Elastic buffer rubber as well as preparation method and application thereof

Through the combination of polyester polyol and natural rubber, elastic buffer with excellent impact resistance and mold printing effect was prepared, which solved the problem of insufficient impact resistance and mold printing effect in the prior art, and realized electronics The lightweight and cost reduction of the product.

CN118879265APending Publication Date: 2024-11-01HANPIN (KUNSHAN) ELECTRONIC CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411104892.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing elastic buffer glues have problems with insufficient impact resistance and mold printing resistance in electronic products, especially in the case of increasing demand for domestic production and lightweighting, the high cost and potential risks of silicon gels are also a major challenge.

Method used

Elastic buffer glue is prepared using polyester polyols, natural rubbers, isocyanates and other materials. Through polymerization and compounding technology, combined with fillers, dispersants and anti-static agents, products with excellent impact resistance and anti-molding effect are formed. .

Benefits of technology

It realizes the lightness and thinness of electronic products, improves the protection effect of the product when it falls, extends the service life, and reduces cost risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879265A_ABST
    Figure CN118879265A_ABST
Patent Text Reader

Abstract

The invention relates to an elastic buffer rubber and a preparation method and application thereof, and belongs to the field of adhesives, and the elastic buffer rubber is prepared from the following raw materials: polyester polyol, a chain extender, natural rubber, sulfur, an accelerant, stearic acid, acrylic ester, filler, isocyanate, a dispersing agent, a flatting agent, a defoaming agent and an antistatic agent. The elastic buffering rubber has excellent buffering and anti-vibration performance and anti-stamping effect, can protect an electronic product from being easily damaged when the electronic product falls off, and prolongs the service life of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of adhesives, and in particular relates to an elastic buffer adhesive and a preparation method and application thereof. Background Art

[0002] With the advancement of the localization wave and the demand for thinner electronic consumer products, the foam of the original under-screen structure is mostly imported foam, and the thickness is relatively thick. The current trend is to reduce the thickness and achieve localization substitution. At present, the emerging materials on the market are mainly silicone gel, but the cost of silicone gel is high, the mold is obvious, and the silicon contains potential risks.

[0003] Therefore, it is of great application value to develop an elastic buffer rubber product that is light, thin, impact-resistant and anti-mold. Summary of the invention

[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide an elastic buffer adhesive and a preparation method and application thereof, wherein the elastic buffer adhesive has excellent impact resistance and anti-mold printing effects.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] In a first aspect, the present invention provides an elastic buffer glue, the raw materials for preparing the elastic buffer glue include the following components: polyester polyol, chain extender, natural rubber, sulfur, accelerator, stearic acid, acrylate, filler, isocyanate, dispersant, leveling agent, defoaming agent and antistatic agent.

[0007] The present invention prepares polyurethane by polymerizing isocyanate and polyester polyol with good elasticity, and introduces acrylate and natural rubber into the polyurethane for compounding, so as to obtain an elastic buffer rubber with both the viscosity of acrylate and the elasticity of natural rubber and polyester polyol. The elastic buffer rubber is easy to recover when deformed by force, has excellent impact resistance and anti-mold effect, and can meet the application requirements in electronic products.

[0008] Preferably, the polyester polyol comprises poly(1,4-butylene adipate) and / or poly(ethylene adipate).

[0009] Preferably, the chain extender comprises an alcohol chain extender.

[0010] Preferably, the alcohol chain extender includes any one or a combination of at least two of 1,4-butanediol (BDO), 1,6-hexanediol, glycerol, trimethylolpropane, diethylene glycol (DEG), triethylene glycol, neopentyl glycol (NPG), sorbitol or diethylaminoethanol (DEAE).

[0011] Preferably, the accelerator comprises a dithiocarbamate accelerator.

[0012] Illustratively, the dithiocarbamate accelerator includes any one of zinc dibenzyl dithiocarbamate, zinc diethyl dithiocarbamate, zinc diisobutyl dithiocarbamate or sodium dibenzyl dithiocarbamate, or a combination of at least two thereof.

