Steel material and preparation method and application thereof

Through pulse current-assisted rolling and heat treatment processes, steel with high strength and good anti-hydrogen embrittlement properties was prepared, which solved the problem that traditional methods were difficult to improve anti-hydrogen embrittlement properties and achieved safer steel applications.

CN118879999APending Publication Date: 2024-11-01BEIJING GRAPHENE TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410832513.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

There are bottlenecks in existing steels in terms of high strength and anti-hydrogen embrittlement properties. Traditional hydrogen removal methods are difficult to effectively improve the anti-hydrogen embrittlement properties of materials, especially during service, the hydrogen embrittlement problem caused by external hydrogen invasion still has serious harm.

Method used

Using pulse current assisted rolling and heat treatment processes, uniformly distributed non-common cementite nanophase and non-common co-carbonized vanadium carbide nanophase are prepared through Joule thermal and polarization effects, which enhances the strength of the steel and improves the anti-hydrogen embrittlement properties. .

Benefits of technology

The anti-hydrogen embrittlement properties of steel are significantly improved, and hydrogen is effectively captured through the uniform distribution of nano-precipitation phases and the deep hydrogen trap effect, reducing the risk of brittle fracture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879999A_ABST
    Figure CN118879999A_ABST
Patent Text Reader

Abstract

The invention provides a steel material and a preparation method and application thereof. The preparation method of the steel material comprises the following steps that raw materials of the steel material are provided and mixed, and a to-be-rolled material is prepared; the to-be-rolled material is subjected to pulse current auxiliary rolling, and a plate is prepared; the plate is subjected to a pulse current auxiliary heat treatment process, and a steel material is prepared; the heat treatment comprises quenching and tempering. According to the method, a composite precipitated phase of a non-coherent cementite nanophase and a non-coherent vanadium carbide nanophase which are uniformly dispersed and distributed is prepared through a Joule heating effect and a polarization effect generated by pulse current in an auxiliary rolling and heat treatment process, so that the strength of a steel material is enhanced; a composite precipitated phase of a non-coherent cementite nanophase and a non-coherent vanadium carbide nanophase dispersed in the structure of the steel material is more uniform, and the composite precipitated phase can serve as a deep hydrogen trap to capture hydrogen more widely in the service process of the steel material, so that the hydrogen embrittlement resistance of the steel material is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metal materials, and in particular to a steel material and a preparation method and application thereof. Background Art

[0002] In order to ensure the safety and reliability of steel materials in the machinery, aerospace, electronics and other industries, the strength and hydrogen embrittlement resistance of steel need to meet higher standards. The strength and hydrogen embrittlement resistance of steel, whether in the production and preparation processes such as smelting, rolling, heat treatment, welding or electroplating, or in the engineering application links such as storage, transportation and service, have always been an important bottleneck restricting its development and application. Generally speaking, the higher the strength, the greater the sensitivity to hydrogen embrittlement. At the same time, brittle fracture is also one of the most dangerous failure modes in engineering components. It is because after hydrogen enters the metal, the local hydrogen concentration reaches saturation, causing the metal plasticity to decrease, resulting in premature failure of the structure. The irregular and sudden nature of brittle fracture may cause catastrophic accidents, resulting in huge casualties and economic losses.

[0003] After continuous research, it is found that the traditional concept of removing large-particle second phase and reducing hydrogen content in high-strength steel production cannot better improve the material's resistance to hydrogen embrittlement. The best way is to make hydrogen evenly dispersed in the grains. The traditional means of dehydrogenation are still limited to raw material control, steel liquid vacuum degassing and stacking slow cooling. These methods can only solve the internal hydrogen embrittlement problem to a certain extent. The external hydrogen embrittlement problem caused by hydrogen intrusion in high-strength steel during service will eventually cause serious harm. Summary of the invention

[0004] Based on this, it is necessary to provide a steel material with high strength and good resistance to hydrogen embrittlement and a preparation method and application thereof.

