Wide-temperature-range superplastic iron-based memory alloy and preparation thereof

Through alloy composition design and heat treatment process, high-density nano-precipitation phases are generated, which solves the problem of improving the performance of iron-based shape memory alloys in a wide temperature range, and achieves stable performance and strengthening effects in the range of -200℃ to 500℃. Meets application needs in extreme environments in wide temperature domains.

CN118880083APending Publication Date: 2024-11-01UNIV OF SHANGHAI FOR SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410972950.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The application performance of existing iron-based shape memory alloys in a wide temperature domain is limited and cannot meet the requirements of extreme service environments. Especially at high or very low temperatures, phase change instability and grain coarse problems are prone to occur, which limits its wide range. Use of the temperature domain.

Method used

Through alloy composition design and elemental alloying effect, high-density nano-precipitation phase is generated, and heat treatment processes such as solid solution treatment, rolling deformation, recrystallization annealing and aging treatment are optimized to form co-categorized nano-precipitation phases in FCC matrix to improve the alloy Phase stability and tissue stability broaden its temperature application range.

Benefits of technology

It realizes excellent shape memory effect and superelasticity of iron-based memory alloys in the range of -200℃ to 500℃, enhances the strength and toughness of the material in a wide temperature domain, ensures stable performance in extreme environments, and broadens its application range. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118880083A_ABST
    Figure CN118880083A_ABST
Patent Text Reader

Abstract

The invention relates to the field of material science, in particular to a wide-temperature-range superplastic iron-based memory alloy and a preparation method thereof.The preparation method comprises the following steps that S1, alloy optimization design is conducted through Thermo-calc software, and five kinds of metal including Fe, Co, Ni, Al and Ti are selected; and S2, raw material distribution is conducted according to the components and the atomic percent, metal raw materials are weighed, cleaned and then put into high-vacuum melting equipment to be vacuumized and filled with shielding gas, heating is conducted till the raw materials are molten, and regular-shape casting is conducted after metal liquid is electromagnetically stirred. And then high-temperature solution treatment and rolling deformation treatment are conducted on the sample with the regular size, and a rolled piece is obtained. And finally, the rolled piece is subjected to recrystallization annealing treatment and aging treatment, and the wide-temperature-range superplastic iron-based memory alloy is obtained after cooling. Compared with the prior art, the iron-based memory alloy material prepared by the method has an excellent strengthening effect in a wide temperature range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material science, and in particular to a wide temperature range superplastic iron-based memory alloy and a preparation method thereof. Background Art

[0002] Iron-based shape memory alloys (Fe-SMAs) are widely used in aerospace, medical devices, engineering structures and other fields due to their shape memory effect, superelasticity, low cost and good processing performance. They perform particularly well under wide temperature range service conditions such as spacecraft and biomedicine, and can be used in vibration control, drive and sensing. However, there are few reports on the application of shape memory alloys in wide temperature range structural materials. The performance improvement of existing shape memory alloys is mainly concentrated in the room temperature range, which cannot meet the requirements of wide temperature range extreme service environments. Therefore, the development of new wide temperature range structural materials is imminent.

[0003] In recent years, superplastic materials have attracted widespread attention due to their property of not producing cracks under large deformation. Materials with superplasticity can show significant ductility and deformation ability under specific conditions. The superplasticity of iron-based memory alloys mainly depends on their microstructure and phase transformation mechanism. Under specific heat treatment processes and alloy composition designs, the superplasticity and mechanical properties of the alloy can be improved by methods such as grain refinement and introduction of nano-precipitation phases. Iron-based memory alloys with superplasticity can withstand large deformations without fracture in a wide temperature range, which is of great significance for improving the reliability and service life of materials in practical applications.

