional groups used in preparing the polymer.

[0021] The negative electrode binder of the present invention is formed by blending a hydroxyl or carboxyl modified liquid metal with a binder composition comprising a carboxyl structural unit, a hydroxyl structural unit, a nitrile structural unit, and an acrylate structural unit. The addition of the liquid metal greatly improves the conductivity of the negative electrode binder, and the binder has a unique response mechanism to current, which can take into account the rigidity and flexibility of the binder and comprehensively improve the mechanical properties of the binder; the internal resistance of the battery is greatly reduced, and the capacity is improved.

[0022] Specifically, when the battery is charged, the liquid metal in the binder can be embedded with lithium and solidified, which greatly enhances the rigidity of the binder and effectively inhibits the failure of the binder due to insufficient rigidity and the large volume change of the silicon negative electrode during charging; when the battery is discharged, the solidified liquid metal can be de-lithiated and liquefied, which greatly enhances the flexibility of the negative electrode binder and effectively solves the problem of electrode powderization caused by the failure to release the mechanical stress caused by the volume change of the negative electrode in time. At the same time, the liquid metal modified with hydroxyl or carboxyl groups improves the compatibility of the liquid metal with the binder, which is conducive to the uniform dispersion of the liquid metal in the binder.

[0023] As an embodiment of the present invention, the mass ratio of the binder composition and the liquid metal material is 1:(0.2-0.6). Specifically, the mass ratio of the binder composition and the liquid metal material is 1:0.2, 1:0.25, 1:0.3, 1:0.35, 1:0.4, 1:0.45, 1:0.5, 1:0.55, 1:0.6 or a range consisting of any two of these values. If the mass ratio of the binder composition and the liquid metal material is lower than 1:0.2, the improvement of the rigidity and flexibility of the negative electrode binder and the current response effect are limited; if the mass ratio of the binder composition and the liquid metal material is higher than 1:0.6, the liquid metal has poor dispersibility in the binder composition, and the bonding network of the binder will be destroyed during the battery charging and discharging process, affecting the conductive properties of the battery.

[0024] As an embodiment of the present invention, the preparation of the negative electrode binder includes: blending the binder composition and the liquid metal material in a mass ratio of 1:(0.2-0.6), stirring at a rate of 100-1500 rpm, and stirring for 2-10 hours to obtain the negative electrode binder.

[0025] As an embodiment of the present invention, the weight average molecular weight of the polymer is 10w-800w, and the PDI is 0.5-3. Preferably, the weight average molecular weight of the polymer is 50w-300w. If the molecular weight of the polymer is greater than 800w, the polymer viscosity is high and the liquid metal material is not easy to disperse; if the molecular weight of the polymer is less than 10w, it cannot play an effective bonding role, affecting the mechanical strength of the pole piece.

[0026] As an embodiment of the present invention, in the polymer, the mass ratio of carboxyl structural units, hydroxyl structural units, nitrile structural units, and acrylate structural units is 1:(0.2-0.8):(0.05-0.4):(0.05-0.4). That is, the polymer is obtained by polymerizing carboxyl functional group-containing monomers, hydroxyl functional group-containing monomers, nitrile monomers, and acrylate monomers in a mass ratio of 1:(0.2-0.8):(0.05-0.4):(0.05-0.4).

[0027] As an embodiment of the present invention, the carboxyl structural unit includes one or more of an acrylic acid structural unit, a maleic anhydride structural unit, an itaconic acid structural unit, and a methacrylic acid structural unit; The hydroxyl structural unit includes one or more of a polyvinyl alcohol structural unit, a dopamine structural unit, a methacryloyl dopamine structural unit, a trimethylol methacrylamide structural unit, a phenyl glycidyl ether acrylic acid structural unit, a 2-hydroxy-3-phenoxypropyl acrylate structural unit, a polyethylene glycol monomethacrylate structural unit, and a hydroxyethyl methacrylate structural unit; The nitrile structural unit includes one or more of an acrylonitrile structural unit, a styrene nitrile structural unit, a methacrylonitrile structural unit, a 2-cyano-3-ethoxyethyl acrylate structural unit, an ethyl cyanoacrylate structural unit, a tetrakis(4-cyanophenyl)ethylene structural unit, a 2-cyano-5-norbornene structural unit, and a benzylmalononitrile structural unit; The acrylic acid ester structural unit includes one or more of a methacrylate structural unit, a methyl acrylate structural unit, an ethyl acrylate structural unit, a propyl acrylate structural unit, a butyl acrylate structural unit, an isooctyl acrylate structural unit, a hydroxypropyl acrylate structural unit, a 3,3-ethyl dimethacrylate structural unit, an ethylene glycol dimethacrylate structural unit, and a polyethylene glycol dimethacrylate structural unit.