[0013] Preferably, the acrylic acid ester comprises polybutyl acrylate and / or polymethyl acrylate.

[0014] Preferably, the filler comprises a combination of nano carbon powder and inorganic filler.

[0015] Preferably, the inorganic filler comprises any one of MgO, CaO, Al2O3, ZrO2, ZnO, MnO2, AlSiO5, Zr2WO3, CuO·Cr2O3, H2O8P2Zr, β-LiAlSiO4, CuO·Cr2O3 or 2MgO·2Al2O3·5SiO2, or a combination of at least two thereof. Preferably, the particle size of the filler is 5-500 μm, for example, 10 μm, 20 μm, 50 μm, 100 μm, 200 μm, 300 μm, 400 μm, etc.

[0016] Preferably, the isocyanate comprises diphenylmethane diisocyanate (TDI) and / or diphenylmethane diisocyanate (MDI).

[0017] Preferably, the dispersant is prepared by the following method:

[0018] S1) weighing 0.5-1.5 g (e.g., 0.5 g, 0.7 g, 1 g, 1.5 g, etc.) of polyoxyethylene sorbitan monolaurate and mixing with water to prepare 30-40 ml (e.g., 30 ml, 33 ml, 36 ml, 40 ml, etc.) of aqueous solution 1;

[0019] S2) weighing 1.5-7 g (e.g., 1.5 g, 2 g, 3 g, 5 g, 6 g, 7 g, etc.) of an aqueous wetting and dispersing agent and mixing with water to prepare 100-120 ml (e.g., 100 ml, 105 ml, 110 ml, 120 ml, etc.) of aqueous solution 2;

[0020] S3) stirring and mixing aqueous solution 1 and aqueous solution 2 to obtain a mixed solution;

[0021] S4) weighing 15 to 25 g (e.g., 15 g, 17 g, 19 g, 21 g, 25 g, etc.) of graphite and adding it to the mixed solution, stirring for 3 to 6 min (e.g., 3 min, 4 min, 5 min, 6 min, etc.) and then performing ultrasonic emulsification for 12 to 15 min (e.g., 12 min, 13 min, 14 min, 15 min, etc.) to obtain the dispersant.

[0022] Among them, polyoxyethylene sorbitan monolaurate, aqueous wetting and dispersing agent, and graphite are commercially available products. For example, polyoxyethylene sorbitan monolaurate can be selected from polyoxyethylene sorbitan monolaurate (CAS 9005-64-5) produced by Hubei Chengfeng Chemical Co., Ltd., the aqueous wetting and dispersing agent can be selected from Tween 20 produced by Jiangsu Hai'an Petrochemical Plant, and the graphite can be selected from flake graphite produced by Qingdao Mingrun Chenyue Graphite Co., Ltd.

[0023] Preferably, the leveling agent includes any one of polydimethylsiloxane, alkyl-modified organic siloxane, acrylic resin or organic-modified polysiloxane acrylic, or a combination of at least two thereof.

[0024] Preferably, the defoaming agent includes any one of polydimethylsiloxane copolymer, ethylene oxide, propylene oxide or phosphate copolymer, or a combination of at least two thereof.

[0025] Preferably, the antistatic agent includes a polythiophene antistatic agent and / or a carbon nanotube antistatic agent.

