Production method of steel for semi-floating type automobile half shaft

By controlling the steel composition and process parameters through converter smelting, LF refining, RH refining and continuous casting heating rolling, the problem of substandard hardness and static torsional strength of steel for axles in existing methods has been solved, and high-quality steel for semi-floating automotive axles has been produced.

CN118879980APending Publication Date: 2024-11-01LINGYUAN IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410974535.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing methods for producing tempered and non-tempered half-shafts cannot simultaneously meet requirements for hardness, static torsional strength, etc., resulting in unstable product quality.

Method used

The process involves converter smelting, LF refining, RH refining, and continuous casting heating rolling. By controlling the steel composition and process parameters, reducing oxygen and boron content, the hardenability and cleanliness of the steel are ensured.

Benefits of technology

We have produced semi-floating automotive half-shaft steel with stable hardenability and high static torsional strength, which meets the requirements for automotive half-shaft use without increasing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879980A_ABST
    Figure CN118879980A_ABST
Patent Text Reader

Abstract

The invention provides a production method of steel for a semi-floating automobile half axle, which comprises the following steps of: smelting molten steel by a converter, refining the molten steel by an LF (ladle furnace), refining the molten steel by an RH (Ruhrstahl Heraeus), continuously casting a blank and heating and rolling to produce the steel for the semi-floating automobile half axle, so that the low boron content of the steel for the semi-floating automobile half axle is ensured; the low-oxygen low-inclusion-content index is guaranteed, the stable hardenability and the high static torsional strength are guaranteed, the requirements of the steel for the semi-floating type automobile half shaft are met, the oxygen content reaches 0.0010% or below, the boron content reaches 0.0004% or below, and the steel can be used for manufacturing the semi-floating type automobile half shaft through the low-oxygen low-inclusion-content index, the stable hardenability and the high static torsional strength. A series of requirements of the steel for the automobile half axle on the quenched and tempered core hardness, surface hardness, effective hardened layer depth, metallographic structure level and the like are completely met, the static torsional strength is high and can be larger than or equal to 7200 N.m, the product quality is stable, and the comprehensive performance is excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of half-axle production, and more specifically, relates to a production method for steel used for a half-axle of a semi-floating vehicle. Background Art

[0002] Automobile axles are important force-transmitting components of automobiles. They need to transmit the torque of the engine and withstand the force of the wheels. They have high requirements on the quality of the raw materials used. The steel used for automobile axles is usually 40Cr, 42CrMo, and 40MnBH. Among them, the 40Cr steel in the GB / T3077-2015 alloy structural steel standard has no requirements for boron content, oxygen content, and inclusions. The boron content in the steel produced by conventional methods is 0.0005% to 0.0009%, and the gas oxygen content is high, resulting in unstable hardenability and poor cleanliness of the steel. After quenching and tempering, automobile axles often have uneven hardness, quenching cracking, low static torsional strength, and other problems that lead to subsequent failures.

[0003] The patent (CN113430463A) discloses "a medium-carbon boron-containing non-quenched and tempered steel and its preparation method". The invention provides a method for preparing steel for automobile half-axles that can be used without quenching and tempering. The steel comprises, by mass percentage: C: 0.37-0.42%, Si: 0.17-0.37%, Mn: 1.40-1.70%, Cr: 0.20-0.60%, B: 0.0008-0.0035%, Ti: 0.015-0.045%, P: ≤0.025%, S: ≤0.035%. The strength of the steel after hot rolling is improved by increasing Mn, adding Ti and B, so that the obtained automobile half-axle steel can be used without quenching and tempering, and has good performance. The tensile strength of the steel after hot rolling is 760-880MPa, and the yield strength is ≥460MPa.

[0004] The method provided in the patent (CN113430463A) fills the gap in the field of automobile half-axle steel due to the poor performance of non-quenched and tempered steel. However, the patent (CN113430463A) produces automobile half-axle steel by adding Mn, Ti and B, which is costly, and the strength and grain size of the obtained automobile half-axle steel are still lower than those of quenched and tempered steel. Summary of the invention

[0005] The purpose of the present invention is to provide a method for producing steel for semi-floating automobile half-axles in view of the deficiencies in the existing technology, so as to solve the problem that the existing tempered half-axle production method and non-tempered half-axle production method mentioned in the above background technology cannot obtain half-axles that meet the requirements of hardness, static torsional strength, etc., and the product quality is unstable.

