A Cr 3+ Doped broadband near-infrared phosphor and preparation method thereof, near-infrared light-emitting device

By using Cr3+ doped broadband near-infrared phosphor of A(3-3x)B4x-yC(1-x)O4:yCr3+, the problem of insufficient emission peak wavelength in the prior art was solved, and a broadband near-infrared of 750~1100nm was achieved Infrared emission and efficient energy conversion, suitable for a variety of applications.

CN118879319BActive Publication Date: 2024-11-29INNER MONGOLIA UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411354862.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-29
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

The emission peak wavelengths of existing Cr3+ doped near-infrared phosphors are all lower than 800 nm, which is difficult to meet the application needs of near-infrared light sources, limiting their practical applications.

Method used

Cr3+ doped broadband near-infrared phosphor with the chemical formula A(3-3x)B4x-yC(1-x)O4:yCr3+ is used to achieve a 750~1100nm through the combination of the matrix structure of the cubic crystal system and the appropriate elements. Broadband near-infrared emission, the emission peak wavelength is 815~845 nm, and the preparation method includes the steps of high-temperature sintering and grinding.

Benefits of technology

It has achieved efficient near-infrared light emission under blue light excitation, with high luminous intensity, high energy conversion efficiency, good chemical stability and thermal stability. It is suitable for food safety, healthy diet and early cancer diagnosis and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879319B_ABST
    Figure CN118879319B_ABST
Patent Text Reader

Abstract

The invention discloses a Cr 3+ Doped broadband near-infrared phosphor and preparation method thereof, near-infrared light-emitting device, the chemical formula of the broadband near-infrared phosphor is: A (3‑3x) B 4x‑y C (1‑x) O 4 : y Cr 3+ ; Wherein A is one or more of Li, Na, and K elements, B is one or more of Mg, Ca, Sr, Zn, and Ba elements, and C is one or a combination of two of Nb and Ta elements; x , y is the mole fraction, and its value range is: 0< x <1,0< y The near-infrared phosphor provided by the present invention can be excited by light with a wavelength in the range of 400 to 500 nm, and the optimal excitation wavelength is 450 to 480 nm, the emission wavelength range is 750 to 1100 nm, and the emission peak is about 815 to 845 nm, which effectively realizes the photoconversion effect of emitting near-infrared light under blue light excitation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of luminescent materials, in particular to a Cr 3+ Doped broadband near-infrared phosphor and preparation method thereof, and near-infrared light-emitting device. Background Art

[0002] In recent years, researchers have proposed the idea of ​​integrating near-infrared spectroscopy technology into portable devices such as mobile phones to achieve the detection of food nutrients and the state of organisms at any time. This technology has the characteristics of rapid and non-destructive detection, and plays an important role in solving food safety problems, healthy diet problems, and early diagnosis of cancer. The basic principle of this technology is to use broadband near-infrared light to irradiate the object to be tested. CH, NH, OH, etc. contained in the object to be tested will absorb specific light bands, causing changes in the scattering spectrum, and then calculate the type and content of specific substances based on the changes in the shape and intensity of the scattering spectrum. Take the application in medicine as an example: broadband near-infrared spectroscopy technology is widely and avant-garde in medicine. Its application in medicine can be traced back to 1977 when Jöbsis used near-infrared spectroscopy to detect cortical oxidation in adults during hyperpnea. It was on this basis that functional near-infrared spectroscopy (fNIRs) was developed. fNIRs mainly uses near-infrared light of 650-1000nm to measure the changes in the content of oxygenated hemoglobin and deoxygenated hemoglobin in the brain, and then estimates the brain's neural activity. It has the advantages of being non-destructive, low-cost, portable, and safe. The person being tested can carry out normal work and learning activities during the test. This technology has been widely used in the field of brain detection. However, this application has strict requirements for near-infrared light sources, such as requiring the light source to have a wide enough spectral band, high enough stability, and be miniaturized and integrated. The lack of efficient broadband near-infrared fluorescent materials is one of the bottlenecks in realizing this technology.