[0026] Preferably, the raw materials for preparing the elastic buffer rubber include the following components in parts by weight: 60-80 parts of polyester polyol (for example, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, etc.), 5-30 parts of chain extender (for example, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, 30 parts, etc.), 50-80 parts of natural rubber (for example, 50 parts, 55 parts, 60 parts, 65 parts, 70 parts, 75 parts, 80 parts, etc.), 3-15 parts of sulfur (for example, 3 parts, 5 parts, 7 parts, 10 parts, 13 parts, 15 parts, etc.), 1-10 parts of accelerator (for example, 1 part, 3 parts, 5 parts, 7 parts, 10 parts, etc.), 1-10 parts of stearic acid (for example, 1 part, 3 parts, 5 parts, 7 parts, 10 parts, etc.), 30-70 parts of acrylate (for example, 30 parts, 40 parts, 5 0 parts, 60 parts, 70 parts, etc.), filler 8-16 parts (for example, 8 parts, 10 parts, 12 parts, 14 parts, 16 parts, etc.), isocyanate 20-40 parts (for example, 20 parts, 24 parts, 28 parts, 32 parts, 36 parts, 40 parts, etc.), dispersant 0.1-3 parts (for example, 0.1 parts, 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 3 parts, etc.), leveling agent 0.1 to 3 parts (for example, 0.1 parts, 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 3 parts, etc.), defoaming agent 0.1 to 3 parts (for example, 0.1 parts, 0.3 parts, 0.5 parts, 1 parts, 1.5 parts, 2 parts, 3 parts, etc.), antistatic agent 0.1 to 7 parts (for example, 0.1 parts, 0.5 parts, 1 parts, 2 parts, 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, etc.).

[0027] In a second aspect, the present invention provides a method for preparing the elastic buffer glue as described in the first aspect, the preparation method comprising the following steps:

[0028] 1) mixing polyester polyol, isocyanate, chain extender, part of filler and part of dispersant to obtain component A;

[0029] 2) mixing and reacting natural rubber, sulfur, an accelerator, stearic acid and another portion of a dispersant to obtain component B;

[0030] 3) Component A, component B, acrylate, another portion of filler, leveling agent, defoaming agent and antistatic agent are mixed to obtain the elastic buffer adhesive.

[0031] Preferably, the part of filler in step 1 is 2-35% of the total mass of the filler, for example, it can be 5%, 10%, 15%, 20%, 25%, 30%, etc.

[0032] Preferably, the part of the dispersant in step 1) is 0.1-10% of the total mass of the dispersant, for example, it can be 0.5%, 1%, 2%, 3%, 5%, 8%, etc.

[0033] Preferably, the temperature of the mixed reaction in step 1) is 30-60°C, for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, etc.

[0034] Preferably, the mixing reaction time in step 1) is 3 to 6 hours, for example, 3 hours, 4 hours, 5 hours, 6 hours, etc.

[0035] Preferably, the temperature of the mixed reaction in step 2) is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, etc.

[0036] Preferably, the mixing reaction time in step 2) is 8 to 14 h, for example, 8 h, 9 h, 10 h, 11 h, 12 h, 13 h, 14 h, etc.

[0037] Preferably, the rotation speed of the mixing reaction in step 1) and step 2) is independently 300-700 r / min, for example, 300 r / min, 400 r / min, 500 r / min, 600 r / min, 700 r / min, etc.

[0038] Preferably, the mixing temperature in step 3) is 15-60°C, for example, 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, etc.

[0039] Preferably, the mixing time in step 3) is 20 to 60 min, for example, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0040] Preferably, the mixing speed in step 3) is 1000-1400 r / min, for example, it can be 1000 r / min, 1100 r / min, 1200 r / min, 1300 r / min, 1400 r / min, etc.

[0041] Preferably, the mixing in step 3) further includes filtering.

[0042] Preferably, the preparation method comprises the following steps:

[0043] 1) Mixing polyester polyol, isocyanate, chain extender, part of filler and dispersant at 30-60° C. and 300-700 r / min for 3-6 hours to obtain component A;

[0044] 2) mixing natural rubber, sulfur, accelerator, stearic acid and dispersant at 60-80° C. and 300-700 r / min for 8-14 hours to obtain component B;

[0045] 3) Component A, component B, acrylate, another part of filler, leveling agent, defoamer and antistatic agent are mixed at 15-30° C. and 1000-1400 r / min for 20-60 min, filtered, and the filtrate is taken to obtain the elastic buffer rubber.

[0046] In a third aspect, the present invention provides an elastic buffer adhesive product, the elastic buffer adhesive product comprising a first release layer, an elastic buffer adhesive layer and a base material layer stacked in sequence;

[0047] The elastic buffer rubber layer includes the elastic buffer rubber as described in the first aspect.