[0006] In order to achieve the above object, the present invention provides a method for producing steel for a semi-floating automobile half-axle, the production method comprising:

[0007] Converter smelting of molten steel, including smelting of steel materials, controlling the C component by mass percentage to ≥ 0.08%, and the P component by mass percentage to ≤ 0.015%;

[0008] According to the final carbon, alloy elements and slag are added in sequence after steel is tapped, among which the full aluminum ingot is used for deoxidation, and argon gas is used throughout the process from steel tapping to hanging ladle;

[0009] LF refining molten steel includes passing argon gas through the molten steel, controlling the heating rate, adding slag-making materials, diffusion deoxidation, adjusting the aluminum composition when the white slag is formed and reaches the set temperature, continuing diffusion deoxidation, and keeping the white slag for ≥15min. After good deoxidation, alloy elements are added according to the composition control target, and calcium wire is fed according to the Als content;

[0010] RH refining of molten steel includes degassing of the molten steel and then passing argon gas to make the molten steel composition reach the control target;

[0011] Continuously casting the billet, including flowing molten steel into a tundish, and then into a crystallizer, and continuously casting into a cross-section billet;

[0012] Heating rolling includes heating the ingot using three-stage heating and rolling it using a rolling mill.

[0013] Preferably, alloy elements and slag are added in sequence after steel is tapped, including: aluminum ingots, medium carbon ferromanganese, ferrosilicon, high carbon ferrochrome, carburizer, low boron refined slag and refined lime are added in sequence after 1 / 4 of the steel is tapped, and all the addition is completed when 3 / 4 of the steel is tapped.

[0014] Preferably, alloy elements and slag are added in sequence after steel is tapped, and the method further comprises: baking the alloy elements before adding the alloy elements.

[0015] Preferably, when the white slag is formed and reaches the set temperature, the aluminum composition is adjusted, including taking a first sample for testing when the white slag is formed and reaches the set temperature, adjusting the composition based on the sampling results, and when the first sample Als≤0.025%, adjusting the aluminum to above 0.030%.

[0016] Preferably, the calcium wire is fed according to the Als content before feeding, including: the wire feeding speed is controlled at 1.5 m / s.

[0017] Preferably, the degassing treatment of the molten steel includes maintaining the working vacuum degree of the molten steel vacuum chamber at ≤67Pa for 12 minutes, so that [H] in the molten steel is ≤2.0ppm and the target value [H] is ≤1.5ppm.

[0018] Preferably, the argon treatment includes adding a covering agent to the molten steel, adjusting the argon gas so that the liquid surface creeps and the molten steel is not exposed, starting the soft blowing timing, and the soft blowing time is ≥20 minutes.

[0019] Preferably, the molten steel flows into the tundish and then into the crystallizer, including: the tundish temperature is maintained at 1512-1532°C, the pulling speed is maintained at 1.00m / min, the specific water volume is maintained at 0.33L / Kg, and the crystallizer water flow rate is maintained at 115±3m3 / h.

[0020] Preferably, continuous casting into cross-section ingots comprises: using rectangular medium-carbon steel protective slag as the mold protective slag, continuously casting into 200mm×240mm cross-section ingots, and stack cooling the ingots for a time of ≥48h.

[0021] Preferably, the ingot is heated using three-stage heating, and rolled using a rolling mill, including: heating stage I temperature ≤ 1040°C, heating stage II temperature 1140°C ~ 1210°C, soaking stage temperature 1150°C ~ 1220°C. The residence time in the furnace for heating stage I is 31min ~ 54min, the residence time in the furnace for heating stage II is 32min ~ 55min, and the residence time in the soaking furnace is 22min ~ 36min. The rolling is carried out using a two-roller short stress line rolling mill with alternating arrangement of vertical and horizontal rollers in a row, wherein the starting rolling temperature is 1060°C ~ 1140°C, the final rolling temperature is 940°C ~ 1020°C, and the semi-axle steel after rolling should be quickly collected after being put on the cooling bed.

