Method for extracting keratin from wool

Through cleaning and disinfection, softener pretreatment and acidolysis reaction, the problem of complex and low purity of wool extraction keratin in the prior art is solved, and the extraction of high-purity keratin is achieved, which significantly improves the repair of hair care products. Effect and hair strength.

CN118879818AInactive Publication Date: 2024-11-01LAFANG CHINA CO LTD

Patent Information

Application Number
CN202411378735.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing process of extracting keratin from wool is complicated, resulting in low extraction purity and affecting the performance of hair care products.

Method used

Using steps such as cleaning and disinfection, softener pretreatment, acidolysis reaction, neutralization reaction and activated carbon decolorization, etc., sterilization is performed by stirring and heating to finally obtain high-purity keratin with a molecular weight between 300-3000 Da.

Benefits of technology

Improves the performance of hair care products, repairs damaged hair, increases the content of disulfide bonds inside the hair, and improves the strength and overall condition of the hair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a method for extracting keratin from wool. The method comprises the following steps: A, firstly, cleaning and disinfecting the wool; b, soaking the cleaned and disinfected wool into a softener for pretreatment; c, cleaning the pretreated wool with clean water again, and drying at low temperature; d, shearing the wool which is dried at low temperature into disintegrating slag; e, firstly adding ionized water into a stirring kettle, starting stirring, then pumping concentrated sulfuric acid which is weighed in advance, adding the sheared wool according to the proportion, and carrying out acidolysis to obtain an acidolysis solution; f, after acidolysis is completed, barium hydroxide is added and slowly poured into acidolysis liquid, the pH value is adjusted to be 5.0, and continuous stirring is conducted till the pH value is stable; g, after cooling, adding activated carbon, stirring and filtering; h, heating and sterilizing the filtrate, and then adding a preservative to obtain the keratin which is added into a hair care product, so that the performance of the hair care product can be improved, damaged hair can be repaired, and the content of disulfide bonds in the hair can be increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of keratin extraction, and in particular to a method for extracting keratin from wool. Background Art

[0002] The main purpose of hair care products is to improve, restore and maintain the conditioning of hair. They are mainly used after shampooing with shampoo or soap. There are two types: rinse with water and leave-in. The purpose is to improve the combing of hair and prevent hair from tangling. When using, let them stay on the hair for a short time and then wash with water to achieve the effect of conditioning the hair. Conditioners are substances that adsorb on the surface of hair to form a coating, making the hair smooth and in good condition overall.

[0003] Wool is a common natural fiber raw material. Keratin is the main component of wool fiber, accounting for more than 90% of wool fiber. As a natural protein material, wool keratin has excellent properties such as good biocompatibility and degradability, and has good application prospects in the preparation of biomedical materials.

[0004] At present, the process of extracting keratin from wool is complicated, and the purity of the extracted keratin is low, which affects the performance of the manufactured hair care products. Therefore, it is necessary to develop a method for extracting keratin from wool. Summary of the invention

[0005] The present application provides a method for extracting keratin from wool to solve the problems of complicated extraction steps and low extraction purity in existing extraction methods, and realizes the ability to extract keratin with higher purity. When added to hair care products, the performance of the hair care products can be effectively improved, damaged hair can be repaired, and the disulfide bond content inside the hair can be increased.

[0006] The present application provides a method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 65℃-75℃, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin with a molecular weight of 300-3000Da.

[0007] Preferably, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0008] Preferably, the softener component in step B includes 2-5 parts of lanolin fatty acid, 2-6 parts of tea tree oil, 3-9 parts of polydimethylsiloxane, 1-5 parts of stearic acid polyoxyethylene ether, and 5-12 parts of deionized water in parts by weight.

[0009] Preferably, in step C, the low-temperature drying temperature is 45° C.-55° C., and the low-temperature drying time is 20 min-30 min.

[0010] Preferably, in step E, the acid hydrolysis solution is heated to 90° C.-120° C. and maintained for 24 h-48 h.

[0011] Preferably, in step G, the stirring rate is 800-1200 rpm, and the stirring time is 30 min-40 min.