[0005] The present application provides a method for preparing a steel material, comprising the following steps:

[0006] Providing raw materials of steel materials, mixing them, and preparing materials to be rolled;

[0007] The material to be rolled is subjected to pulse current assisted rolling to prepare a plate;

[0008] The plate is subjected to a pulse current assisted heat treatment process to prepare a steel material; the heat treatment includes quenching and tempering.

[0009] In one embodiment, the conditions for the pulse current assisted rolling include: an effective pulse current density of 400 A / mm 2 ~480 A / mm 2 The processing time is 1min~5 min.

[0010] In one embodiment, the conditions for the pulse current assisted rolling also include one or more of the following:

[0011] (1) Pulse power supply is 220V~380V;

[0012] (2) Frequency: 30 Hz to 80 Hz;

[0013] (3) Output voltage is 3V~8V;

[0014] (4) The rolling reduction is 30% to 70% of the height of the material to be rolled.

[0015] In one embodiment, the heat treatment satisfies one or both of the following conditions:

[0016] (1) The quenching conditions include an effective pulse current density of 350 A / mm 2 ~410 A / mm 2 , processing time 5min ~10min;

[0017] (2) The tempering conditions include an effective pulse current density of 120 A / mm 2 ~230 A / mm 2 , processing time is 1min ~3min.

[0018] In one of the embodiments, the raw materials of the steel material include, by mass percentage, 0.35% to 0.45% carbon, 0.1% to 0.3% silicon, 0.7% to 1.2% aluminum, 0.80% to 1.8% chromium, 0.6% to 1.6% manganese, 0.15% to 0.4% alum, 0.01% to 0.03% titanium, 0.1% to 1% graphene and 94% to 97% iron.

[0019] In one embodiment, a cold isostatic pressing step is further included after mixing and before preparing the material to be rolled.

[0020] In one embodiment, the cold isostatic pressing conditions include: pressure of 200 MPa to 220 MPa, and time of 5 min to 15 min.

[0021] Furthermore, the present application also provides a steel material prepared according to the above-mentioned preparation method.

[0022] In one embodiment, the steel material includes an incoherent cementite nanophase and an incoherent vanadium carbide nanophase.

[0023] Furthermore, the present application also provides the use of the above steel material in the preparation of aerospace materials, chemical materials, mechanical materials or electronic materials.

[0024] The present application uses the Joule heating effect and polarization effect generated by pulse current to assist the rolling and heat treatment process to prepare a composite precipitation phase of uniformly dispersed incoherent cementite nanophase and incoherent vanadium carbide nanophase, so as to enhance the strength of the steel material. The composite precipitation phase of the dispersed incoherent cementite nanophase and incoherent vanadium carbide nanophase in its structure is more uniform, and during the service of the steel material, the composite nano-precipitation phase can also serve as a deep hydrogen trap to capture hydrogen more widely, thereby greatly improving the steel material's resistance to hydrogen embrittlement. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the transmission electron microscope image of the steel material in Example 2. DETAILED DESCRIPTION

[0026] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0028] The term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of the related listed items, wherein the any and all combinations include any combination of two related listed items, any more related listed items, or all related listed items. For example, "A and / or B" includes three parallel solutions: A, B, and "a combination of A and B".

[0029] In this article, unless otherwise specified, "one or more" means any one of the listed items or any combination of the listed items. Similarly, "one or more" and other expressions that mean "one or more" are also understood in the same way unless otherwise specified.

[0030] In this document, "further", "further", "particularly", "for example", "such as", "example", "for example", etc. are used for descriptive purposes, indicating that the previous and subsequent technical solutions are related in terms of the content covered, but should not be understood as limiting the previous technical solution, nor can they be understood as limiting the scope of protection of this document. In this document, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0031] Herein, "optionally", "optional", and "optional" mean optional, that is, any one of the two parallel schemes of "yes" or "no". If multiple "optional" items appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" item is independent of each other. In this application, descriptions such as "optionally contain", "optionally include", etc. mean "contain or not contain". "Optional component X" means that component X exists or does not exist, or means that component X is contained or not contained.