[0048] Preferably, the base material layer includes a substrate layer and / or a second release layer.

[0049] Preferably, the substrate layer includes any one of a metal substrate, PET (polyethylene terephthalate), a conductive cloth or a non-woven fabric;

[0050] Preferably, the metal substrate comprises copper foil and / or aluminum foil.

[0051] Preferably, the first release layer and the second release layer are independently selected from any one of a single silicon release film, a double silicon release film, a release paper or a fluorine release film.

[0052] Preferably, the thickness of the release layer is 0.025-0.15 mm, for example, 0.03 mm, 0.05 mm, 0.08 mm, 0.1 mm, 0.12 mm, etc.

[0053] Preferably, the thickness of the elastic buffer rubber layer is 0.01-0.35 mm, for example, it can be 0.03 mm, 0.05 mm, 0.08 mm, 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, etc.

[0054] Preferably, the thickness of the base material layer is 0.01-0.2 mm, for example, 0.03 mm, 0.05 mm, 0.08 mm, 0.1 mm, 0.12 mm, 0.15 mm, 0.18 mm, etc.

[0055] In a fourth aspect, the present invention provides a method for preparing the elastic buffer rubber product according to the third aspect, the preparation method comprising the following steps:

[0056] 1) coating the elastic buffer adhesive described in the first aspect on the surface of the base material layer, and drying and curing the elastic buffer adhesive layer;

[0057] 2) Covering the surface of the elastic buffer adhesive layer with a first release layer to obtain the elastic buffer adhesive product.

[0058] Compared with the prior art, the present invention has the following beneficial effects:

[0059] The elastic buffer rubber product of the present invention has excellent buffering and shock-resistant performance and anti-mold printing effect, realizes the lightness and thinness of electronic products, can protect electronic products from being easily damaged when falling, and improves the service life of products. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 It is a schematic diagram of the structure of an elastic buffer glue product, wherein 1 is a base material layer; 2 is an elastic buffer glue; and 3 is a release layer. DETAILED DESCRIPTION

[0061] For the convenience of understanding the present invention, the present invention lists the following embodiments. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0062] In the following examples, unless otherwise specified, the raw materials used are all common commercially available products that can be directly purchased or prepared using conventional techniques in the art.

[0063] The raw material information used in the specific examples and comparative examples of the present invention is as follows:

[0064] 1) Polyester polyol

[0065] Polybutylene adipate, 1,4-butylene adipate, Shineng Chemical Technology Co., Ltd., PBA1000

[0066] 2) Natural rubber

[0067] Shanghai Sanlian Industrial Co., Ltd., No. 1 standard glue

[0068] 3) Sulfur

[0069] Luoyang Tianzhidao New Materials Co., Ltd., Sulfur powder S-80

[0070] 4) Accelerator

[0071] Zinc dibenzyl dithiocarbamate, MacLean Biochemical Technology Co., Ltd., D836186

[0072] 5) Stearic acid

[0073] Jinan Shuangping Chemical Co., Ltd., Stearic acid 1801

[0074] 6) Acrylate

[0075] Polybutyl acrylate, Kunshan Shimei Chemical Co., Ltd., PS8281

[0076] 7) Filling

[0077] Nano carbon powder, Shanghai Xiaohuang Nano Technology Co., Ltd. High purity nano carbon powder Ultrafine spherical micro carbon powder

[0078] MgO, Ningbo Actmix New Materials Co., Ltd. Actmix MgO-75GE F140

[0079] CaO, Langfang Pengcai Fine Chemical Co., Ltd., 1305-78-8

[0080] Al2O3, Shanghai Maoguo Nanotechnology Co., Ltd., α-phase alumina

[0081] MnO2, Merck Reagent Co., Ltd., 217646

[0082] AlSiO5, Tuoyi New Materials (Guangzhou) Co., Ltd., aluminum silicate powder 325-4000 mesh

[0083] Zr2WO3, Shanghai Dianyang Industrial Co., Ltd.