[0028] As an embodiment of the present invention, the carboxyl functional group-containing monomer includes one or more of acrylic acid, maleic anhydride, itaconic acid, and methacrylic acid; The hydroxyl functional group-containing monomer includes one or more of polyvinyl alcohol, dopamine, methacryloyl dopamine, trimethylol methacrylamide, phenyl glycidyl ether acrylic acid, 2-hydroxy-3-phenoxypropyl acrylate, polyethylene glycol monomethacrylate, and hydroxyethyl methacrylate; The nitrile monomer includes one or more of acrylonitrile, styrene nitrile, methacrylonitrile, 2-cyano-3-ethoxyethyl acrylate, ethyl cyanoacrylate, tetrakis(4-cyanophenyl)ethylene, 2-cyano-5-norbornene, and benzylmalononitrile; The acrylate-based monomer includes one or more of methacrylate, methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, isooctyl acrylate, hydroxypropyl acrylate, 3,3-ethyl dimethacrylate, ethylene glycol dimethacrylate, and polyethylene glycol dimethacrylate.

[0029] As an embodiment of the present invention, the synthesis method of the adhesive composition is: synthesizing a polymer adhesive by copolymerizing and grafting carboxyl functional group-containing monomers, hydroxyl functional group-containing monomers, nitrile monomers, and acrylate monomers in a mass ratio of 1:(0.2-0.8):(0.05-0.4):(0.05-0.4), and then purifying by phase inversion method and dialysis method to obtain the adhesive composition.

[0030] As an embodiment of the present invention, the volume average particle size of the liquid metal material is less than 200nm. Specifically, the particle size of the liquid metal material is 5nm, 10nm, 20nm, 30nm, 40nm, 50nm, 70nm, 80nm, 100nm, 120nm, 150nm, 160nm, 175nm, 200nm or a range consisting of any two of these values; preferably, the volume average particle size of the liquid metal material is 50-200nm. If the volume average particle size of the liquid metal material is greater than 200nm, the mechanical properties of the binder will fail. Since the present invention is a nano-scale liquid metal material, other groups except hydroxyl or carboxyl cannot be effectively modified.

[0031] The weight percentage of hydroxyl or carboxyl groups in the liquid metal material is 0.01‰-0.1‰. If the weight percentage of hydroxyl or carboxyl groups in the liquid metal material is less than 0.01‰, it will affect the dispersibility of the liquid metal in the binder composition, causing the battery to destroy the bonding network of the binder during the charge and discharge process, affecting the conductivity of the battery; if the weight percentage of hydroxyl or carboxyl groups in the liquid metal material is higher than 0.1‰, it will affect the lithium ion deintercalation of the liquid metal, resulting in limited improvement of the rigidity and flexibility of the negative electrode binder and the current response effect of the liquid metal.

[0032] As an embodiment of the present invention, the liquid metal material includes at least one of a gallium-indium alloy and a gallium-indium-tin alloy; Specifically, the mass ratio of gallium to indium in the gallium-indium alloy is (0.85-0.9):(0.1-0.15); more specifically, the mass ratio of gallium to indium in the gallium-indium alloy is 0.85:0.15, 0.86:0.14, 0.87:0.13, 0.88:0.12, 0.89:0.11, 0.9:0.1 or a range consisting of any two of these values.

[0033] Specifically, the mass ratio of gallium, indium and tin in the gallium-indium-tin alloy is (0.6-0.7):(0.2-0.25):(0.1-0.15); more specifically, the mass ratio of gallium, indium and tin in the gallium-indium-tin alloy is 0.6:0.25:0.15, 0.62:0.21:0.12, 0.65:0.22:0.13, 0.67:0.23:0.1, 0.7:0.2:0.1 or a range consisting of any two of these values.

[0034] As an embodiment of the present invention, the preparation method of the hydroxyl or carboxyl liquid metal material is as follows: subjecting the gallium-indium alloy or gallium-indium-tin alloy to constant temperature ultrasound at 25°C for 2 to 10 hours to hydroxyl or carboxyl modification of the liquid metal to obtain a hydroxyl or carboxyl modified liquid metal solution. The solvent used in the liquid metal solution is any one of ethanol, acetone, and water, and the solid content of the liquid metal in the solution is 10 to 45%.