[0004] The performance improvement of existing iron-based memory alloys is mainly concentrated in the room temperature range, but how to broaden the application temperature range of the alloy and realize the engineering application of the alloy in a wide temperature range still faces many challenges and cannot meet the requirements of extreme service environments in a wide temperature range. Traditional alloys are prone to phase change instability, grain coarsening and creep in high or very low temperature ranges, which limits their use under extreme conditions. In addition, superplastic iron-based memory alloys can withstand extreme deformation without breaking in a wide temperature range, which is of great significance for improving the reliability and service life of materials in practical applications. Summary of the invention

[0005] The purpose of the present invention is to provide a wide temperature range superplastic iron-based memory alloy and its preparation in order to overcome the shortcomings of the above-mentioned prior art. Through alloy composition design and element alloying effect, a high-density nano-precipitated phase is generated in the memory alloy, thereby effectively strengthening the alloy, reducing the coarsening rate of grains and strengthening phases, improving phase stability and organizational stability, and broadening the temperature application range of the alloy.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A method for preparing a wide temperature range superplastic iron-based memory alloy comprises the following steps:

[0008] S1: Thermo-calc software is used to design the alloy system and five metals, Fe, Co, Ni, Al and Ti, are selected;

[0009] S2: The raw materials are weighed according to the components and atomic percentages, and then placed in a high vacuum melting furnace for evacuation, filling with protective gas, and heating until the raw materials are melted to obtain molten metal, which is stirred and then sequentially cast into a regular shape, subjected to high-temperature solution treatment, and subjected to rolling deformation treatment to obtain a rolled piece, which is subjected to recrystallization annealing treatment, aging treatment, and cooling to obtain the wide temperature range superplastic iron-based memory alloy.

[0010] Further, in step S1, the components in atomic percentage are:

[0011] Fe=25~48%; Co=10~25%; Ni=30~35%; Al=10~12%; Ti=2~3%.

[0012] Furthermore, in step S2, the system pressure is not greater than 10 -3 Pa.

[0013] Furthermore, in step S2, the heating temperature is 2500-3000°C.

[0014] Furthermore, in step S2, the cooling method is furnace cooling.

[0015] Furthermore, in step S2, the temperature of the high temperature solution treatment is 1000-1250°C, and the time is 0.5-2h.

[0016] Furthermore, in step S2, the deformation amount of the rolling deformation treatment is 5-90%.

[0017] Furthermore, in step S2, the temperature of the recrystallization annealing treatment is 1000-1200°C and the time is 3-5 minutes.

[0018] Furthermore, in step S2, the aging treatment is performed at a temperature of 600-900°C and for a time of 1 min-24 h.

[0019] A method for preparing a wide temperature range superplastic iron-based memory alloy is prepared by adopting the above-mentioned preparation method.

[0020] The present invention takes FeCoNiAlTi alloy as a model, firstly obtains the optimal alloy composition ratio through alloy design, and then obtains a wide temperature range superplastic iron-based memory alloy through the steps of solution treatment, cold rolling, recrystallization, aging treatment, etc. by optimizing the preparation process. The developed new alloy has excellent shape memory effect and superelasticity in the range of -200°C to 500°C, and the structure remains stable to meet the needs of extreme service environments, and has broad application prospects.

[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0022] (1) The present invention forms a coherent nano-precipitation phase in the FCC matrix of the alloy obtained by recrystallization and aging treatment, and obtains a γ / γ' coherent structure, in which the γ phase is the matrix phase and the γ' phase is the nano-precipitation phase. The coherent interface has a lower lattice mismatch and interface energy, which helps the material to deform uniformly under the action of external force and promotes the alloy to produce large plastic strain.

[0023] (2) The present invention improves the heat resistance stability of iron-based shape memory alloys (Fe-SMAs). By optimizing the alloying element ratio and coordinating the optimization of the heat treatment system, the grain size and micro-element segregation of the alloy are regulated, thereby enhancing the strength of the alloy at high temperatures. At the same time, the entire alloy system has a low stacking fault, which can induce nano-strengthening at low temperatures, improve the low-temperature toughness and high-temperature strength of the material, and further enhance the material's strength-plasticity combination over a wide temperature range, making it suitable for extreme environments over a wide temperature range.