[0022] The present invention provides a method for producing steel for a semi-floating automobile half-axle, which has the following beneficial effects:

[0023] This production method adopts the process path of converter smelting molten steel, LF refined molten steel, RH refined molten steel, continuous casting billet and hot rolling to produce steel for semi-floating automobile half-axles, which not only ensures the low boron content of the steel for semi-floating automobile half-axles, but also ensures low oxygen and low inclusion content indicators, and also ensures stable hardenability and high static torsional strength, meeting the needs of steel for semi-floating automobile half-axles.

[0024] The purpose of the production method is to ensure that the steel for the automobile half-axle has lower oxygen and boron contents, clean steel and stable hardenability by reasonably selecting process routes and raw materials, optimizing component design and controlling process parameters without increasing costs; the oxygen content is within 0.0010%, and the boron content is within 0.0004%, which fully meets a series of requirements of the automobile half-axle for the core hardness, surface hardness, effective hardened layer depth, metallographic structure level and the like after quenching and tempering, and has high static torsional strength, which can reach ≥7200N·m, stable product quality and excellent comprehensive performance.

[0025] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, wherein like reference numerals generally represent like components throughout the exemplary embodiments of the present invention.

[0027] Figure 1 A flow chart of a method for producing steel for a semi-floating vehicle half-axle according to an embodiment of the present invention is shown. DETAILED DESCRIPTION

[0028] The preferred embodiments of the present invention will be described in more detail below. Although the preferred embodiments of the present invention are described below, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.

[0029] In order to solve the problem that the existing quenched and tempered half-axle production method and the non-quenched and tempered half-axle production method cannot obtain the half-axle to meet the requirements of hardness, torsional strength and the like, and the product quality is unstable, the present invention provides a production method for semi-floating automobile half-axle steel, the production method comprises the following steps: smelting molten steel in a converter, refining molten steel in a LF ladle refining furnace, refining molten steel by RH vacuum degassing, continuous casting of 200mm×240mm cross-section rectangular billet, and hot rolling. The composition of the molten steel in the steps is controlled by mass percentage to be C: 0.37-0.43%, Si: 0.20-0.35%, Mn: 0.63-0.75%, Cr: 0.87-1.00%, P: ≤0.025%, S: ≤0.025%, B: ≤0.0004%, Cu: ≤0.20%, Ni: ≤0.20%, O: ≤0.0020%, and the balance is iron and inevitable impurities. The production method comprises the following specific steps:

[0030] The converter smelts molten steel, including smelting iron and steel materials, controlling the C component in mass percentage ≥ 0.08%, and the P component in mass percentage ≤ 0.015%, adding alloy elements and slag in sequence after steelmaking according to the end carbon, wherein all-aluminum ingots in the alloy elements are used for deoxidation, and argon gas treatment is used throughout the process from steelmaking to hanging.

[0031] Specifically, according to the conventional method, converter smelting is carried out, the C component of the steel is controlled at ≥0.08% by mass percentage, double-block slag is used for steel tapping, the amount of slag is strictly controlled to prevent the top slag from returning to phosphorus, and the P component is controlled at ≤0.015% by mass percentage; according to the end carbon, aluminum ingots, medium carbon ferromanganese, ferrosilicon, high carbon ferrochrome, carburizer, low boron refining slag and refining (top) lime are added in sequence after 1 / 4 of the steel is tapped, and the addition is completed when 3 / 4 of the steel is tapped, and it is not allowed to add alloy elements and slag to the ladle before tapping; the double permeable bricks of the ladle are good, argon is passed throughout the process from tapping to hanging the ladle, and the alloy elements used must be baked before use; the composition is controlled by mass percentage as C: 0.30%~0.35%, Mn: 0.63%~0.69%, Si: 0.23%~0.29%, Cr: 0.88%~0.94%, Als: 0.030%~0.040% when the converter leaves the station.

[0032] LF refining molten steel includes passing argon gas through the molten steel, controlling the heating rate, adding slag-making materials, adjusting the aluminum composition when the white slag is formed and reaches the set temperature, continuing diffusion deoxidation, and keeping the white slag for ≥15 minutes. After good deoxidation, alloy elements are added according to the composition control target, and calcium wire is fed according to the Als content.

