Burning-free fracturing propping agent for deep well reinjection as well as preparation method and application of burning-free fracturing propping agent
By using raw materials such as coal gangue and other raw materials in deep well return injection, reacting with water glass, sodium hydroxide, etc. to form burn-free fracturing proppants, the problems of high production costs and complex processes in the existing technology are solved, and high efficiency and low cost are achieved Deep well reinfusion proppant preparation simplifies the process and is suitable for deep well reinfusion of concentrated saline water.
Patent Information
- Application Number
- CN202410929027.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-01
AI Technical Summary
The production cost of existing deep well back injection fracturing proppants is high and the process is complex, especially in coal gangue. It is necessary to separate kaolinite and quartz sand, resulting in waste of resources and pollution, and the calcination process increases costs.
Coal gangue, water glass, sodium hydroxide, sodium dodecylbenzenesulfonate and hydrogen peroxide are used as raw materials to prepare burn-free fracturing proppants through corrosion and granulation process, and chemical reagents react with kaolinite in coal gangue to form High-strength gelling materials avoid calcination process and simplify the process flow.
It effectively reduces the production cost of fracturing proppants, simplifies the process, realizes on-site material extraction and solid waste treatment, and can adjust the proppant density, increase applicability, and meets the needs of deep well return injection.
Smart Images

Figure CN118879302A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of deep well reinjection, and particularly relates to a burn-free fracturing proppant for deep well reinjection, a preparation method and an application thereof. Background Art
[0002] The coal mining process brings many environmental problems, such as mine water and coal gangue discharge. At present, the main means of treating mine water is to concentrate the mine water step by step and purify it to the target water quality. However, the concentration will produce a large amount of brine as a byproduct. The disposal of brine has the problems of high cost and low efficiency. An effective way to solve this problem is to implement large-diameter deep well reinjection. In order to ensure that the reinjection volume of a single well meets the design requirements, when the formation fissures are small and the water intake does not meet the requirements, in order to dredge the water injection space and water guide channels, the target layer section can be fracturing. During the fracturing process, fracturing proppants are also required to ensure the long-term stability of the rock formation fissures. Whether the preparation of fracturing proppants can be made from local materials and prepared with simple processes will significantly reduce the cost of the deep well reinjection process. Existing fracturing proppants include two types: quartz sand and artificial ceramsite. Coal gangue is an excellent material for preparing quartz sand and artificial ceramsite because it is rich in quartz and kaolinite. However, the existing technology prepares quartz sand and artificial ceramsite separately, which requires the separation of kaolinite in the coal gangue during the preparation of quartz sand, wastes the aluminosilicate raw materials in the coal gangue, and also produces pollutants. In the production process of artificial ceramsite, because quartz is difficult to convert, high temperature is required to sinter the ceramsite. The use of calcination technology makes the preparation of the material difficult and costly.
[0003] Therefore, how to obtain local materials, reduce the production cost of deep well reinjection fracturing proppants, and simplify the production process has become a technical problem that needs to be solved urgently. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a burn-free fracturing proppant for deep well reinjection, a preparation method and application, so as to solve the technical problems of high production cost and complex production process of deep well reinjection fracturing proppant.
[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0006] The invention discloses a method for preparing a burn-free fracturing proppant for deep well reinjection. The method uses coal gangue, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate, hydrogen peroxide and water as raw materials and adopts a corrosion granulation process to prepare the burn-free fracturing proppant. The raw materials include, by mass percentage, 45.5-55.6% of coal gangue, 15.7-26.8% of water glass, 9.8-14.6% of sodium hydroxide, 0.5-1.3% of sodium dodecylbenzene sulfonate, 2.5-4.6% of hydrogen peroxide and 11.3-15.7% of water, and the mass percentage of each component totals 100%.
[0007] The present invention also has the following technical features:
[0008] Specifically, the method comprises the following steps:
[0009] Step 1, crushing the coal gangue into powder to obtain coal gangue particles as master particles and coal gangue powder as auxiliary powder;
[0010] Step 2, putting the coal gangue particles into a granulator; mixing the formulated amount of coal gangue powder, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate and water to obtain a slurry;
[0011] Step 3, spraying the slurry obtained in step 2 into a rotating granulator, and obtaining an intermediate after the spraying is completed;
[0012] Step 4: Prepare a foaming liquid using water and hydrogen peroxide as raw materials, and spray the prepared foaming liquid into a rotating granulator to obtain a burn-free fracturing proppant for deep well reinjection.