[0024] (3) The alloy prepared by the present invention is heat treated at 800° C. for 24 h, and the austenite phase structure remains unchanged, the microstructure is uniform, and there is no phase transformation and new phase generation.

[0025] (4) The alloy obtained by the present invention has different intrinsic strengthening characteristics in a wide temperature range: at low temperatures (such as minus 200°C), the lower stacking faults can enable the alloy to form a high-density twin structure during low-temperature deformation, thereby improving the material strength and maintaining the plasticity. At room temperature, due to the heat treatment process, a high-density nano-precipitation phase is formed in the alloy matrix alloy, and multiple deformation mechanisms promote alloy strengthening, including solid solution strengthening and precipitation strengthening, and enhance strain hardening ability. At high temperatures, the crystals form nano-precipitation phases, showing excellent strengthening structural stability and microstructural heat resistance stability, and can effectively inhibit high-temperature softening in a certain medium and high temperature range. The above characteristics help to achieve excellent strengthening effects of the alloy in a wide temperature range, and have important engineering value and scientific significance. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Room temperature XRD phase spectrum of the memory alloy prepared in Example 1-2;

[0027] Figure 2 The microstructure and element distribution of the alloy prepared in Example 2;

[0028] Figure 3 Schematic diagram of the stress-strain-temperature relationship of the alloy (X) prepared in Example 2 from low temperature to room temperature to high temperature and a schematic diagram of the stress-strain-temperature relationship of the material of Comparative Example 1 (Y) without aging treatment. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0031] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained.

[0032] Example 1-2

[0033] This embodiment provides a wide temperature range superplastic iron-based memory alloy and a preparation method thereof.

[0034] First, alloy design was carried out. Thermo-calc software was used to design the alloy system. The Fe-base memory alloy analysis module was selected and the Fe-Co-Ni system thermodynamic database was established to assist in the design of the quantitative relationship between the alloy phase composition, element content and heat treatment temperature. Finally, five metals, Fe, Co, Ni, Al and Ti, were selected:

[0035] S1: Establishment of thermodynamic database for Fe-Co-Ni system;

[0036] S2: The Fe-Co-Ni system thermodynamic database and Fe-base memory alloy analysis module established in step S1 are used to calculate and simulate the phase equilibrium relationship of the Fe-Co-Ni alloy at a temperature of 600-900°C using the Thermo-Calc software to determine the addition amounts of Co and Ni in the alloy;

[0037] S3: Using the Fe-Co-Ni system thermodynamic database established in step S1, according to the addition amounts of Co and Ni in the alloy determined in step S2, calculate the phase stability and heat treatment temperature change of the alloy under different addition amounts of Al and Ti elements, and calculate the optimal alloy composition ratio based on computer simulation. In this embodiment, the components are respectively in atomic percentage as follows: Fe=40%; Co=15%; Ni=30%; Al=12%; Ti=3%, and the rest are unavoidable impurities.

[0038] The preparation process is as follows:

[0039] (1) The raw materials are all high-purity metals with a purity of more than 99%. According to the optimal composition ratio obtained in the design, they are weighed, cleaned, and placed in a high vacuum arc melting furnace in turn. The furnace is evacuated to 4×10 -3 Pa, and then filled with protective gas, high-purity Ar gas, this process is repeated many times to reduce the oxygen content in the smelting environment.

[0040] (2) The raw materials are melted multiple times, and the electrodes provide a high temperature of up to 3000°C to fully melt the metal raw materials. With the help of electromagnetic stirring, the metal liquid is fully stirred to achieve uniformity of solid metal structure. After the alloy melting is completed, it is cast by gravity or negative pressure to obtain a regular ingot of 5×10×50 mm. In this embodiment, the cooling method of this step is furnace cooling.

[0041] (3) Perform high-temperature solution treatment, solution temperature: 1250°C, solution time: 1h, and then cool by water.

[0042] (4) The material in step (3) is subjected to rolling deformation treatment, with the deformation amount being 70%.