[0084] 8) Isocyanate

[0085] Isocyanate with 45% solid content, Kunshan Shimei Chemical Co., Ltd., PX2300AM

[0086] 9) Dispersant

[0087] The dispersant is prepared by the following method:

[0088] S1) weighing 1 g of polyoxyethylene sorbitan monolaurate and mixing with water to prepare 35 mL of aqueous solution 1;

[0089] S2) weighing 4.5 g of an aqueous wetting and dispersing agent and mixing it with water to prepare 110 mL of aqueous solution 2;

[0090] S3) stirring and mixing aqueous solution 1 and aqueous solution 2 to obtain a mixed solution;

[0091] S4) weighing 20 g of graphite and adding it to the mixed solution, stirring for 4.5 min and then performing ultrasonic emulsification for 13 min to obtain the dispersant;

[0092] Among them, polyoxyethylene sorbitan monolaurate is polyoxyethylene sorbitan monolaurate (CAS 9005-64-5) from Hubei Chengfeng Chemical Co., Ltd., the aqueous wetting and dispersing agent is Tween 20 from Jiangsu Hai'an Petrochemical Plant, and the graphite is flake graphite from Qingdao Mingrun Chenyue Graphite Co., Ltd.

[0093] 10) Leveling agent

[0094] Polydimethylsiloxane, Shandong Qimin Chemical Technology Co., Ltd.

[0095] Alkyl modified organosiloxane, --Hubei Longsheng Sihai Core Materials Co., Ltd., FJN9803

[0096] Acrylic resin, BASF, HPD 96-E

[0097] Organic modified polysiloxane acrylic acid, Shanghai Longquan Chemical Technology Co., Ltd., OEBNYS-89RE1142

[0098] 11) Defoaming agent

[0099] Ethylene oxide, Beijing Wanjia

[0100] 1,2-Propylene oxide, Jinan Shuangying Chemical Co., Ltd.

[0101] Phosphate copolymer, Zhangjiagang Tianchang New Materials Co., Ltd., TMP

[0102] Polydimethylsiloxane Copolymer, Yizu Elements, Silsurf D212-CG

[0103] 12) Antistatic agent

[0104] Fuxin Technology Co., Ltd., XT-BA002

[0105] 13) Chain Extender

[0106] 1,4-Butanediol (BDO), Jinan Shuangying Chemical Co., Ltd.

[0107] Embodiments 1 to 5

[0108] An elastic buffer rubber, the raw materials for its preparation are shown in Table 1, wherein the units of each component are "parts by weight"

[0109] Table 1

[0110]

[0111]

[0112] The preparation method of the elastic buffer rubber provided in Examples 1 to 3 comprises the following steps:

[0113] 1) polyester polyol, isocyanate, chain extender, 10% of filler and 2% of dispersant were mixed and reacted at 60° C. and 700 r / min for 3 hours to obtain component A;

[0114] 2) mixing natural rubber, sulfur, accelerator, stearic acid and the remaining dispersant at 80° C. and 700 r / min for 8 hours to obtain component B;

[0115] 3) Component A, component B, acrylate, remaining filler, leveling agent, defoamer and antistatic agent are mixed at 30° C. and 1400 r / min for 20 min, filtered, and the filtrate is collected to obtain the elastic buffer rubber.

[0116] The preparation method of the elastic buffer rubber provided in Examples 4 and 5 comprises the following steps:

[0117] 1) polyester polyol, isocyanate, chain extender, 30% of the total filler and 8% of the total dispersant were mixed and reacted at 40° C. and 500 r / min for 5 hours to obtain component A;

[0118] 2) mixing natural rubber, sulfur, accelerator, stearic acid and the remaining dispersant at 70° C. and 500 r / min for 10 hours to obtain component B;

[0119] 3) Component A, component B, acrylate, remaining filler, leveling agent, defoamer and antistatic agent are mixed at 20° C. and 1100 r / min for 40 min, filtered, and the filtrate is collected to obtain the elastic buffer rubber.