[0013] Furthermore, in step 1, the particle size of the coal gangue particles is 5 to 50 meshes, and the particle size of the coal gangue powder is less than 200 meshes.
[0014] Furthermore, in step 2, the mass ratio of the gangue particles to the gangue powder is (2.5-3.5):1.
[0015] Furthermore, in step 3, the rotation speed of the granulator is 100-150 r / min, the spraying speed of the slurry is 1-1.5 L / min, and the spraying time is 5-10 min.
[0016] Furthermore, in step 4, the mass ratio of water to hydrogen peroxide is (3.5-4.5):1, the spraying speed is 0.5-0.7 L / h, and the spraying time is 1-2 min.
[0017] Furthermore, the particle size of the unburned fracturing proppant for deep well reinjection prepared in step 4 is 106-3350 microns, the sphericity is greater than 0.7, the maximum acid solubility is greater than 1.5%, and the density is less than 2.13 g / cm 3 , crushing stress value>28MPa.
[0018] The present invention also protects an unburned fracturing proppant for deep well reinjection, which is prepared by the above-mentioned preparation method. The unburned fracturing proppant comprises the following raw material components by mass percentage: 45.5-55.6%, 15.7-26.8% water glass, 9.8-14.6% sodium hydroxide, 0.5-1.3% sodium dodecylbenzene sulfonate, 2.5-4.6% hydrogen peroxide and 11.3-15.7% water, and the mass percentage of each component totals 100%.
[0019] Furthermore, the particle size of the unburned fracturing proppant is 106-3350 microns, the sphericity is greater than 0.7, the maximum acid solubility is greater than 1.5%, and the density is less than 2.13 g / cm 3 , crushing stress value>28MPa.
[0020] The present invention also protects the use of the unburned fracturing proppant for deep well reinjection prepared by the above preparation method in the deep well reinjection of concentrated brine.
[0021] Compared with the prior art, the present invention has the following technical effects:
[0022] (I) The preparation method of the present invention uses coal gangue particles and coal gangue powder as main raw materials, which realizes the local acquisition of raw materials, can effectively reduce the production cost of fracturing proppants, and can also process part of the coal gangue solid waste on site.
[0023] (II) Preparation method of the present invention The process method of the present invention abandons the calcination process used in the preparation process of traditional fracturing proppants, and utilizes the characteristics of chemical reagents reacting with kaolinite in coal gangue to form high-strength cementitious materials, giving full play to the role of quartz phase and kaolinite phase in coal gangue. While simplifying the proppant preparation process, it avoids the high-temperature calcination process and can effectively reduce the production cost of the enterprise.
[0024] (III) The foaming agent added in the preparation method provided by the present invention can adjust the density of the proppant within the same particle size range, thereby increasing the applicability of the proppant. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The following are the physical picture and SEM picture of the burn-free fracturing proppant prepared in Example 1;
[0026] Figure 2 This is the phase distribution diagram of the unburned fracturing proppant obtained in Examples 1 to 5;
[0027] Figure 3 This is a process diagram of using the burn-free fracturing support of Example 1 for deep well reinjection of concentrated brine.
[0028] The specific contents of the present invention are further described in detail below in conjunction with the accompanying drawings and embodiments. DETAILED DESCRIPTION
[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by any ordinary technician in the field belong to the scope of protection of the present invention.
[0030] It should be noted that all raw materials in the present invention, unless otherwise specified, are raw materials known in the art.
[0031] In the present invention, concentrated brine refers to water with a TDS greater than 10,000.
[0032] The technical concept of the present application is: using coal gangue, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate, hydrogen peroxide and water as raw materials, utilizing the properties of chemical reagents reacting with kaolinite in coal gangue to form high-strength gelling materials, and preparing unburned fracturing proppants through a corrosion granulation process.
[0033] The gangue used in the present application is solid waste from coal mining. In terms of mass percentage, the components of the gangue include SiO2 45.1-58.3%, Al2O3 14.2-30.7%, Fe2O3 1.4-8.1%, CaO 0.7-4.7%, MgO 0.5-1.3%, K2O 2.1-2.9%, TiO2 0.4-0.9%, carbon, organic matter and other trace components 10.5-12.5%, and the mass percentages of each component add up to 100%.