[0035] The present invention also provides a negative electrode sheet, the negative electrode sheet includes the above-mentioned negative electrode binder. The negative electrode sheet also includes a negative electrode active material and a conductive agent. The conductive agent includes one or more of conductive carbon black, conductive carbon balls, conductive graphite, conductive carbon fibers, carbon nanotubes, graphene or reduced graphene oxide. The negative electrode active material includes any one of graphite, silicon negative electrode, and silicon-carbon negative electrode.

[0036] The present invention also provides a battery, the battery comprising the above-mentioned negative electrode sheet, the battery also comprising a positive electrode sheet and an electrolyte.

[0037] The present invention will be further described below in conjunction with specific embodiments.

[0038] Example 1

[0039] 1) Preparation of negative electrode binder In this embodiment, the negative electrode binder includes a binder composition and a gallium indium hydroxylate alloy in a mass ratio of 1:0.4.

[0040] The preparation method comprises: (1) Hydroxylated gallium-indium alloy: Gallium metal and indium metal were mixed in a mass ratio of 0.87:0.13 and added to an aqueous solution. The liquid metal was subjected to constant temperature ultrasound at 25°C for 8 hours to undergo hydroxylation modification. The solid content of the liquid metal solution was 25%, and the particle size of the liquid metal was 100 nm.

[0041] (2) Binder composition: Methacrylic acid, methacryloyl dopamine, methacrylonitrile and ethyl 3,3-dimethacrylate were free radical copolymerized in a mass ratio of 1:0.6:0.2:0.4 to obtain a poly(methacrylic acid-co-methacryloyl dopamine-co-methacrylonitrile-co-ethyl 3,3-dimethacrylate) multi-block copolymer. The primary product was dialyzed using a dialysis bag with a molecular weight cutoff specification of 20K to obtain a polymer binder. The polymer molecular weight was 300±50w and the PDI was 1±0.2.

[0042] (3) Negative electrode binder: The binder composition and the gallium indium hydroxylate alloy were blended at a mass ratio of 1:0.4, with a stirring rate of 500 rpm and a stirring time of 8 h to obtain a negative electrode binder.

[0043] 2) Preparation of negative electrode The negative electrode active material silicon negative electrode, conductive carbon black Super-P, and negative electrode binder are mixed in a mass ratio of 97:1:2, and then dispersed in deionized water to obtain negative electrode slurry. The slurry is coated on both sides of the copper foil, dried, rolled and vacuum dried, and the nickel lead wire is welded with an ultrasonic welder to obtain the negative electrode sheet.

[0044] 3) Preparation of positive electrode NCM811, conductive carbon black Super-P and binder polyvinylidene fluoride (PVDF) were mixed evenly in a mass ratio of 96:2:2, and then dispersed in N-methyl-2-pyrrolidone (NMP) to obtain a positive electrode slurry. The slurry was evenly coated on both sides of the aluminum foil, dried, rolled and vacuum dried to obtain a positive electrode material layer, and an aluminum lead wire was welded with an ultrasonic welder to obtain a positive electrode sheet.

[0045] 4) Preparation of electrolyte: Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in a mass ratio of 1:1, and then lithium hexafluorophosphate (LiPF6) was added to a molar concentration of 1.0 mol / L.

[0046] 5) Battery Assembly: A three-layer separator with a thickness of 20 μm is placed between the positive plate and the negative plate, and then the positive plate, the negative plate and the separator are assembled into a laminated soft-pack battery cell; the electrolyte is injected into the battery cell, which is vacuum-sealed and left to rest for 72 hours.

[0047] Example 2

[0048] Most of the steps of Example 2 are the same as those of Example 1, except that carboxylated gallium-indium alloy is used in the preparation of the negative electrode binder.

[0049] Example 3

[0050] Most of the steps of Example 3 are the same as those of Example 1, except that a hydroxylated gallium indium tin alloy is used in the preparation of the negative electrode binder. Specifically, the mass ratio of metal gallium, metal indium and metal tin is 0.65:0.25:0.1.

[0051] Example 4

[0052] Most of the steps of Example 4 are the same as those of Example 1, except that the binder composition is different in the preparation of the negative electrode binder, as follows: The binder composition in Example 4 is: maleic anhydride, trimethylol methacrylamide, styrene nitrile and ethyl 3,3-dimethacrylate are free radical copolymerized in a mass ratio of 1:0.8:0.35:0.15 to obtain a poly(maleic anhydride-co-trimethylol methacrylamide-co-styrene nitrile-co-ethyl 3,3-dimethacrylate) multi-block copolymer.