[0033] Specifically, the ladle is first blown with strong argon from the ladle seat to the soft blowing station, and the argon flow rate is controlled at 600-700NL / min for 1 minute. After the ventilation is normal, the argon is adjusted to weak blowing, and the argon flow rate is controlled at 200-300NL / min, and then it enters the smelting station; the argon is adjusted to medium blowing when the ladle enters the smelting station, and the argon flow rate is controlled at 400-500NL / min, and then the temperature is measured, and the voltage and current are reasonably controlled according to the temperature and production rhythm. Heating rate, adding slag-making materials in batches, lime, low-boron refined slag, etc. are selected as slag-making materials, and the weight of each batch is not more than 100kg to prevent slag from agglomerating; adding deoxidizer to the slag surface for diffusion deoxidation, after 10 minutes of power on, the slag melts and has good fluidity, and white slag is formed. When the temperature is 1530-1540℃, the power is turned off and argon is blown for 2 minutes, and the first sample is taken for testing; taking slag samples to observe the slag condition, according to the sampling results, the composition is adjusted according to the required chemical composition internal control lower limit, when the first sample Als ≤ 0.025%, aluminum is adjusted to more than 0.030%, and aluminum is avoided in the later stage; continue diffusion deoxidation, maintain the reducing atmosphere until leaving the station, and the white slag retention time ≥ 15min; after good deoxidation, add medium carbon ferromanganese, high carbon ferrochrome and other alloys according to the control composition target to adjust the composition to the target; after the composition is qualified and the temperature is appropriate, feed the calcium wire according to the Als content of the sample before feeding the wire, the reference amount = Als × 4~6 rounded number, and the lower limit of calcium wire feeding is not less than 50m, and the reference feeding speed is 1.5m / s; the LF endpoint composition is controlled by mass percentage as C: 0.38%~0.40%, Mn: 0.70%~0.73%, Si: 0.26%~0.32%, Cr: 0.92%~0.98%, S: ≤0.015%, P: ≤0.020%, B: ≤0.0004%, Als: 0.025%~0.035%.

[0034] RH refining of molten steel includes degassing of the molten steel and then passing argon gas to make the molten steel composition reach the control target.

[0035] Specifically, the ladle moves from the ladle seat to the RH degassing station, the working vacuum degree of the RH refined molten steel vacuum chamber is ≤67Pa and maintained for 12min, [H] in the molten steel is ≤2.0ppm, and the target value [H] is ≤1.5ppm. After the degassing is completed, the ladle is opened to the soft blowing station to add a covering agent, and at the same time, the argon gas is adjusted to make the liquid surface creep and the molten steel not exposed, and the soft blowing timing is started. The soft blowing time is ≥20min, and the RH endpoint composition is controlled by mass percentage to be C: 0.38%~0.40%, Mn: 0.67%~0.73%, Si: 0.26%~0.32%, Cr: 0.92%~0.98%, S: ≤0.015%, P: ≤0.020%, B: ≤0.0004%, Als: 0.020%~0.030%.

[0036] Continuous casting of billets includes flowing molten steel into a tundish, then into a crystallizer, and continuously casting into cross-section billets.

[0037] Specifically, the tundish temperature is controlled at 1512-1532°C, the pulling speed is controlled at 1.00m / min, the specific water volume is controlled at 0.33L / Kg, the water flow rate of the crystallizer is controlled at 115±3m3 / h, and the electromagnetic stirring parameters are M-EMS: 240A / 2.5Hz; F-EMS: 350A / 6.5Hz. The whole process protective casting is strictly implemented, and the crystallizer protective slag uses rectangular medium carbon steel protective slag, and the continuous casting is into 200mm×240mm cross-section ingots, and the ingots are pile cooled for ≥48h.

[0038] Heating rolling includes: heating the ingot using three-stage heating and rolling it using a rolling mill.

[0039] Specifically, heating adopts a walking beam regenerative heating furnace with an effective length of 30.0m. The heating furnace adopts three-stage heating, and the total residence time of the ingot in the furnace is not less than 85min; the temperature of heating section I is ≤1040℃, the temperature of heating section II is 1140℃~1210℃, and the temperature of the soaking section is 1150℃~1220℃; the residence time in the furnace of heating section I is 31min~54min, the residence time in the furnace of heating section II is 32min~55min, and the residence time in the furnace of soaking section is 22min~36min; rolling adopts a two-roll short stress line rolling mill with a sequential vertical and horizontal alternating (rough rolling 7 + finishing rolling 4), wherein the starting rolling temperature is 1060℃~1140℃, and the final rolling temperature is 940℃~1020℃. After rolling, the semi-axle steel should be quickly collected on the cooling bed, the collection and stacking temperature should be increased, and it should be stacked in a windproof place to ensure sufficient slow cooling.