[0120] Example 6

[0121] This embodiment provides an elastic buffer rubber and a preparation method thereof, which is different from Embodiment 1 only in that 30 parts of natural rubber are added, and other conditions are the same as those of Embodiment 1.

[0122] Example 7

[0123] This embodiment provides an elastic buffer glue and a preparation method thereof. The difference between this embodiment and embodiment 1 is that 15 parts of acrylate are added, and other conditions are the same as those in embodiment 1.

[0124] Example 8

[0125] This embodiment provides an elastic buffer glue and a preparation method thereof, which is different from Embodiment 1 only in that 50 parts of isocyanate are added, and other conditions are the same as those in Embodiment 1.

[0126] Example 9

[0127] This embodiment provides an elastic buffer glue and a preparation method thereof, which is different from Embodiment 1 only in that an equal amount of nano-carbon powder is replaced by Al2O3, and other conditions are the same as those in Embodiment 1.

[0128] Comparative Example 1

[0129] This comparative example provides an elastic buffer glue and a preparation method thereof, which differs from Example 1 only in that the polyester polyol is replaced by an equal amount of trimethylolpropane polyether polyol (Guangzhou Fufei Chemical Technology Co., Ltd., DL-4000D), and other conditions are the same as those in Example 1.

[0130] Comparative Example 2

[0131] This comparative example provides an elastic buffer rubber and a preparation method thereof, which is different from Example 1 only in that no natural rubber is added, and other conditions are the same as those of Example 1.

[0132] Comparative Example 3

[0133] This comparative example provides an elastic buffer rubber and a preparation method thereof, which differs from Example 1 only in that an equal amount of natural rubber is replaced by styrene-butadiene rubber (Dongguan Shanyi Plastic Chemical Co., Ltd., SBS1475), and other conditions are the same as those in Example 1.

[0134] Comparative Example 4

[0135] This comparative example provides an elastic buffer glue and a preparation method thereof, which is different from Example 1 only in that no acrylate is added, and other conditions are the same as those of Example 1.

[0136] Comparative Example 5

[0137] This comparative example provides an elastic buffer glue and a preparation method thereof, which is different from Example 1 only in that isocyanate and polyester polyol are not added, and other conditions are the same as those in Example 1.

[0138] Application Examples 1 to 9 and Application Comparative Examples 1 to 5

[0139] Provided are an elastic buffer rubber product and a preparation method thereof. The elastic buffer rubber product comprises a release layer (Yangzhou Wanrun Film Co., Ltd., 7906Y), an elastic buffer rubber layer and a base material layer (China Aluminum Shanghai Copper Co., Ltd., C1100, 0.035 mm) stacked in sequence.

[0140] The preparation method of the elastic buffer rubber product comprises the following steps:

[0141] The elastic buffer adhesive prepared in Examples 1 to 9 and Comparative Examples 1 to 5 was coated on the surface of the base material layer, dried and cured at 130° C. for 5 min to form an elastic buffer adhesive layer, and then the surface of the elastic buffer adhesive layer was covered with a release layer to obtain the elastic buffer adhesive product.

[0142] Performance Testing

[0143] (1) Impact force and absorption percentage: The impact force and absorption percentage of the elastic buffer rubber products prepared in Application Examples 1 to 9 and Application Comparative Examples 1 to 5 were tested using a falling ball impact tester (Kejian Instrument, KJ-10790-Y). The mass of the falling ball was 11.2 g and the height of the falling ball was 100 mm.

[0144] (2) CFD extrusion:

[0145] The diameter of the test sample is 29mm, and the total thickness of the elastic buffer rubber layer and the release layer is 2mm, of which the thickness of the release film is recorded as A. Use a 5kN sensor, calibrate the height H between the upper and lower pressure plates, reset it, manually lower the upper pressure plate first, make it contact the sample and the force value is displayed as 0.4N, at this time the height of the upper and lower pressure plates is B, keep it for 2min, the total height of the silicone is C=BA, after entering the total thickness C of the sample, click to start the test (the displacement when the rebound force is 1N is defined as the compression displacement 0 point), the compression speed is 5mm / min, press to the maximum force, and record the corresponding stress under 25% strain.