[0012] Preferably, in step H, the temperature is cooled to 42°C-48°C.

[0013] Beneficial effects: (1) The extraction method of the present invention is simple and is jointly developed with Huzhou Huxing Daily Chemical Co., Ltd. The extracted keratin has high purity and can be added to hair care products to effectively improve the performance of hair care products, repair damaged hair, and increase the disulfide bond content inside the hair.

[0014] (2) The wool keratin extracted by the present invention contains a higher content of cystine / cysteine, and its amino acid composition is similar to that of hair (such as high cystine / cysteine ​​and glutamic acid content). It penetrates into the hair and builds disulfide bonds on damaged keratin bonds. Keratin improves hair strength through the disulfide bond repair mechanism.

[0015] (3) In the extraction process of the present invention, the wool is first treated with a softener and then subjected to an acid hydrolysis reaction, so that purer keratin can be extracted.

[0016] The above description is only an overview of the technical solution of the embodiment of the present application. In order to more clearly understand the technical means of the embodiment of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the embodiment of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. DETAILED DESCRIPTION

[0017] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used in the specification of the application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0019] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase "embodiments" in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0020] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application is clearly and completely described below.

[0021] Embodiment 1: The present application provides a method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 65°C, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin, the molecular weight of which is 300 Da.

[0022] In this embodiment, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0023] In this embodiment, the softener component in step B includes 2 parts of lanolin fatty acid, 6 parts of tea tree oil, 3 parts of polydimethylsiloxane, 1 part of stearic acid polyoxyethylene ether, and 5 parts of deionized water in parts by weight.

[0024] In this embodiment, the low-temperature drying temperature in step C is 45° C., and the low-temperature drying time is 20 min.

[0025] In this embodiment, in step E, the acid hydrolysis solution is heated to 90° C. and maintained for 24 hours.

[0026] In this embodiment, the stirring rate in step G is 800 rpm and the stirring time is 30 min.

[0027] In this embodiment, the temperature is cooled to 42° C. in step H.

[0028] Embodiment 2: A method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 75°C, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin, the molecular weight of which is 3000Da.

[0029] In this embodiment, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0030] In this embodiment, the softener component in step B includes 5 parts of lanolin fatty acid, 6 parts of tea tree oil, 9 parts of polydimethylsiloxane, 5 parts of stearic acid polyoxyethylene ether, and 12 parts of deionized water in parts by weight.

[0031] In this embodiment, the low-temperature drying temperature in step C is 55° C., and the low-temperature drying time is 30 min.

[0032] In this embodiment, in step E, the acid hydrolysis solution is heated to 120° C. and maintained for 48 hours.

[0033] In this embodiment, the stirring rate in step G is 1200 rpm and the stirring time is 40 min.

[0034] In this embodiment, the temperature is cooled to 48° C. in step H.

[0035] Embodiment 3: A method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 67°C, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin, the molecular weight of which is 500Da.

[0036] In this embodiment, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0037] In this embodiment, the softener component in step B includes 3 parts of lanolin fatty acid, 3 parts of tea tree oil, 5 parts of polydimethylsiloxane, 2 parts of stearic acid polyoxyethylene ether, and 6 parts of deionized water in parts by weight.

[0038] In this embodiment, the low-temperature drying temperature in step C is 47° C., and the low-temperature drying time is 22 minutes.

[0039] In this embodiment, in step E, the acid hydrolysis solution is heated to 100° C. and maintained for 30 hours.

[0040] In this embodiment, the stirring rate in step G is 900 rpm and the stirring time is 32 min.

[0041] In this embodiment, the temperature is cooled to 43° C. in step H.

[0042] Embodiment 4: A method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 72°C, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin with a molecular weight of 2800Da.

[0043] In this embodiment, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0044] In this embodiment, the softener component in step B includes 4 parts of lanolin fatty acid, 5 parts of tea tree oil, 8 parts of polydimethylsiloxane, 4 parts of stearic acid polyoxyethylene ether, and 10 parts of deionized water in parts by weight.