[0003] Broadband near-infrared phosphors are mainly composed of Cr 3+ Activated luminescent material, Cr 3+ In the octahedral crystal field, using Cr 3+ Ground State 4 A 2 to excited state 4 T 1 The transition absorbs blue light, and then 4 T 1 Relax down 4 T 2 Energy level, through 4 T 2 To the ground state 4 A 2 transition, achieving broadband near-infrared emission.

[0004] For example, in patent CN118064147A, the general chemical formula is Zn 2-x A x Ti y B z O 4 :mCr, a representative example is Zn 2 Ti 0 .792 Sn 0 .198 O 4 : 0.01Cr, belonging to the perovskite-like structure, each embodiment mainly consists of Zn 2 SnO 4 It is a near-infrared phosphor with an excitation wavelength range of 300-700nm and an emission spectrum range of 650-1100nm. When the near-infrared phosphor is excited at 468nm, its emission peak is at 742nm.

[0005] Patent CN116376551B, its chemical formula is A a M b N c O 19 :xD, a representative example is Ca 0 .85 Ga 4 Al 7 .4 Sc 0 .5 O 19 :0.25 Cr 3+, The luminescent material is based on alkali metal aluminate oxide, has a perovskite-like structure, belongs to the tetragonal system, and has a space group of P4mm. The material can be excited by light in the wavelength range of 250nm to 80nm, 360nm to 460nm, and 540nm to 600nm, and the luminescent band is located in the range of 700nm to 850nm, with an emission peak wavelength at 780nm.

[0006] Patent CN115368889B, its chemical formula is K 2.3 Na 0.7 Al 0.9-x Ga 0.1 O 3 :xCr, representative example is K 2.3 Na 0.7 Al 0.8955 Ga 0.1 O 3 :0.0045Cr. This material uses alkali metal aluminate oxide as the matrix and trivalent chromium ions as the activator. Its structure is similar to K 3 AlO 3The phosphor can be excited by the near-ultraviolet-blue light band and has broadband emission characteristics: it can achieve broadband near-infrared light emission of 700 to 1100 nanometers, with the emission peak wavelength at 740nm.

[0007] Patent CN114426844A, its chemical formula is A 3 B 3 M 2 F 12 :xCr 3+ , a representative example is Na 3 Li 3 Al 2 F 12 :Cr 3+ The crystal structure belongs to the cubic system, and the space group is Ia3d. The patent states that the material can be excited by a violet LED chip, a blue LED chip or a red LED chip, and after being excited, it can emit near-infrared light with a wavelength range of 650-1000nm, with a peak value in the range of 730-800nm.

[0008] Patent CN117586774A, chemical formula is A1 3- y A2 y B 2-x C1 y C2 3-y O 12 :xCr 3+ , a representative example is Ca 2 Y 1 Al 1 .95 Al 1 Ge 2 O 12 :0 .05Cr 3+ Its crystal structure belongs to garnet structure, which can be excited by blue LED, achieving a half-peak width of 95-153nm, an excitation peak of 450nm, and an emission peak of 780nm.

[0009] In the above patents, all are Cr 3+ The doped near-infrared phosphors have high luminescence efficiency and good thermal stability, but the emission peaks are all below 800 nm, which is difficult to meet the application requirements of near-infrared light sources, seriously affecting the overall performance of near-infrared light sources and limiting their practical applications. Summary of the invention

[0010] The first object of the present invention is to provide a Cr 3+ The doped broadband near-infrared phosphor can be effectively excited by blue light, has good thermal stability, high luminous efficiency and an emission peak wavelength greater than 800 nm.

[0011] The second object of the present invention is to provide a Cr 3+ Preparation method of doped broadband near-infrared phosphor.

[0012] A third object of the present invention is to provide a near-infrared light-emitting device.