[0146] (3) Viscosity

[0147] The adhesion test was obtained with reference to the national standard GB / T 2792. The object to be tested was cut into 25.4mm*150mm specimens. First, one layer of release film was peeled off and replaced with 25U transparent PET. Then the other side was attached to a mirror steel plate. After standing at room temperature for 20 minutes, the peeling force was tested by a tensile testing machine.

[0148] The test results are shown in Table 2:

[0149] Table 2

[0150]

[0151]

[0152] Analysis of the data in Table 2 shows that, taking Examples 1 to 9 as examples, the elastic buffer glue of the present invention has excellent buffering performance and anti-mold printing effect, and the impact absorption rate of the elastic buffer glue product is 44-70%, CFD extrusion is 762-1200kPa, and the viscosity is 1100-3000gf / 25.4mm.

[0153] Analysis of Example 1 and Examples 6 to 8 shows that without adding a specific amount of natural rubber, acrylate or isocyanate, the cushioning performance and anti-mold effect of the elastic buffer glue decrease. This shows that the present invention, by adopting specific ratios of the components, obtains an elastic buffer glue with better application effect.

[0154] From the analysis of Example 1 and Example 9, it can be seen that when the elastic buffer glue only includes inorganic fillers, the buffering performance and anti-mold printing effect of the elastic buffer glue decrease. This is because the hardness of the inorganic filler itself is relatively large, which will increase the hardness of the product after filling, and it is difficult to recover after deformation under force.

[0155] Analysis of Example 1 and Comparative Example 1 shows that in Comparative Example 1, the polyester polyol is replaced by polyether polyol in equal amounts, and the cushioning performance and anti-mold effect of the elastic cushioning rubber are reduced. This is because the cross-linking density between the polyether polyol and other components is large, the molecular weight formed is high, the overall hardness is relatively high, and it is not easy to recover after being subjected to force.

[0156] Analysis of Example 1 and Comparative Examples 2 to 3 shows that when no natural rubber is added or when an equal amount of natural rubber is replaced by styrene-butadiene rubber, the cushioning performance and anti-mold printing effect of the elastic cushioning rubber decrease.

[0157] By analyzing Example 1 and Comparative Example 4, it is found that in Comparative Example 4, no acrylate having certain flexibility and polar groups is added, and the viscosity and CFD extrusion performance of the elastic buffer glue are deteriorated, and the application performance of the elastic buffer glue is deteriorated.

[0158] From the analysis of Example 1 and Comparative Example 5, it can be seen that when isocyanate and polyester polyol are not added, the elastic buffer rubber does not contain polyurethane, the CFD extrusion performance is deteriorated, and the anti-mold effect is poor.

[0159] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. An elastic buffer rubber, characterized in that: The raw materials for preparing the elastic buffer rubber include the following components: polyester polyol, chain extender, natural rubber, sulfur, accelerator, stearic acid, acrylate, filler, isocyanate, dispersant, leveling agent, defoamer and antistatic agent.

2. The elastic buffer rubber according to claim 1, characterized in that: The polyester polyol includes poly(1,4-butylene adipate) and / or poly(ethylene adipate); The chain extender includes an alcohol chain extender; The accelerator includes a dithiocarbamate accelerator; The acrylic acid ester includes polybutyl acrylate and / or polymethyl acrylate.

3. The elastic buffer rubber according to claim 1, characterized in that: The filler comprises a combination of nano carbon powder and inorganic filler; The inorganic filler includes any one of MgO, CaO, Al2O3, ZrO2, ZnO, MnO2, AlSiO5, Zr2WO3, CuO·Cr2O3, H2O8P2Zr, β-LiAlSiO4, CuO·Cr2O3 or 2MgO·2Al2O3·5SiO2, or a combination of at least two thereof; The particle size of the filler is 5-500 μm.