[0045] In this embodiment, the low-temperature drying temperature in step C is 52° C., and the low-temperature drying time is 28 min.

[0046] In this embodiment, in step E, the acid hydrolysis solution is heated to 110° C. and maintained for 46 hours.

[0047] In this embodiment, the stirring rate in step G is 1100 rpm and the stirring time is 38 min.

[0048] In this embodiment, the temperature is cooled to 47° C. in step H.

[0049] Embodiment 5: A method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 67°C, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin, the molecular weight of which is 1200Da.

[0050] In this embodiment, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0051] In this embodiment, the softener component in step B includes 3 parts of lanolin fatty acid, 5 parts of tea tree oil, 4 parts of polydimethylsiloxane, 4 parts of stearic acid polyoxyethylene ether, and 7 parts of deionized water in parts by weight.

[0052] In this embodiment, the low-temperature drying temperature in step C is 47° C., and the low-temperature drying time is 28 min.

[0053] In this embodiment, in step E, the acid hydrolyzate is heated to 95° C. and maintained for 46 hours.

[0054] In this embodiment, the stirring rate in step G is 900 rpm and the stirring time is 38 min.

[0055] In this embodiment, the temperature is cooled to 43° C. in step H.

[0056] Embodiment 6: A method for extracting keratin from wool, the keratin extraction method comprising the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 70°C, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin with a molecular weight of 2000Da.

[0057] In this embodiment, the specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

[0058] In this embodiment, the softener component in step B includes 4 parts of lanolin fatty acid, 4 parts of tea tree oil, 6 parts of polydimethylsiloxane, 3 parts of stearic acid polyoxyethylene ether, and 8 parts of deionized water in parts by weight.

[0059] In this embodiment, the low-temperature drying temperature in step C is 50° C., and the low-temperature drying time is 25 min.

[0060] In this embodiment, in step E, the acid hydrolysis solution is heated to 100° C. and maintained for 36 hours.

[0061] In this embodiment, the stirring rate in step G is 1000 rpm and the stirring time is 35 min.

[0062] In this embodiment, the temperature is cooled to 45° C. in step H.

[0063] The wool used in the present invention comes from a unique Chinese breed - Hu sheep. Hu sheep is a unique Chinese sheep breed for white lambskin. It is known for its rapid growth and development, early maturity, four-season estrus, multiple births and beautiful lambskin patterns. It is one of the few white lambskin sheep breeds in the world. It is concentrated in Jiangsu, Zhejiang and Shanghai in the Taihu Lake Basin. In recent years, a large number of Hu sheep have been introduced to western regions such as Xinjiang, Gansu and Inner Mongolia. The wool fiber of Hu sheep is delicate, long and soft. It was one of the sources for the ancients to make brushes, and it is still the source of materials for making Hu brushes in modern times. According to literature records, compared with Australian wool, Argentine wool, New Zealand wool, South African wool, Inner Mongolia wool, Gansu wool and Xinjiang wool, the wool of Hu sheep unique to China contains a higher content of crystalline regions in structure, that is, it contains a higher content of α-helical structure intermediate filaments, and the hair has the highest tensile strength and is not easy to break. The following table shows the tensile strength of different varieties of wool: It can be seen from the above table that the wool used in the present invention comes from Hu sheep, which has the best tensile strength.

[0064] Experimental example: The amino acid content of keratin extracted from each embodiment of the present invention was measured, and the data obtained are as follows:

[0065] In addition, the keratin extracted by the present invention was added to shampoo containing 15% sodium laureth sulfate, 7% cocamidopropyl betaine, an appropriate amount of pH regulator, an appropriate amount of sodium chloride, an appropriate amount of essence, and the balance of water. After the volunteers used the shampoo, they scored the perception of reduced hair breakage. If the perception of reduced hair breakage was obvious, it was scored as 10 points, and if the perception was not obvious, it was scored as 1 point. The scoring data were as follows:

[0066] As can be seen from the above table, when the keratin prepared in Example 6 was used in hair care products, volunteers perceived less hair breakage, and the keratin resulted in less hair breakage than the blank.