[0032] In this document, the terms "first", "second", "third", "fourth", etc. in "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.

[0033] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0034] Herein, when it comes to a numerical interval (i.e., a numerical range), unless otherwise specified, the distribution of the optional numerical values ​​within the numerical interval is considered to be continuous and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical interval, and each numerical value between the two numerical endpoints. Unless otherwise specified, when a numerical interval only refers to integers within the numerical interval, including the two endpoint integers of the numerical range, and each integer between the two endpoints, is equivalent to directly listing each integer. When multiple numerical ranges are provided to describe features or characteristics, these numerical ranges can be combined. In other words, unless otherwise specified, the numerical ranges disclosed herein should be understood to include any and all sub-ranges included therein. The "numerical value" in the numerical interval can be any quantitative value, such as a number, a percentage, a ratio, etc. "Numerical interval" allows broadly including numerical interval types such as percentage intervals, ratio intervals, and ratio intervals.

[0035] Herein, the term "room temperature" or "normal temperature" generally refers to 4°C~35°C, for example, 20°C±5°C. In some embodiments herein, "room temperature" or "normal temperature" refers to 10°C~30°C. In some embodiments herein, "room temperature" or "normal temperature" refers to 20°C~30°C.

[0036] In this article, if there are multiple steps involved in the method flow, unless there is a clear different description in this article, there is no strict order restriction for the execution of these steps, and they can be executed in other orders than described. Moreover, any step can include multiple sub-steps or multiple stages, and these sub-steps or stages are not necessarily executed at the same time, but can be executed at different times, and their execution order is not necessarily sequential, but can be executed in turn, alternating or simultaneously with other steps or parts of sub-steps or stages of other steps.

[0037] The present application provides a method for preparing a steel material, comprising the following steps:

[0038] Providing raw materials of steel materials, mixing them, and preparing materials to be rolled;

[0039] The material to be rolled is subjected to pulse current assisted rolling to prepare a plate;

[0040] The plate is subjected to a pulse current assisted heat treatment process to prepare the steel material; the heat treatment includes quenching and tempering.

[0041] It can be understood that the conditions for providing the raw material mixture of the steel material include: mixing the raw material of the steel material with the solvent, stirring, and drying.

[0042] Furthermore, the mixing time is 1 hour to 2 hours, and the drying temperature is 50° C. to 70° C.

[0043] In a specific example, the conditions for pulse current assisted rolling include: an effective pulse current density of 400 A / mm 2 ~480 A / mm 2 The processing time is 1min~5 min.

[0044] The effective pulse current density in pulse current assisted rolling can be but is not limited to 400 A / mm 2 , 410 A / mm 2 , 420 A / mm 2 , 430 A / mm 2 , 440 A / mm 2 、4500A / mm 2 , 460 A / mm 2 , 470 A / mm 2 or 480 A / mm 2 The processing time may be, but is not limited to, 1 min, 2 min, 3 min, 4 min or 5 min. It can be understood that the actual temperature of the workpiece during the pulse current assisted rolling is 900°C to 1100°C due to the Joule heating effect.

[0045] In a specific example, the conditions for pulse current assisted rolling also include one or more of the following: the pulse power supply is 220V~380V; the frequency is 30Hz~80Hz; the output voltage is 3V~8V; and the rolling reduction is 30%~70% of the height of the material to be rolled.

[0046] It can be understood that the pulse power supply is 220V or 380V, the frequency can be but not limited to 30Hz, 40Hz, 50Hz, 60Hz, 70Hz or 80Hz, the output voltage can be but not limited to 3V, 4V, 5V, 6V, 7V or 8V, and the height of the material to be rolled can be but not limited to 30%, 40%, 50%, 60% or 70%.

[0047] In a specific example, the quenching conditions include an effective pulse current density of 350 A / mm 2 ~410 A / mm 2 , processing time is 5 min ~10min.