[0053] Example 5

[0054] Most of the steps of Example 5 are the same as those of Example 1, except that in the preparation of the negative electrode binder, the binder composition is different, as follows: The adhesive composition in Example 5 is: acrylic acid, phenyl glycidyl ether acrylic acid, tetrakis (4-cyanophenyl) ethylene and methacrylate are copolymerized by free radicals in a mass ratio of 1:0.2:0.05:0.05 to obtain a poly (methacrylic acid-co-methacryloyl dopamine-co-methacrylonitrile-co-3,3-dimethacrylate) multi-block copolymer.

[0055] Example 6

[0056] Most of the steps of Example 6 are the same as those of Example 1, except that, in the preparation of the negative electrode binder, the negative electrode binder includes a binder composition and a gallium indium hydroxylate alloy in a mass ratio of 1:0.2.

[0057] Example 7

[0058] Most of the steps of Example 7 are the same as those of Example 1, except that, in the preparation of the negative electrode binder, the negative electrode binder includes a binder composition and a gallium indium hydroxylate alloy in a mass ratio of 1:0.6.

[0059] Example 8

[0060] Most of the steps of Example 8 are the same as those of Example 1, except that, in the preparation of the negative electrode binder, the negative electrode binder includes a binder composition and a gallium indium hydroxylate alloy in a mass ratio of 1:0.1.

[0061] Example 9

[0062] Most of the steps of Example 9 are the same as those of Example 1, except that, in the preparation of the negative electrode binder, the negative electrode binder includes a binder composition and a gallium indium hydroxylate alloy in a mass ratio of 1:0.7.

[0063] Comparative Example 1 Most of the steps of Comparative Example 1 are the same as those of Example 1, except that polyacrylic acid PAA binder (molecular weight of 100-300w) is used as the negative electrode binder.

[0064] Comparative Example 2 Most of the steps of Comparative Example 2 are the same as those of Example 1, except that polyacrylamide (PAM) binder (molecular weight of 100-300w) is used as the negative electrode binder.

[0065] Comparative Example 3 Comparative Example 3 has most of the same steps as Example 1, except that the liquid metal is not hydroxylated, specifically: In the preparation of the negative electrode binder, the negative electrode binder includes a binder composition and a gallium-indium alloy in a mass ratio of 1:0.4.

[0066] The negative electrode sheets and lithium-ion batteries prepared in the above examples and comparative examples were subjected to the following performance tests: 1) Negative electrode peel strength test: After the negative electrode sheet is compacted, a tensile testing machine is used to measure the peel strength of the negative electrode sheet. The test method refers to GB2792-2014.

[0067] 2) Rate performance test Let the soft-pack battery stand until the temperature reaches 25℃±2℃, charge to 4.35V at 1C constant current and constant voltage, with a cut-off current of 0.05C; discharge to 2.75V at 1C constant current, and record the discharge capacity; repeat the cycle for 3 weeks, and take the discharge capacity in the third week as the 1C discharge benchmark capacity; charge to 4.35V at 1C constant current and constant voltage, with a cut-off current of 0.05C; discharge to 2.75V at 2C current, record the discharge capacity, and calculate the 2C discharge capacity retention rate.

[0068] The test results are shown in Table 1.

[0069] Table 1 Group Negative electrode peel strength (N / m) 2C discharge capacity retention rate (%) Example 1 9.25 98.17 Example 2 9.34 98.78 Example 3 9.29 98.35 Example 4 9.15 97.99 Example 5 9.26 98.20 Example 6 8.36 97.01 Example 7 8.23 96.11 Example 8 7.98 95.89 Example 9 8.15 96.25 Comparative Example 1 7.55 80.03 Comparative Example 2 6.92 81.24 Comparative Example 3 4.31 78.64 It can be seen from the test results of Examples 1-9 and Comparative Examples 1-3 in Table 1 that the negative electrode binder of the present invention enhances the rigidity and flexibility of the negative electrode binder through the action of the liquid metal material modified by hydroxyl or carboxyl and the binder composition, so that the negative electrode sheet of the present invention has a higher peel strength, and the prepared lithium ion battery has better electrical performance. At the same time, it can be seen from the test results of Examples 1 and 6-9 that when the mass ratio of the binder composition to the liquid metal material is between 1: (0.2-0.6), the performance improvement effect on the negative electrode sheet and the lithium battery is better. It can be seen from the test results of Example 1 and Comparative Examples 1-2 that compared with conventional negative electrode binders, the negative electrode binder of the present invention has excellent comprehensive performance; and it can be seen from the test results of Example 1 and Comparative Example 3 that the liquid metal modified by hydroxyl or carboxyl has better stability of the binder than the unmodified liquid metal, and the corresponding negative electrode sheet has better peel strength and the performance of the lithium battery is also better.