[0034] According to the above technical scheme, the present invention discloses a non-burning fracturing proppant for deep well reinjection, which uses coal gangue, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate, hydrogen peroxide and water as raw materials and adopts a corrosion granulation process to prepare the non-burning fracturing proppant;
[0035] The unburned fracturing proppant comprises the following raw material components by mass percentage: 45.5-55.6% coal gangue, 15.7-26.8% water glass, 9.8-14.6% sodium hydroxide, 0.5-1.3% sodium dodecylbenzene sulfonate, 2.5-4.6% hydrogen peroxide and 11.3-15.7% water, and the mass percentage of each component totals 100%.
[0036] The specific method includes the following steps:
[0037] Step 1, crushing the gangue into powder to obtain gangue particles as master particles and gangue powder as auxiliary powder; the particle size of the gangue particles is 5 to 50 meshes, and the particle size of the gangue powder is less than 200 meshes;
[0038] Step 2, putting the coal gangue particles into a granulator; mixing the formulated amount of coal gangue powder, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate and water to obtain a slurry; the mass ratio of the coal gangue particles to the coal gangue powder is (2.5-3.5):1.
[0039] Step 3, spraying the slurry obtained in step 2 into a rotating granulator, and obtaining an intermediate after the spraying is completed;
[0040] Preferably, the rotation speed of the granulator is 100-150 r / min, the spraying speed of the slurry is 1-1.5 L / min, and the spraying time is 5-10 min.
[0041] Step 4: preparing a foaming liquid using water and hydrogen peroxide as raw materials, and spraying the prepared foaming liquid into a rotating granulator to obtain a burn-free fracturing proppant for deep well reinjection;
[0042] Preferably, the mass ratio of water to hydrogen peroxide is (3.5-4.5):1, the spraying speed is 0.5-0.7 L / h, and the spraying time is 1-2 min.
[0043] The particle size of the prepared unburned fracturing proppant for deep well reinjection is 106-3350 microns, the sphericity is greater than 0.7, the maximum acid solubility is greater than 1.5%, and the density is less than 2.13 g / cm 3 , crushing stress value>28MPa.
[0044] The invention also discloses the application of the above-mentioned unburned fracturing proppant for deep well reinjection in the reinjection of concentrated brine into deep wells.
[0045] Specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical solution of this application fall within the protection scope of the present invention.
[0046] Example 1
[0047] This embodiment provides a method for preparing a burn-free fracturing proppant for deep well reinjection, which specifically comprises the following steps:
[0048] Step 1, crushing the gangue into powder to obtain gangue particles as master particles and gangue powder as auxiliary powder, wherein the particle size of the gangue particles is 5 to 50 meshes, and the particle size of the gangue powder is less than 200 meshes;
[0049] Step 2, putting the coal gangue particles into a granulator; mixing the formulated amount of coal gangue powder, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate and water to obtain a slurry;
[0050] Step 3, start the granulator, set the speed to 120r / min, spray the slurry prepared in step 2 into the rotating granulator at a spraying speed of 1L / h, and continue to run the granulator for 10min after the spraying, until the masterbatch continuously absorbs the slurry material to form a number of intermediates of different sizes;
[0051] Step 4: Compound the formulated amount of water and hydrogen peroxide into a foaming liquid, and spray the obtained foaming liquid evenly into a rotating granulator at a spraying rate of 0.5 L / h. After the foaming liquid spraying is completed, the granulator continues to operate for 10 minutes to obtain a burn-free fracturing proppant for deep well reinjection.
[0052] Among them, in terms of mass percentage, the mass percentage of each raw material component is: 55.4% of coal gangue, 16.5% of water glass, 10.3% of sodium hydroxide, 0.6% of sodium dodecylbenzene sulfonate, 4.3% of hydrogen peroxide and 12.9% of water; the mass ratio of coal gangue particles to coal gangue powder is 3:1; the mass ratio of water used to prepare the slurry to water used to prepare the foaming liquid is 4:1.
[0053] The unburned fracturing proppant prepared in this embodiment was tested and the following results were obtained: Figure 1 The SEM images shown in Figure 2 The physical and chemical properties of the fracturing proppant are shown in Table 1.
[0054] Example 2
[0055] The present embodiment provides a method for preparing a burn-free fracturing proppant for deep well reinjection. The steps and raw material components of the preparation method used in the present embodiment are basically the same as those in Example 1. The only difference is that, in the present embodiment, the mass percentage of each raw material component is: 50.4% coal gangue, 20.2% water glass, 12.3% sodium hydroxide, 0.6% sodium dodecylbenzene sulfonate, 3.1% hydrogen peroxide and 13.4% water.