[0048] Furthermore, the effective pulse current density in pulse current assisted quenching can be, but is not limited to, 350 A / mm 2 、360 A / mm 2 、365 A / mm 2 、370 A / mm 2 、375 A / mm 2 、380 A / mm 2 、390 A / mm 2 , 400 A / mm 2 or 410A / mm 2 The processing time may be, but is not limited to, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min. It is understandable that the actual temperature of the workpiece during pulse current assisted quenching is 750°C to 950°C due to the Joule heating effect.

[0049] In a specific example, the tempering conditions include an effective pulse current density of 120 A / mm 2 ~230 A / mm 2 , processing time is 1min ~3min.

[0050] The effective pulse current density in pulse current assisted tempering can be but is not limited to 120 A / mm 2 , 125A / mm 2 , 130A / mm 2 、135A / mm 2 , 140 A / mm 2 , 145 A / mm 2, 150 A / mm 2 , 160A / mm 2 , 170 A / mm 2 , 180 A / mm 2 , 190 A / mm 2 , 200 A / mm 2 , 210 A / mm 2 , 22 0A / mm 2 or 230A / mm 2 The processing time may be, but is not limited to, 1 min, 2 min or 3 min. It is understandable that the actual temperature of the workpiece during pulse current assisted tempering is 250°C to 550°C due to the Joule heating effect.

[0051] It can be understood that oil quenching is also performed after quenching.

[0052] In a specific example, the raw materials of the steel material include, by mass percentage, 0.35% to 0.45% carbon, 0.1% to 0.3% silicon, 0.7% to 1.2% aluminum, 0.80% to 1.8% chromium, 0.6% to 1.6% manganese, 0.15% to 0.4% alum, 0.01% to 0.03% titanium, 0.1% to 1% graphene, and 94% to 97% iron.

[0053] It can be understood that the raw material of the steel material also includes ≤0.1% of inevitable impurity elements. Specifically, the inevitable impurity elements include but are not limited to one or more of phosphorus, sulfur, nitrogen and oxygen.

[0054] In a specific example, a cold isostatic pressing step is further included after mixing and before preparing the material to be rolled.

[0055] In a specific example, the conditions for cold isostatic pressing include: pressure of 200 MPa to 220 MPa, and time of 5 min to 15 min.

[0056] Specifically, the pressure in cold isostatic pressing can be but is not limited to 200 MPa, 205 MPa, 210 MPa, 215 MPa or 220 MPa, and the time can be but is not limited to 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min.

[0057] Furthermore, the present application also provides a steel material prepared according to the above-mentioned preparation method.

[0058] The steel material comprises an incoherent cementite nanophase and an incoherent vanadium carbide nanophase.

[0059] The present application uses the Joule heating effect and polarization effect generated by pulse current to assist the rolling and heat treatment process to prepare a composite precipitation phase of uniformly dispersed incoherent cementite nanophase and incoherent vanadium carbide nanophase, so as to enhance the strength of the steel material. The composite precipitation phase of the dispersed incoherent cementite nanophase and incoherent vanadium carbide nanophase in its structure is more uniform, and during the service of the steel material, the composite nano-precipitation phase can also serve as a deep hydrogen trap to capture hydrogen more widely, thereby greatly improving the steel material's resistance to hydrogen embrittlement.

[0060] Furthermore, the present application also provides the use of the above steel material in the preparation of aerospace materials, chemical materials, mechanical materials or electronic materials.

[0061] The present application is further described in detail below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are preferably referred to the guidance given in the present application, and can also be based on the experimental manuals or conventional conditions in the art, can also be based on the conditions recommended by the manufacturer, or refer to experimental methods known in the art.

[0062] In the following specific embodiments, the measured parameters of raw material components may have slight deviations within the range of weighing accuracy unless otherwise specified. For temperature and time parameters, acceptable deviations caused by instrument test accuracy or operation accuracy are allowed. "Normal temperature" refers to 25°C; "normal pressure" refers to 100KPa or 101KPa.