[0070] The present invention is further described above with the aid of specific embodiments. However, it should be understood that the specific description here should not be construed as limiting the essence and scope of the present invention. Various modifications made to the above embodiments by ordinary technicians in the field after reading this specification are all within the scope of protection of the present invention.

Claims

1. A negative electrode binder, characterized in that: The invention comprises a binder composition and a liquid metal material, wherein the binder composition comprises a polymer, and the polymer comprises a carboxyl structural unit, a hydroxyl structural unit, a nitrile structural unit, and an acrylate structural unit; and the liquid metal material is a hydroxyl or carboxyl modified liquid metal material.

2. The negative electrode binder according to claim 1, characterized in that The mass ratio of the binder composition to the liquid metal material is 1:(0.2-0.6).

3. The negative electrode binder according to claim 1, characterized in that The weight average molecular weight of the polymer is 10w-800w, and the PDI is 0.5-3.

4. The negative electrode binder according to claim 1, characterized in that In the polymer, the mass ratio of the carboxyl structural unit, the hydroxyl structural unit, the nitrile structural unit and the acrylate structural unit is 1:(0.2-0.8):(0.05-0.4):(0.05-0.4).

5. The negative electrode binder according to any one of claims 1 to 4, characterized in that: The carboxyl structural unit includes one or more of an acrylic acid structural unit, a maleic anhydride structural unit, an itaconic acid structural unit, and a methacrylic acid structural unit; The hydroxyl structural unit includes one or more of a polyvinyl alcohol structural unit, a dopamine structural unit, a methacryloyl dopamine structural unit, a trimethylol methacrylamide structural unit, a phenyl glycidyl ether acrylic acid structural unit, a 2-hydroxy-3-phenoxypropyl acrylate structural unit, a polyethylene glycol monomethacrylate structural unit, and a hydroxyethyl methacrylate structural unit; The nitrile structural unit includes one or more of an acrylonitrile structural unit, a styrene nitrile structural unit, a methacrylonitrile structural unit, a 2-cyano-3-ethoxyethyl acrylate structural unit, an ethyl cyanoacrylate structural unit, a tetrakis(4-cyanophenyl)ethylene structural unit, a 2-cyano-5-norbornene structural unit, and a benzylmalononitrile structural unit; The acrylic acid ester structural unit includes one or more of a methacrylate structural unit, a methyl acrylate structural unit, an ethyl acrylate structural unit, a propyl acrylate structural unit, a butyl acrylate structural unit, an isooctyl acrylate structural unit, a hydroxypropyl acrylate structural unit, a 3,3-ethyl dimethacrylate structural unit, an ethylene glycol dimethacrylate structural unit, and a polyethylene glycol dimethacrylate structural unit.

6. The negative electrode binder according to claim 1, characterized in that The volume average particle size of the liquid metal material is less than 200 nm.

7. The negative electrode binder according to claim 1, characterized in that The liquid metal material includes at least one of a gallium-indium alloy and a gallium-indium-tin alloy; The mass ratio of gallium to indium in the gallium-indium alloy is (0.85-0.9):(0.1-0.15); and / or, The mass ratio of gallium, indium and tin in the gallium-indium-tin alloy is (0.6-0.7):(0.2-0.25):(0.1-0.15).

8. The negative electrode binder according to claim 1, characterized in that The weight percentage of hydroxyl or carboxyl groups in the liquid metal material is 0.01‰-0.1‰.

9. A negative electrode sheet, characterized in that: The negative electrode sheet comprises the negative electrode binder according to any one of claims 1 to 8.

10. A battery, characterized in that: The battery comprises the negative electrode sheet according to claim 9.

Citation Information

Patent Citations

  • Negative electrode slurry composition and application

    CN114583173A

  • Conductive polyacrylate pressure-sensitive adhesive and preparation method thereof

    CN117551405A

  • Acrylate adhesive composition, acrylate adhesive as well as preparation method and application of acrylate adhesive

    CN118272013A

  • Thermally conductive connection with matrix material and randomly dispersed filler containing liquid metal

    US5445308A

Cited By

  • Specialized hyperbranched network polyacrylic acid resin for silicon-carbon negative electrode, preparation method and application thereof

    CN120209217B