[0040] In summary, the production method can control the composition of molten steel in mass percentage to C: 0.37-0.43%, Si: 0.20-0.35%, Mn: 0.63-0.75%, Cr: 0.87-1.00%, P: ≤0.025%, S: ≤0.025%, B: ≤0.0004%, Cu: ≤0.20%, Ni: ≤0.20%, O: ≤0.0020%, and the remainder is iron and unavoidable impurities.

[0041] The production method adopts the process of smelting molten steel in a converter, LF refined molten steel and RH refined molten steel in external refining, continuously casting 200mm×240mm cross-section rectangular billets, and hot rolling φ70mm bars to obtain a steel for automobile half-axles with stable hardenability and high cleanliness. The core hardness, surface hardness, effective hardened layer depth and metallographic structure level of the automobile half-axle steel after quenching and tempering meet the use requirements of automobile half-axles, the static torsional strength is ≥7200N·m, and the comprehensive performance is excellent.

[0042] The converter smelting steel adopts the all-aluminum ingot deep deoxidation process to improve the cleanliness of the molten steel, and uses medium-carbon ferromanganese and ferrosilicon instead of silicon-manganese alloy to control the boron content in the steel.

[0043] The slag-making material for LF refined steel liquid is low-boron refined slag, and the boron content is controlled at ≤0.0050%. The boron content in the refined slag is controlled to avoid the reduction of boron in the refined slag to the steel during the refining process.

[0044] Example

[0045] Converter smelting molten steel, including:

[0046] The steel material is molten iron (118.2t) with scrap steel (13t), and is smelted in a converter according to the conventional method. The C component of the steel is controlled to be 0.113% by mass percentage, and the P component is controlled to be 0.012% by mass percentage. The steel tapping temperature is 1628℃. After 1 / 4 of the steel is tapped, 143kg of pre-deoxidizer aluminum ingot, 150kg of carburizer, 868kg of medium carbon ferromanganese, 361kg of ferrosilicon, and high carbon chromium iron are added in sequence. 1940kg, 480kg low-boron refined slag and 296kg refined (top) lime are added when 3 / 4 of the steel is tapped. All alloys are baked and double slag is used to control the slag amount during tapping. The double air-permeable bricks of the ladle are in good condition, and argon is passed throughout the process from tapping to hanging the ladle. When the converter leaves the station, the composition is controlled by mass percentage as C: 0.311%, Mn: 0.64%, Si: 0.263%, Cr: 0.88%, Als: 0.029%.

[0047] LF refined molten steel, including:

[0048] When the ladle moves from the ladle seat to the soft blowing station, argon strong blowing is first started, and the argon flow rate is controlled at 650NL / min for 1 minute. After the ventilation is normal, the argon is adjusted to weak blowing, and the argon flow rate is controlled at 300NL / min, and then it enters the smelting station; when the ladle enters the smelting station, the argon is adjusted to medium blowing, and the argon flow rate is controlled at 500NL / min. Then the temperature is measured, and the voltage and current are selected according to the temperature and production rhythm to reasonably control the heating rate. Slag-making materials are added in batches. The slag-making materials are 356kg of lime, 57kg of silica, and 360kg of low-boron refined slag. The weight of each batch is not more than 100kg to prevent the slag from agglomerating. Deoxidizer is added to the slag surface. The deoxidizer is selected from 224kg of calcium carbide and 20kg of aluminum particles. Mix and add in batches for diffusion deoxidation. After 10 minutes of power-on, the slag melts and has good fluidity, white slag is formed, and the temperature is When the temperature is 1539℃, turn off the power and blow in argon for 2 minutes, then take the first sample for testing; take the slag sample and observe that the slag is white slag. According to the sampling result, adjust the composition according to the required lower and middle limits of the internal control of the chemical composition, continue diffusion deoxidation, maintain the reducing atmosphere until leaving the station, and keep the white slag for 25 minutes; after good deoxidation, add 108kg of medium carbon ferromanganese, 109kg of high carbon ferrochrome, and 50kg of recarburizer according to the control composition target, and adjust the composition to the target; after the composition is qualified and the temperature is appropriate, feed 180m of calcium wire at a feeding speed of 1.5m / s; the LF endpoint composition is controlled by mass percentage as C: 0.384%, Mn: 0.71%, Si: 0.294%, Cr: 0.94%, S: 0.000%, P: 0.012%, B: 0.0003%, Als: 0.033%.