[0063] GNPs are polypropylene / multilayer graphene nanocomposites purchased from Beijing Graphene Technology Research Institute Co., Ltd.

[0064] Example 1

[0065] This embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.1% GNPs, and the rest is Fe and ≤0.01% inevitable impurities, and the sum of the masses of the components is 100%.

[0066] The composite powders were mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatically pressed at a pressure of 220 MPa for 10 minutes.

[0067] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective pulse current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0068] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0069] Example 2

[0070] This embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.3% GNPs, and the rest is Fe and ≤0.01% inevitable impurities, and the sum of the masses of the components is 100%.

[0071] The composite powders were mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatically pressed at a pressure of 220 MPa for 10 minutes.

[0072] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0073] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0074] Example 3

[0075] The present embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.5% GNPs, and the rest is Fe and ≤0.01% inevitable impurities, and the sum of the masses of the components is 100%.

[0076] The composite material powder was mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatic pressing was performed at a pressure of 220 MPa for 10 minutes.

[0077] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2, after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0078] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0079] Example 4

[0080] The present embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.3% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 1% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0081] The composite material powder was mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatic pressing was performed at a pressure of 220 MPa for 10 minutes.

[0082] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0083] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0084] Example 5

[0085] The present embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.3% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.1% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0086] The composite material powder was mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatic pressing was performed at a pressure of 220 MPa for 10 minutes.

[0087] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 480 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0088] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0089] Example 6

[0090] The present embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.3% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 1% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0091] The composite material powder was mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatic pressing was performed at a pressure of 220 MPa for 10 minutes.

[0092] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0093] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 400 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0094] Example 7

[0095] The present embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.3% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 1% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0096] The composite material powder was mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatic pressing was performed at a pressure of 220 MPa for 10 minutes.

[0097] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0098] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was performed, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 220 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0099] Comparative Example 1 (Pulse current assisted rolling forming is not used)

[0100] This comparative example provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.3% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0101] The composite powders were mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatically pressed at a pressure of 220 MPa for 10 minutes.

[0102] The ingot was then heated to 1080°C after machining and rolled after 2 hours with a rolling reduction of 50%. The rolled steel plate was subjected to pulse current assisted quenching and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0103] Comparative Example 2 (no pulse current assisted heat treatment)

[0104] This comparative example provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.3% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0105] The composite powders were mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatically pressed at a pressure of 220 MPa for 10 minutes.

[0106] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0107] The rolled plate was heated to 800°C and kept at that temperature for 30 minutes, then oil quenched and cooled, and then kept at 460°C for 80 minutes and tempered and naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0108] Comparative Example 3 (without pulse current assisted rolling and pulse current assisted heat treatment)

[0109] This comparative example provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V, 0.02% Ti, 0.3% GNPs, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the masses of the components is 100%.

[0110] The composite material powder was mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatic pressing was performed at a pressure of 220 MPa for 10 minutes.

[0111] The ingot was then machined and heated to 1080°C, treated for 2 hours and then rolled with a reduction of 50%.

[0112] Subsequently, the rolled plate was heated to 800°C and kept at that temperature for 30 minutes, and then oil quenched and cooled. Then, the rolled plate was kept at 460°C for 80 minutes and tempered and naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0113] Comparative Example 4 (without graphene addition)

[0114] This embodiment provides a steel material, wherein the raw material composition includes, by weight percentage, 0.36% C, 0.30% Si, 0.8% Al, 0.8% Mn, 1.2% Cr, 0.2% V and 0.02% Ti, and the rest is Fe and ≤0.01% of inevitable impurities, and the sum of the weights of the components is 100%.

[0115] The composite powders were mechanically mixed for 2 hours by mechanical stirring and then vacuum dried, and then cold isostatically pressed at a pressure of 220 MPa for 10 minutes.