[0013] The first object of the present invention is implemented by the following technical solution: a Cr 3+ Doped broadband near-infrared phosphor, the chemical formula of the broadband near-infrared phosphor is: (3-3x) B 4x-y C (1-x) O 4 : y Cr 3+ ; A is one or more of Li, Na, and K elements, B is one or more of Mg, Ca, Sr, Zn, and Ba elements, and C is one or a combination of two of Nb and Ta elements; x , y is the mole fraction, and its value range is: 0< x <1,0< y ≤0.3.

[0014] Furthermore, the crystal structure of the matrix lattice of the broadband near-infrared phosphor belongs to the cubic crystal system, and the space group is Fm3m.

[0015] Furthermore, the broadband near-infrared phosphor achieves broadband near-infrared emission of 750 to 1100 nm under the excitation of blue light with a wavelength of 400 to 500 nm, and its emission peak wavelength is 815 to 845 nm.

[0016] The second object of the present invention is implemented by the following technical solution: a Cr 3+ The method for preparing the doped broadband near-infrared phosphor comprises the following steps:

[0017] Step 1: According to the chemical formula A (3-3x) B 4x-y C (1-x) O 4 : y Cr 3+ The stoichiometric ratio of each element in x <1,0< y≤0.3, wherein A is one or more of Li, Na, and K, B is one or more of Mg, Ca, Sr, Zn, and Ba, and C is one or a combination of Nb and Ta; weigh one or more of the compounds of Li, Na, or K; weigh one or more of the compounds of Mg, Ca, Sr, Zn, or Ba; weigh one or more of the compounds of Nb, Ta, or tantalum; weigh a compound of Cr; all of them are ground in an agate mortar and mixed evenly to obtain a mixture;

[0018] Step 2: placing the mixture at a temperature of 1100° C. to 1350° C. for high temperature sintering for 4 to 10 hours;

[0019] Step 3: After the sintering is completed and the mixture is naturally cooled, it is ground to obtain the broadband near-infrared phosphor.

[0020] Furthermore, the compound of Li element, the compound of Na element or the compound of K element is one or more of oxides, carbonates, nitrates, sulfates, halides or hydroxides of the corresponding elements.

[0021] Furthermore, the compound of Mg element, the compound of Ca element, the compound of Sr element, the compound of Zn element or the compound of Ba element is one or more of oxides, carbonates, nitrates, sulfates, halides or hydroxides of the corresponding elements.

[0022] Furthermore, the compound of the Nb element is one or more of niobium oxide, niobium chloride, niobium hydroxide, niobium nitrate or ammonium niobate.

[0023] Furthermore, the compound of the Ta element is one or more of tantalum oxide, tantalum chloride or tantalum oxyfluoride.

[0024] Furthermore, the Li element compound in the mixture is added in an amount of 105% to 120% of the amount calculated according to the stoichiometric ratio to compensate for the reduction in the stoichiometric ratio due to volatilization during the sintering process.

[0025] The third object of the present invention is implemented by the following technical scheme: a near-infrared light-emitting device, comprising the broadband near-infrared phosphor and an excitation source described in the first object of the present invention; the wavelength range of the excitation source is within the excitation wavelength range of the broadband near-infrared phosphor.

[0026] Advantages of the present invention:

[0027] (1) The near-infrared phosphor provided by the present invention can be excited by light with a wavelength in the range of 400 to 500 nm, with the optimal excitation wavelength being 450 to 480 nm, the emission wavelength being in the range of 750 to 1100 nm, and the emission peak wavelength being 815 to 845 nm, thereby effectively achieving the photoconversion effect of emitting near-infrared light under blue light excitation.

[0028] (2) The near-infrared phosphor provided by the present invention has high luminous intensity, high energy conversion efficiency, and good chemical stability and thermal stability, and plays an important role in solving food safety issues, healthy diet issues, and early diagnosis of cancer.

[0029] (3) The preparation method of the near-infrared phosphor provided by the present invention has low synthesis temperature, low raw material and equipment costs, is easy to operate, does not pollute the environment, and is suitable for widespread promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0031] Figure 1 It is a comparison chart of the XRD spectra in Examples 1, 2 and 3 of the present invention and the standard card PDF36-1018.