[0056] The physical and chemical properties of the unburned fracturing proppant prepared in this example are shown in Table 1.
[0057] Example 3
[0058] The present embodiment provides a method for preparing a burn-free fracturing proppant for deep well reinjection. The steps and raw material components of the preparation method used in the present embodiment are basically the same as those in Example 1. The only difference is that, in the present embodiment, the mass percentage of each raw material component is: 45.5% coal gangue, 24.1% water glass, 14.3% sodium hydroxide, 0.6% sodium dodecylbenzene sulfonate, 3.1% hydrogen peroxide and 12.4% water.
[0059] The physical and chemical properties of the unburned fracturing proppant prepared in this example are shown in Table 1.
[0060] Example 4
[0061] The present embodiment provides a method for preparing a burn-free fracturing proppant for deep well reinjection. The steps and raw material components of the preparation method used in the present embodiment are basically the same as those in Example 1. The only difference is that, in the present embodiment, the mass percentage of each raw material component is: 55.4% coal gangue, 16.5% water glass, 10.3% sodium hydroxide, 0.6% sodium dodecylbenzene sulfonate, 2.0% hydrogen peroxide, and 15.2% water.
[0062] The physical and chemical properties of the unburned fracturing proppant prepared in this example are shown in Table 1.
[0063] Example 5
[0064] The present embodiment provides a method for preparing a burn-free fracturing proppant for deep well reinjection. The steps and raw material components of the preparation method used in the present embodiment are basically the same as those in Example 1. The only difference is that, in the present embodiment, the mass percentage of each raw material component is: 55.4% coal gangue, 16.5% water glass, 10.3% sodium hydroxide, 0.6% sodium dodecylbenzene sulfonate, 0.8% hydrogen peroxide and 16.4% water.
[0065] The physical and chemical properties of the unburned fracturing proppant prepared in this example are shown in Table 1.
[0066]
[0067] Table 1. Physical and chemical properties of fracturing proppants of Examples 1 to 5
[0068] The unburned fracturing proppant prepared in Example 1 can be used for deep well reinjection of concentrated brine. Figure 3 The application of the unburned fracturing proppant of Example 1 in the deep well reinjection of concentrated brine in Xiaobaodang Coal Mine is shown. The fracturing process parameter design and fracturing effect are shown in Table 2 and Table 3:
[0069]
[0070] Table 2. Fracturing process parameter design
[0071]
[0072] Table 3. Fracturing effect
[0073] Depend on Figure 1It can be seen that the unburned fracturing proppant prepared in Example 1 presents spherical structures of different sizes. It can be seen from Table 1 that the unburned fracturing proppant prepared in Examples 1 to 5 can meet the basic performance requirements of fracturing proppant, wherein Examples 1 to 3 change the proportion of water glass and sodium hydroxide in the raw materials. With the increase of the proportion of water glass and sodium hydroxide, the particle size, sphericity, maximum acid solubility and density of the fracturing proppant have no obvious changes, and the strength is significantly increased. This is because: the increase in the proportion of water glass and sodium hydroxide can further promote the production of gelling materials, improve the density of the proppant, and increase the material strength.
[0074] Compared with Example 1, Example 4 and Example 5, the proportion of hydrogen peroxide in the foaming liquid is changed. It can be seen from Table 1 that as the hydrogen peroxide content decreases, the sphericity of the fracturing proppant decreases significantly (after the hydrogen peroxide content decreases, the proppant particles are close to the shape and size of the masterbatch, resulting in a significant decrease in sphericity), and the strength and density are significantly improved. This is because the pore structure of the material is mainly obtained by the decomposition of hydrogen peroxide in the gelling material to produce oxygen. It can be seen that adjusting the hydrogen peroxide content can directly affect the sphericity of the proppant, and ultimately a variety of different types of non-burning fracturing proppants can be provided for different working conditions.
[0075] like Figure 2 It can be seen that the main crystal phase in the unburned fracturing proppant is quartz, and no obvious kaolinite phase is observed, indicating that the preparation method provided by the present invention can convert the kaolinite in the gangue into an unoriented gelling material, which is wrapped around the irregular quartz phase to form a spherical fracturing proppant, thereby achieving full utilization of the main phases in the gangue.