[0049] RH refined steel, including:

[0050] The ladle moves from the ladle seat to the RH degassing station. The working vacuum degree of the RH refined molten steel vacuum chamber is ≤67Pa and maintained for 12 minutes and 22 seconds. The [H] in the molten steel is 1.03ppm. After the degassing is completed, it is opened to the soft blowing station to add a covering agent. At the same time, the argon liquid level is adjusted to creep slightly. The molten steel is not exposed. The soft blowing time is 22min. The RH endpoint composition is controlled by mass percentage as C: 0.388%, Mn: 0.70%, Si: 0.29%, Cr: 0.94%, S: ≤0.000%, P: ≤0.012%, B: ≤0.0003%, Als: 0.026%.

[0051] Continuous casting billets, including:

[0052] The temperature of the tundish is controlled at 1525℃, 1530℃, 1531℃, and 1528℃, the pulling speed is controlled at 1.00m / min, the specific water volume is controlled at 0.33L / Kg, the water flow rate of the crystallizer is controlled at 115±3m3 / h, and the electromagnetic stirring parameters are M-EMS: 240A / 2.5Hz; F-EMS: 350A / 6.5Hz; the whole process protective casting is strictly implemented, and the crystallizer protective slag uses rectangular medium carbon steel protective slag, and the continuous casting is into 200mm×240mm cross-section ingot, and the ingot is pile cooled for 50h.

[0053] Heated rolling, including:

[0054] Heating adopts a 30.0m effective length walking beam regenerative heating furnace, the heating furnace adopts three-stage heating, and the total residence time of the billet in the furnace is not less than 85min; the temperature of heating section I is 1019℃~1026℃, the temperature of heating section II is 1161℃~1172℃, and the temperature of the soaking section is 1185℃~1194℃. The residence time in the furnace of heating section I is 47min~51min, the residence time in the furnace of heating section II is 49min~52min, and the residence time in the furnace of soaking section is 33min~36min; rolling adopts a two-roller short stress line rolling mill with a sequential vertical horizontal alternation (rough rolling 7+finishing rolling 4), in which the starting rolling temperature is 1070℃~1098℃, and the final rolling temperature is 965℃~994℃. After rolling, the semi-axle steel should be quickly collected on the cooling bed, the collection and stacking temperature should be increased, and the stacking should be placed in a sheltered place to ensure sufficient slow cooling.

[0055] In summary, the properties of the half-axle steel produced by the production method of the half-axle steel for semi-floating vehicles of the present invention are as follows:

[0056] Axle shaft steel cleanliness:

[0057] The oxygen content of the steel used for the half shaft is 0.00073%, the inclusions of category A are 0.5, category B are both 0.5, category C are all 0, category D is 0.5, category Ds is 0, and has a high degree of cleanliness.

[0058] Axle blank and product inspection results:

[0059] Surface hardness after quenching. The surface hardness of the half-shaft blank after quenching is tested and the results are shown in Table 1: all meet the requirements.

[0060] Table 1: Surface hardness after quenching, HRC

[0061]

[0062]

[0063] The hardness of the core (1 / 2R) after high temperature tempering. The hardness results of the core (1 / 2R) after high temperature tempering are shown in Table 2: all meet the requirements.

[0064] Table 2: Hardness after high temperature tempering, HRC

[0065]

[0066] The metallographic structure after quenching and tempering and the metallographic structure grade results after quenching and tempering are shown in Table 3: all meet the requirements.

[0067] Table 3: Metallographic structure level after quenching and tempering, level

[0068]

[0069] The surface hardness after low temperature tempering and the surface hardness results after low temperature tempering are shown in Table 4: all meet the requirements.

[0070] Table 4: Surface hardness after low temperature tempering, HRC

[0071] Detection area Hardness 1 Hardness 2 average value Require Eligibility spline surface 54 54 54 48~52 qualified Rod surface 53.5 54 53.8 52~58 qualified

[0072] The effective hardened layer depth and the effective hardened layer depth after low temperature tempering are shown in Table 5: all meet the requirements.