[0032] Figure 2 This is the emission spectrum of the phosphors in Examples 1, 2, 3 and 6 of the present invention under 450nm excitation.

[0033] Figure 3 This is the excitation spectrum of the phosphors in Examples 1, 2, 3 and 6 of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The raw materials for preparing the phosphor in the following examples are: analytically pure BaCO 3 , high purity Li 2 CO 3 、Na 2 CO3 (anhydrous), K 2 CO 3 ,MgO,Nb 2 O 5 、CaCO 3 、SrCO 3 、ZnO、Ta 2 O 5 Cr 2 O 3 .

[0036] Example 1: Li 0.9 Mg 2.77 Nb 0.3 O 4 :0.03Cr 3+ Preparation

[0037] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.0765 g, MgO: 0.2257 g, Nb 2 O 5 : 0.0797 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is easy to volatilize. The calculated amount is 15% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1300℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0038] Figure 1 Curve 1 in the figure is the powder X-ray diffraction pattern of the sample prepared in this embodiment. It can be seen from the figure that when an appropriate amount of transition metal ions Cr is doped 3+ When compared with the standard card, except for a slight shift in the position of the characteristic diffraction peak inherent to the sample, its crystal structure has not changed.

[0039] Figure 2 Curve 1 in FIG. 1 is the emission spectrum of the sample of this embodiment obtained under 450nm excitation. Figure 2 It can be seen that the phosphor can emit broadband near-infrared light with a wavelength range of 750-1100 nm, but the intensity is slightly lower than that of Example 3 (see Figure 2 Curve 3) in the phosphor.

[0040] Figure 3 Curve 1 is the excitation spectrum of the sample of this embodiment obtained when monitoring 819nm. Figure 3It can be seen that the phosphor contains two effective excitation bands, 400nm~525nm and 550nm~700nm respectively.

[0041] Example 2: Li 1.5 Mg 1.97 Nb 0.5 O 4 :0.03Cr 3+ Preparation

[0042] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1275 g, MgO: 0.1604 g, Nb 2 O 5 : 0.1302 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is easy to volatilize. The calculated amount is 15% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1300℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0043] Figure 1 Curve 2 is the powder X-ray diffraction pattern of the sample prepared in this embodiment. It can be seen from the figure that when an appropriate amount of transition metal ions Cr is doped 3+ When compared with the standard card, except for a slight shift in the position of the characteristic diffraction peak inherent to the sample, its crystal structure has not changed.

[0044] Figure 2 Curve 2 is the emission spectrum of the sample of this embodiment obtained under 450nm excitation. Figure 2 It can be seen that the phosphor can emit broadband near-infrared light with a wavelength range of 750-1100 nm, but the intensity is slightly lower than that of Example 3 (see Figure 2 Curve 3) in the phosphor.

[0045] Figure 3 Curve 2 is the excitation spectrum of the sample of this embodiment obtained when monitoring 819nm. Figure 3 It can be seen that the phosphor contains two effective excitation bands, 400nm~525nm and 550nm~700nm respectively.

[0046] Example 3: Li 2 Mg 1.3 Nb 0.66 O 4 :0.03Cr 3+Preparation

[0047] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1626 g, MgO: 0.1056 g, Nb 2 O 5 : 0.1754 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1300℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0048] Figure 1 Curve 3 is the powder X-ray diffraction pattern of the sample prepared in this embodiment. It can be seen from the figure that when an appropriate amount of transition metal ions Cr is doped 3+ When compared with the standard card, except for a slight shift in the position of the characteristic diffraction peak inherent to the sample, its crystal structure has not changed.

[0049] Figure 2 Curve 3 is the emission spectrum of the sample of this embodiment obtained under 450nm excitation. Figure 2 It can be seen that the phosphor emits broadband near-infrared light with a peak value at 819nm under ultraviolet light excitation, and its emission intensity is higher than that of the samples in Example 1 and Example 2 under the same conditions (see Figure 2 Curves 1 and 2) have both improved.