4. The elastic buffer rubber according to claim 1, characterized in that: The isocyanate includes diphenylmethane diisocyanate and / or diphenylmethane diisocyanate; The leveling agent includes any one of polydimethylsiloxane, alkyl-modified organic siloxane, acrylic resin or organic-modified polysiloxane acrylic acid or a combination of at least two thereof; The defoaming agent includes any one or a combination of at least two of polydimethylsiloxane copolymer, ethylene oxide, propylene oxide or phosphate copolymer; The antistatic agent includes a polythiophene antistatic agent and / or a nano carbon tube antistatic agent.

5. The elastic buffer rubber according to claim 1, characterized in that: The raw materials for preparing the elastic buffer rubber include the following components in parts by weight: 60-80 parts of polyester polyol, 5-30 parts of chain extender, 50-80 parts of natural rubber, 3-15 parts of sulfur, 1-10 parts of accelerator, 1-10 parts of stearic acid, 30-70 parts of acrylate, 8-16 parts of filler, 20-40 parts of isocyanate, 0.1-3 parts of dispersant, 0.1-3 parts of leveling agent, 0.1-3 parts of defoaming agent, and 0.1-7 parts of antistatic agent.

6. A method for preparing the elastic buffer rubber according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: 1) mixing polyester polyol, isocyanate, chain extender, part of filler and part of dispersant to obtain component A; 2) mixing and reacting natural rubber, sulfur, an accelerator, stearic acid and another portion of a dispersant to obtain component B; 3) Component A, component B, acrylate, another portion of filler, leveling agent, defoaming agent and antistatic agent are mixed to obtain the elastic buffer adhesive.

7. The preparation method according to claim 6, characterized in that: The part of filler in step 1) is 2-35% of the total mass of the filler; The part of the dispersant in step 1) is 0.1-10% of the total mass of the dispersant; The temperature of the mixed reaction in step 1) is 30-60°C; The mixing reaction time in step 1) is 3 to 6 hours; The temperature of the mixed reaction in step 2) is 60-80°C; The mixing reaction time in step 2) is 8 to 14 hours; The rotation speed of the mixing reaction in step 1) and step 2) is independently 300-700 r / min; The mixing temperature in step 3) is 15-60°C; The mixing time in step 3) is 20 to 60 minutes; The mixing speed in step 3) is 1000-1400 r / min; The step 3) further comprises filtering after the mixing.

8. The preparation method according to claim 6, characterized in that: The preparation method comprises the following steps: 1) Mixing polyester polyol, isocyanate, chain extender, part of filler and dispersant at 30-60° C. and 300-700 r / min for 3-6 hours to obtain component A; 2) mixing natural rubber, sulfur, accelerator, stearic acid and dispersant at 60-80° C. and 300-700 r / min for 8-14 hours to obtain component B; 3) Component A, component B, acrylate, another part of filler, leveling agent, defoamer and antistatic agent are mixed at 15-30° C. and 1000-1400 r / min for 20-60 min, filtered, and the filtrate is taken to obtain the elastic buffer rubber.

9. An elastic buffer rubber product, characterized in that: The elastic buffer adhesive product comprises a first release layer, an elastic buffer adhesive layer and a base material layer stacked in sequence; The elastic buffer rubber layer comprises the elastic buffer rubber according to any one of claims 1 to 5; The base material layer includes a substrate layer and / or a second release layer; The substrate layer includes any one of a metal substrate, PET, a conductive cloth or a non-woven fabric; The metal substrate includes copper foil and / or aluminum foil.

10. A method for preparing the elastic buffer rubber product according to claim 9, characterized in that: The preparation method comprises the following steps: 1) coating the elastic buffer adhesive as claimed in any one of claims 1 to 5 on the surface of the base material layer, drying and curing to form an elastic buffer adhesive layer; 2) Covering the surface of the elastic buffer adhesive layer with a first release layer to obtain the elastic buffer adhesive product.

Citation Information