[0076] It can be seen from Table 3 that before and after hydraulic fracturing, there is no obvious change in the support height of the crack height, indicating that the fracturing proppant prepared by the method of the present invention can better support the cracks generated by hydraulic fracturing, play a role in long-term stable support for rock cracks, and facilitate long-term reinjection of concentrated brine.
[0077] During the process of concentrated brine reinjection, formation fissure blockage is often encountered. By adopting the technology of the present invention, a granulator and raw materials such as coal gangue activator are directly used to prepare fracturing proppant at the concentrated brine reinjection wellhead, and then mixed with concentrated brine and injected into the well. The raw material composition can be slightly changed according to different working conditions.
[0078] Compared with purchasing fracturing proppants from outside, the method of the present invention can not only obtain local materials and reduce costs, but also has strong process adaptability.
[0079] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0080] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a burn-free fracturing proppant for deep well reinjection, It is characterized in that The unburned fracturing proppant is prepared by using coal gangue, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate, hydrogen peroxide and water as raw materials and adopting the corrosion granulation process; The unburned fracturing proppant comprises the following raw material components by mass percentage: 45.5-55.6% coal gangue, 15.7-26.8% water glass, 9.8-14.6% sodium hydroxide, 0.5-1.3% sodium dodecylbenzene sulfonate, 2.5-4.6% hydrogen peroxide and 11.3-15.7% water, and the mass percentage of each component totals 100%.
2. The method for preparing the burn-free fracturing proppant for deep well reinjection according to claim 1, It is characterized in that The method comprises the following steps: Step 1, crushing the coal gangue into powder to obtain coal gangue particles as master particles and coal gangue powder as auxiliary powder; Step 2, putting the coal gangue particles into a granulator; mixing the formulated amount of coal gangue powder, water glass, sodium hydroxide, sodium dodecylbenzene sulfonate and water to obtain a slurry; Step 3, spraying the slurry obtained in step 2 into a rotating granulator, and obtaining an intermediate after the spraying is completed; Step 4: Prepare a foaming liquid using water and hydrogen peroxide as raw materials, and spray the prepared foaming liquid into a rotating granulator to obtain a burn-free fracturing proppant for deep well reinjection.
3. The method for preparing the unburned fracturing proppant for deep well reinjection according to claim 2, It is characterized in that In the step 1, the particle size of the coal gangue particles is 5 to 50 meshes, and the particle size of the coal gangue powder is less than 200 meshes.
4. The method for preparing the unburned fracturing proppant for deep well reinjection according to claim 1, It is characterized in that In step 2, the mass ratio of coal gangue particles to coal gangue powder is (2.5-3.5):
1.
5. The method for preparing the burn-free fracturing proppant for deep well reinjection according to claim 1, It is characterized in that In the step 3, the rotation speed of the granulator is 100-150 r / min, the spraying speed of the slurry is 1-1.5 L / min, and the spraying time is 5-10 min.
6. The method for preparing the unburned fracturing proppant for deep well reinjection according to claim 1, It is characterized in that In step 4, the mass ratio of water to hydrogen peroxide is (3.5-4.5):1, the spraying speed is 0.5-0.7 L / h, and the spraying time is 1-2 min.
7. The method for preparing the unburned fracturing proppant for deep well reinjection according to claim 1, It is characterized in that The particle size of the unburned fracturing proppant for deep well reinjection prepared in step 4 is 106-3350 microns, the sphericity is greater than 0.7, the maximum acid solubility is greater than 1.5%, and the density is less than 2.13 g / cm 3 , crushing stress value>28MPa.
8. A burn-free fracturing proppant for deep well reinjection, It is characterized in that The unburned fracturing proppant is prepared by the preparation method according to any one of claims 1 to 7, and the unburned fracturing proppant comprises the following raw material components by mass percentage: 45.5-55.6%, 15.7-26.8% of water glass, 9.8-14.6% of sodium hydroxide, 0.5-1.3% of sodium dodecylbenzene sulfonate, 2.5-4.6% of hydrogen peroxide and 11.3-15.7% of water, and the mass percentage of each component totals 100%.
9. The burn-free fracturing proppant for deep well reinjection according to claim 8, It is characterized in that Particle size is 106-3350 microns, sphericity>0.7, maximum acid solubility>1.5%, density<2.13g / cm 3 , crushing stress value>28MPa.
10. Use of the unburned fracturing proppant for deep well reinjection prepared by the preparation method according to any one of claims 1 to 7 in the deep well reinjection of concentrated brine.