[0043] (5) The rolled piece in step (4) is subjected to recrystallization annealing in air atmosphere at 1100° C. for 5 minutes, followed by cooling, wherein the cooling method is rapid cooling, such as water cooling or oil cooling. The recrystallization annealing temperature and time are adjusted according to the designed alloy composition and performance.

[0044] (6) The sample in step (5) is subjected to aging treatment at 600° C. The aging treatment time is 3 h (Example 1) and 24 h (Example 2), respectively, to obtain nano-precipitation phase strengthened alloys with different structures, and then cooled. The cooling method is rapid cooling, such as water cooling or oil cooling.

[0045] The components obtained in the above process are characterized. Figure 1 It is the XRD spectrum of the sample. The alloys obtained by short-aging heat treatment and long-aging heat treatment maintain the austenite phase structure. It can be seen from the figure that the parts obtained by short-aging and long-aging treatment are characterized by XRD, and both have peaks corresponding to 75° of the austenite phase. The obtained alloys all have austenite structure.

[0046] The microstructure of the material of Example 2 and the distribution of its main elements are as follows Figure 2 As shown, it can be seen that there are obvious grain boundaries and internal grain structures in the material, the grain size distribution is uniform, and each element is segregated in the matrix and precipitated phase.

[0047] Comparative Example

[0048] This comparative example provides an iron-based memory alloy and a preparation method thereof, which is different from Example 2 in that step (6) is omitted, that is, no aging treatment is performed and only recrystallization annealing treatment is performed.

[0049] The stress-strain-temperature relationship between the material obtained in Example 2 and the material obtained in Comparative Example 1 is as follows: Figure 3 As shown, through the temperature treatment process from low temperature to room temperature (25°C) and then to high temperature, the material prepared by the present invention maintains strength in a wide temperature range, does not become brittle at low temperature and soften at high temperature, and has a good combination of toughness and plasticity.

[0050] The technical solution and embodiments of the present invention explain in detail how to achieve the high-performance iron-based memory alloy required in extreme environments by rationally designing alloy composition and heat treatment process. The development of this alloy broadens the application scope of iron-based memory alloys and also provides a specific solution for the application of high-performance iron-based alloys.

[0051] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a wide temperature range superplastic iron-based memory alloy, characterized in that: The following steps are involved: S1: Select five metals: Fe, Co, Ni, Al, and Ti; S2: The raw materials are weighed according to the components and atomic percentages, and then placed in a high vacuum melting furnace, evacuated, filled with protective gas, and heated until the raw materials are melted to obtain molten metal, which is stirred and then cast into a regular shape, subjected to high-temperature solution treatment, and rolled and deformed to obtain a rolled piece. The rolled piece is subjected to recrystallization annealing treatment, aging treatment, and cooling to obtain the wide temperature range superplastic iron-based memory alloy.

2. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S1, the alloy system is designed using Thermo-calc software, and five metals, Fe, Co, Ni, Al, and Ti, are selected. The atomic percentages of the components are as follows: Fe=25~48%; Co=10~25%; Ni=30~35%; Al=10~12%; Ti=2~3%.

3. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the system pressure is kept at no more than 10 -3 Pa.

4. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the heating temperature is 2500-3000°C.

5. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the cooling method is furnace cooling.

6. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the temperature of the high temperature solution treatment is 1000-1250°C and the time is 0.5-2h.

7. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the deformation amount of the rolling deformation treatment is 5-90%.

8. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the temperature of the recrystallization annealing treatment is 1000-1200°C and the time is 3-5 minutes.

9. The method for preparing a wide temperature range superplastic iron-based memory alloy according to claim 1, characterized in that: In step S2, the aging treatment is carried out at a temperature of 600-900°C and for a time of 1 min-24 h.

10. A method for preparing a wide temperature range superplastic iron-based memory alloy, characterized in that: The preparation is obtained by the preparation method according to any one of claims 1 to 9.