[0050] Figure 3 Curve 3 is the excitation spectrum of the sample of this embodiment obtained when monitoring 819nm. Figure 3 It can be seen that the phosphor contains two effective excitation bands, 400nm~525nm and 550nm~700nm respectively.

[0051] Example 4: Li 2.7 Mg 0.34 Nb 0.9 O 4 :0.06Cr 3+ Preparation

[0052] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.2194 g, MgO: 0.0291 g, Nb 2 O 5 : 0.2339 g, Cr 2O 3 :0.0091 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1250℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0053] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0054] Example 5: Li 2 Mg 1.3 Nb 0.33 Ta 0.33 O 4 :0.03Cr 3+ Preparation

[0055] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1150 g, MgO: 0.1056 g, Nb 2 O 5 : 0.0877 g, Ta 2 O 5 : 0.1458 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1330°C in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0056] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0057] Example 6: Li 2 Mg 1.3 Ta 0.66 O 4 :0.03Cr 3+ Preparation

[0058] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1150 g, MgO: 0.1056 g, Ta 2 O 5 : 0.2916 g, Cr 2 O3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1350℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0059] Figure 2 Curve 4 is the emission spectrum of the sample of this embodiment obtained under 450nm excitation. Figure 2 It can be seen that the phosphor emits broadband near-infrared light with a peak at 840nm under ultraviolet light excitation.

[0060] Figure 3 Curve 4 is the excitation spectrum of the sample of this embodiment obtained when monitoring 840nm. Figure 3 It can be seen that the phosphor contains two effective excitation bands, namely 445nm~550nm and 615nm~745nm.

[0061] Example 7: Li 2 Mg 0.97 Ca 0.33 Nb 0.66 O 4 :0.03Cr 3+ Preparation

[0062] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1150 g, MgO: 0.0806 g, Nb 2 O 5 : 0.0877 g, CaCO 3 : 0.0665 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1350℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0063] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0064] Example 8: Li 2 Mg 0.97 Sr 0.33Nb 0.66 O 4 :0.03Cr 3+ Preparation

[0065] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1150 g, MgO: 0.0696 g, Nb 2 O 5 : 0.0877 g, SrCO 3 : 0.1131 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1350℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0066] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0067] Example 9: Li 2 Mg 0.63 Ba 0.66 Nb 2 / 3 O 4 :0.03Cr 3+ Preparation

[0068] Weigh Li according to the stoichiometric ratio 2 CO 3 : 0.1150 g, MgO: 0.0430 g, Nb 2 O 5 : 0.0877 g, BaCO 3 : 0.1342 g, Cr 2 O 3 : 0.0048 g. Among them, due to Li 2 CO 3 The melting point is low and it is volatile. The calculated amount is 10% excess. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter at 1350℃ in an air atmosphere for 6 hours. Take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0069] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0070] Example 10: Na 2 Mg1.3 Nb 0.66 O 4 :0.03Cr 3+ Preparation

[0071] Weigh Na according to the stoichiometric ratio 2 CO 3 : 0.1829 g, MgO: 0.1596 g, Nb 2 O 5 : 0.1302 g, Cr 2 O 3 : 0.0048 g. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter it at 1150°C in an air atmosphere for 6 hours, and take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0072] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0073] Example 11: K 2 Mg 1.3 Nb 0.66 O 4 :0.03Cr 3+ Preparation

[0074] Weigh K according to the stoichiometric ratio 2 CO 3 : 0.2385 g, MgO: 0.1596 g, Nb 2 O 5 : 0.1302 g, Cr 2 O 3 : 0.0048 g. Grind and mix evenly in an agate mortar, put into a corundum crucible, cover it, place it in a high-temperature furnace, and pre-sinter it at 1150°C in an air atmosphere for 6 hours, and take it out after natural cooling; grind the obtained sintered product into a uniform powder to obtain a near-infrared phosphor.

[0075] Its crystal structure, excitation spectrum and emission spectrum are similar to those of Example 3.

[0076] From the above examples, it can be seen that the preparation method of the phosphor of the present invention is simple, pollution-free and low-cost. The material will become a near-infrared phosphor suitable for blue light excitation and has great practical value.