[0067] The wool keratin extracted by the present invention contains a higher content of cystine / cysteine, and the amino acid composition is similar to the amino acid composition of hair (such as high cystine / cysteine ​​and glutamic acid content). It penetrates into the interior of the hair and constructs disulfide bonds on damaged keratin bonds. The keratin improves the strength of the hair through the disulfide bond repair mechanism and can increase the disulfide bond content of the hair. In the extraction process of the present invention, the wool is first treated with a softener and then subjected to an acid hydrolysis reaction, so that purer keratin can be extracted.

[0068] In summary, the extraction method of the present invention is simple and is jointly developed with Huzhou Huxing Daily Chemical Co., Ltd. The extracted keratin has high purity and can be added to hair care products to effectively improve the performance of hair care products, repair damaged hair, and increase the disulfide bond content inside the hair.

[0069] As described above, the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A method for extracting keratin from wool, characterized in that: The keratin extraction method includes the following steps: A. First, clean and disinfect the wool; B. Soak the cleaned and disinfected wool in softener for pretreatment; C. Wash the pretreated wool again with clean water and dry at low temperature; D. Cut the low-temperature dried wool into pieces; E. Acid hydrolysis reaction: first add ionized water into the stirring kettle, start stirring, then draw in pre-weighed concentrated sulfuric acid, add shredded wool according to the proportion, perform acid hydrolysis, and obtain an acid hydrolyzate; F. Neutralization reaction: After the acid hydrolysis is completed, add barium hydroxide and slowly pour it into the acid hydrolysis solution to adjust the pH value to 5.0, and continue stirring until the pH value reaches a stable value; G. Activated carbon decolorization: After cooling to 65℃-75℃, add activated carbon, stir, and filter; H. The filtrate is pumped into a special sterilizing pot according to the ratio of hydrolyzed keratin and disodium EDTA specified in the finished product formula, and heated and sterilized. After the sterilization is completed and cooled, a preservative is added, and the mixture is packaged after being stirred evenly to obtain keratin with a molecular weight of 300-3000Da.

2. A method for extracting keratin from wool according to claim 1, characterized in that: The specific operation process of step A is as follows: a. Put the wool into clean water and rinse it with clean water; b. Use 75% disinfectant to remove viruses and bacteria carried by wool; c. Rinse again with clean water after disinfection.

3. The method for extracting keratin from wool according to claim 1, characterized in that: The softener components in step B include 2-5 parts of lanolin fatty acid, 2-6 parts of tea tree oil, 3-9 parts of polydimethylsiloxane, 1-5 parts of stearic acid polyoxyethylene ether, and 5-12 parts of deionized water in parts by weight.

4. The method for extracting keratin from wool according to claim 1, characterized in that: In step C, the low-temperature drying temperature is 45° C.-55° C., and the low-temperature drying time is 20 min-30 min.

5. The method for extracting keratin from wool according to claim 1, characterized in that: In the step E, the acid hydrolysis solution is heated to 90° C.-120° C. and maintained for 24 h-48 h.

6. The method for extracting keratin from wool according to claim 1, characterized in that: In step G, the stirring rate is 800-1200 rpm, and the stirring time is 30 min-40 min.

7. The method for extracting keratin from wool according to claim 1, characterized in that: In the step H, the mixture is cooled to 42°C-48°C.

Citation Information

Patent Citations

  • Liquid shampoo for nourishing hair and preventing break and phalacrosis

    CN101129313A

  • Natural plant liquid shampoo

    CN107049846A

  • Method for production of amino-acid plant tonic liquor and product thereof

    CN1123261A

  • Yak hair keratin extraction method

    CN113512204A

  • Method for preparing keratin solution by hydrolyzing wool

    CN113855588A

Cited By

  • Elastin emulsion capable of improving toughness and elasticity of hair as well as preparation method and application of elastin emulsion

    CN119326678A

  • Elastin essence capable of improving toughness and elasticity of hair

    CN119326679A