[0073] Table 5: Effective hardened layer depth, mm

[0074]

[0075]

[0076] Static torsional strength. The static torsional strength results are shown in Table 6: All meet the requirements, and the half-axle product has high static torsional strength.

[0077] Table 6: Static torsional strength, N·m

[0078]

[0079] While various embodiments of the present invention have been described, the above description is intended to be exemplary, not exhaustive, and not limited to the disclosed embodiments. Many modifications and variations will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments.

Claims

1. A method for producing steel for a semi-floating vehicle half-axle, characterized in that: The production method comprises: Converter smelting of molten steel, including smelting of steel materials, controlling the C component by mass percentage to ≥ 0.08%, and the P component by mass percentage to ≤ 0.015%; According to the final carbon, alloy elements and slag are added in sequence after steel is tapped, among which the full aluminum ingot is used for deoxidation, and argon gas is used throughout the process from steel tapping to hanging ladle; LF refining molten steel includes passing argon gas through the molten steel, controlling the heating rate, adding slag-making materials, diffusion deoxidation, adjusting the aluminum composition when the white slag is formed and reaches the set temperature, continuing diffusion deoxidation, and keeping the white slag for ≥15min. After good deoxidation, alloy elements are added according to the composition control target, and calcium wire is fed according to the Als content; RH refining of molten steel includes degassing of the molten steel and then passing argon gas to make the molten steel composition reach the control target; Continuously casting the billet, including flowing molten steel into a tundish, and then into a crystallizer, and continuously casting into a cross-section billet; Heating rolling includes heating the ingot using three-stage heating and rolling it using a rolling mill.

2. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: After steel is tapped, alloy elements and slag are added in sequence, including: aluminum ingots, medium carbon ferromanganese, ferrosilicon, high carbon ferrochrome, carburizer, low boron refined slag and refined lime are added in sequence after 1 / 4 of the steel is tapped, and all are added when 3 / 4 of the steel is tapped.

3. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: After the steel is tapped, alloy elements and slag are added in sequence, and the process also includes: baking the alloy elements before adding them.

4. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: When the white slag is formed and reaches the set temperature, the aluminum composition is adjusted, including taking the first sample for testing, adjusting the composition based on the sampling results, and when the first sample Als≤0.025%, adjusting the aluminum to above 0.030%.

5. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: Feed the calcium wire according to the Als content before feeding, including: controlling the feeding speed at 1.5m / s.

6. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: The degassing treatment of molten steel includes maintaining the working vacuum degree of the molten steel vacuum chamber at ≤67Pa for 12 minutes, so that [H] in the molten steel is ≤2.0ppm and the target value [H] is ≤1.5ppm.

7. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: Argon treatment includes adding covering agent to the molten steel and adjusting the argon gas to make the liquid surface creep and the molten steel not exposed. The soft blowing timing starts and the soft blowing time is ≥20min.

8. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: The molten steel flows into the tundish and then into the crystallizer, including: the tundish temperature is maintained at 1512-1532°C, the pulling speed is maintained at 1.00m / min, the specific water volume is maintained at 0.33L / Kg, and the crystallizer water flow rate is maintained at 115±3m3 / h.

9. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: Continuously casting into cross-section ingots, including: using rectangular medium carbon steel protective slag as the mold protective slag, continuously casting into 200mm×240mm cross-section ingots, and stack cooling the ingots for a time of ≥48h.

10. The method for producing steel for a semi-floating vehicle half-axle according to claim 1, characterized in that: The ingot is heated by three-stage heating and rolled by a rolling mill, including: heating stage I temperature ≤ 1040℃, heating stage II temperature 1140℃~1210℃, soaking stage temperature 1150℃~1220℃. The residence time in the furnace of heating stage I is 31min~54min, the residence time in the furnace of heating stage II is 32min~55min, and the residence time in the soaking furnace is 22min~36min. The rolling is carried out by a two-roller short stress line rolling mill with alternating arrangement of vertical and horizontal in series, wherein the starting rolling temperature is 1060℃~1140℃, the final rolling temperature is 940℃~1020℃, and the semi-axle steel after rolling should be quickly collected after being put on the cooling bed.