[0116] Subsequently, pulse current was introduced to assist rolling, with an output voltage of 5V, a frequency of 50Hz, and an effective current density of 430 A / mm 2 , after processing for 2 minutes, rolling is carried out with a rolling reduction of 50%.

[0117] The rolled steel plate was subjected to pulse current assisted quenching, and the effective current density was adjusted to 360 A / mm 2 After 5 minutes of heat preservation, oil quenching was carried out, and then pulse current was introduced to assist tempering, and the effective current density was adjusted to 135 A / mm 2 After keeping warm for 2 minutes, the steel was naturally cooled to obtain hydrogen embrittlement resistant steel material.

[0118] The mechanical properties of the steel materials obtained in the above embodiments and comparative examples are summarized in the following Table 1.

[0119] Table 1

[0120]

[0121] The hydrogenation solution contained 0.05 mol / L sulfuric acid and 0.22 g / L thiourea. 2 The hydrogen embrittlement sensitivity is the percentage of elongation loss after hydrogen charging.

[0122] like Figure 1 The transmission electron microscope (TEM) image of Example 2 is shown. By comparing the mechanical properties of the steel materials of the Example and the comparative example, it can be seen that the pulse current assisted rolling forming and pulse current assisted heat treatment are necessary for the steel materials. In addition, with graphene as a reinforcement phase, the mechanical properties of the steel materials of the comparative example are not only inferior to those of the steel materials of the Example when they are prepared, but also far inferior to those of the steel materials prepared by the Example after hydrogen charging.

[0123] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0124] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims, and the specification and drawings may be used to interpret the scope of the claims.

Claims

1. A method for preparing a steel material, characterized in that: The following steps are involved: Providing raw materials of steel materials, mixing them, and preparing materials to be rolled; The material to be rolled is subjected to pulse current assisted rolling to prepare a plate; The plate is subjected to a pulse current assisted heat treatment process to prepare a steel material; the heat treatment includes quenching and tempering.

2. The preparation method according to claim 1, characterized in that The conditions for the pulse current assisted rolling include: an effective pulse current density of 400 A / mm 2 ~480 A / mm 2 The processing time is 1min~5 min.

3. The preparation method according to claim 1 or 2, characterized in that: The conditions for the pulse current assisted rolling also include one or more of the following: (1) Pulse power supply is 220V~380V; (2) Frequency: 30 Hz to 80 Hz; (3) Output voltage is 3V~8V; (4) The rolling reduction is 30% to 70% of the height of the material to be rolled.

4. The preparation method according to claim 1, characterized in that: The heat treatment satisfies one or both of the following conditions: (1) The quenching conditions include: effective pulse current density of 350 A / mm 2 ~410 A / mm 2 , processing time 5 min~10 min; (2) The tempering conditions include: effective pulse current density of 120 A / mm 2 ~230 A / mm 2 , processing time is 1min ~3min.

5. The preparation method according to claim 1, characterized in that: The raw materials of the steel material include, by mass percentage, 0.35% to 0.45% carbon, 0.1% to 0.3% silicon, 0.7% to 1.2% aluminum, 0.80% to 1.8% chromium, 0.6% to 1.6% manganese, 0.15% to 0.4% alum, 0.01% to 0.03% titanium, 0.1% to 1% graphene and 94% to 97% iron.

6. The preparation method according to any one of claims 1 to 2 and 4 to 5, characterized in that: After mixing and before preparing the material to be rolled, a cold isostatic pressing step is also included.

7. The preparation method according to claim 6, characterized in that: The cold isostatic pressing conditions include: pressure of 200 MPa to 220 MPa, and time of 5 min to 15 min.

8. A steel material, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 7.

9. The steel material according to claim 8, characterized in that The steel material includes an incoherent cementite nanophase and an incoherent vanadium carbide nanophase.

10. Use of the steel material according to claim 8 or 9 in the preparation of aerospace materials, chemical materials, mechanical materials or electronic materials.