[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A Cr 3+ Doped broadband near-infrared phosphor, characterized in that The chemical formula of the broadband near-infrared phosphor is: (3-3x) B 4x-y C (1-x) O4: y Cr 3+ ; Wherein A is one or more of Li, Na, and K elements, B is one or more of Mg, Ca, Sr, and Ba elements, and C is one or a combination of two of Nb and Ta elements; x , y is the mole fraction, and its value range is: 0< x <1,0< y ≤0.

3.

2. A Cr according to claim 1 3+ Doped broadband near-infrared phosphor, characterized in that The crystal structure of the matrix lattice of the broadband near-infrared phosphor belongs to the cubic crystal system, and the space group is Fm3m.

3. A Cr according to claim 1 3+ Doped broadband near-infrared phosphor, characterized in that The broadband near-infrared phosphor realizes broadband near-infrared emission of 750 to 1100 nm under the excitation of blue light with a wavelength of 400 to 500 nm, and its emission peak wavelength is 815 to 845 nm.

4. A Cr 3+ The method for preparing a doped broadband near-infrared phosphor is characterized in that: The following steps are involved: Step 1: According to the chemical formula A (3-3x) B 4x-y C (1-x) O4: y Cr 3+ The stoichiometric ratio of each element in x <1,0< y ≤0.3, wherein A is one or more of Li, Na, and K, B is one or more of Mg, Ca, Sr, and Ba, and C is one or a combination of Nb and Ta; weigh one or more of the compounds of Li, Na, or K; weigh one or more of the compounds of Mg, Ca, Sr, or Ba; weigh one or more of the compounds of Nb, Ta, or tantalum; weigh a compound of Cr; all are ground in an agate mortar and mixed evenly to obtain a mixture; Step 2: placing the mixture at a temperature of 1100° C. to 1350° C. for high temperature sintering for 4 to 10 hours; Step 3: After the sintering is completed and the mixture is naturally cooled, it is ground to obtain the broadband near-infrared phosphor.

5. A Cr according to claim 4 3+ The method for preparing a doped broadband near-infrared phosphor is characterized in that: The Li compound, Na compound or K compound is one or more of oxides, carbonates, nitrates, sulfates, halides or hydroxides of the corresponding elements.

6. A Cr according to claim 4 3+ The method for preparing doped broadband near-infrared phosphor is characterized by: The compound of Mg, the compound of Ca, the compound of Sr or the compound of Ba is one or more of oxides, carbonates, nitrates, sulfates, halides or hydroxides of the corresponding elements.

7. A Cr according to claim 4 3+ The method for preparing doped broadband near-infrared phosphor is characterized by: The compound of the Nb element is one or more of niobium oxide, niobium chloride, niobium hydroxide, niobium nitrate or ammonium niobate.

8. A Cr according to claim 4 3+ The method for preparing doped broadband near-infrared phosphor is characterized by: The compound of Ta element is one or more of tantalum oxide, tantalum chloride or tantalum oxyfluoride.

9. A Cr according to any one of claims 4 to 8 3+ The method for preparing doped broadband near-infrared phosphor is characterized by: The Li element compound in the mixture is added in an amount of 105% to 120% of the amount calculated according to the stoichiometric ratio to compensate for the reduction in the stoichiometric ratio due to volatilization during the sintering process.

10. A near-infrared light-emitting device, characterized in that: It comprises the broadband near-infrared phosphor and an excitation source as described in any one of claims 1 to 3; the wavelength range of the excitation source is within the excitation wavelength range of the broadband near-infrared phosphor.

Citation Information

Patent Citations

  • Cr &lt; 3 + &gt;-doped broadband near-infrared fluorescent powder and application thereof

    CN117586774A

  • Production of laminar compound having interlaminar crosslinked structure

    JP1999139826A

  • Piezoelectric ceramic composition, method of manufacturing piezoelectric ceramic composition and piezoelectric ceramic part

    JP2004075448A