Novel high-performance double-phase titanium alloy heat treatment method

Through the new heat treatment method for duplex titanium alloy, the solution treatment and aging conditions of titanium alloy are coordinated, and the problem of insufficient plasticity in room temperature is solved, the tensile strength and yield strength are significantly improved, and the high performance in aerospace and other fields is met. Require.

CN118932264AInactive Publication Date: 2024-11-12BEIJING INST OF TECH

Patent Information

Application Number
CN202410877103.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Dual-phase titanium alloys have poor plasticity at room temperature and are prone to cracking during processing. The elongation of traditional high-strength titanium alloys is insufficient, making it difficult to meet the strict requirements in aerospace and other fields.

Method used

The heat treatment method of the new titanium alloy Ti-Al-Mo-Cr-Fe is adopted to control the morphology and volume fraction of secondary α in β and the content of alloy elements in primary α by coordinating the aging temperature and aging time after solid solution treatment. Improve the microstructure of titanium alloys, improve tensile strength and yield strength.

Benefits of technology

It significantly improves the tensile strength and yield strength of the biphasic titanium alloy, while maintaining high plasticity, with mechanical properties reaching 1312MPa, 1345MPa and 1517MPa, and the elongation after break reaches 15.07%, 8.57% and 10.9%, which is significantly better than traditional doubles. Phase titanium alloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932264A_ABST
    Figure CN118932264A_ABST
Patent Text Reader

Abstract

The invention relates to a novel high-performance double-phase titanium alloy heat treatment method, and belongs to the field of titanium alloy heat treatment. The novel titanium alloy comprises the following components in percentage by mass: 5%-8% of Al, 4%-8% of Mo, 1%-3% of Cr, 0.5%-2% of Fe and the balance of commercial pure Ti and inevitable impurities. The method comprises the following steps: rolling a smelted cast ingot at 40-60 DEG C below a phase transformation point, carrying out solution treatment in a two-phase region, cooling to room temperature at a certain rate, aging at 450-650 DEG C for a certain time, and carrying out air cooling. Through component design and coordination of the aging temperature and the aging time of the novel titanium alloy after solution treatment, the morphology and the volume fraction of secondary alpha in beta and the number of alpha / beta interfaces are controlled. The process is simple, the production efficiency is high, the plasticity of the high-strength titanium alloy is improved, the high-performance double-phase titanium alloy is prepared, and application of the double-phase titanium alloy in multiple fields is promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of heat treatment of titanium alloys, and in particular relates to a novel high-performance dual-phase titanium alloy heat treatment method. Background Art

[0002] In recent years, titanium and titanium alloys have the advantages of high specific strength, corrosion resistance, strong heat resistance, and good biocompatibility. They are increasingly widely used in aerospace, weapons and equipment, chemical industry, medical and other fields. With the continuous expansion of the application field of titanium alloys, the demand and requirements for high-performance titanium alloys are constantly increasing. Especially in the fields of aerospace, titanium alloys are used as structural parts of rockets, missiles and high-speed aircraft. The harsh working environment requires materials to have high strength, high toughness, impact resistance and other properties. Among different types of titanium alloys, duplex titanium alloys are the most widely used and the largest in usage. They have the characteristics of both α-type titanium alloys and β-type titanium alloys and have good comprehensive mechanical properties. However, α+β-type duplex titanium alloys have the problem of insufficient strength and plasticity matching, resulting in poor room temperature plasticity, easy cracking during processing, and limited application environment. For traditional high-strength titanium alloys, their elongation is usually less than 10%. Improving the plasticity of high-strength duplex titanium alloys and improving the matching of strength and plasticity are still challenges in the preparation of high-performance duplex titanium alloys.

[0003] For dual-phase titanium alloys, elements such as Mo, Cr, V, Mn, Fe, and Al can be added by alloying, the element content ratio can be adjusted, and the solid solution strengthening of alloying elements and their influence on the phase transformation of titanium alloys can be utilized to improve the comprehensive performance of titanium alloys. In order to achieve further improvement in performance, it is also necessary to study small-scale microstructures: secondary phases and α / β interfaces, which have an important influence on the improvement of the performance of dual-phase titanium alloys through the Hall-Petch effect. Therefore, the present invention develops a novel heat treatment method for dual-phase titanium alloys, controls the morphology and volume fraction of secondary α in β and the content of alloying elements in primary α, improves the plasticity of high-strength titanium alloys, prepares high-performance dual-phase titanium alloys, and promotes the application of dual-phase titanium alloys in multiple fields. Summary of the invention

[0004] The purpose of the present invention is to provide a new type of heat treatment method for a dual-phase titanium alloy Ti-Al-Mo-Cr-Fe in order to solve the problem of insufficient plasticity of existing high-strength dual-phase titanium alloys; the method coordinates the aging temperature and aging time after the solution treatment of the new type of titanium alloy, thereby controlling the morphology and volume fraction of the secondary α in β and the content of alloying elements in the primary α, thereby improving the microstructure of the titanium alloy and significantly improving its tensile strength and yield strength while maintaining a low plasticity loss of the titanium alloy.

[0005] The technical solution adopted by the present invention specifically includes the following steps:

[0006] 1) Melting: obtaining a titanium alloy ingot by melting in a vacuum consumable arc furnace, removing the riser and performing rough processing to obtain a cylindrical ingot.

[0007] 2) Rolling: rolling the ingot obtained in step 1), and rolling after keeping it at 40°C to 60°C below the phase transformation point for t1 time.

[0008] 3) Solution treatment: the rolled sample is kept at a temperature of 40°C to 60°C below the phase transformation point for t2 time, and then cooled to room temperature at a certain rate.

[0009] 4) Aging treatment: the sample after solution treatment is kept at temperature T1 for t3 time and then air-cooled to room temperature.

[0010] Preferably, the novel titanium alloy of the present invention has the following components in mass percentage: Al: 5%-8%, Mo: 4%-8%, Cr: 1%-3%, Fe: 0.5%-2%, and the balance is commercial pure Ti and unavoidable impurities.

[0011] Preferably, in the present invention, in step 2), the holding time t1=0.5h-1h, the pressing amount of a single rolling pass is 1mm, the total deformation is 80%, and air cooling is performed after rolling.

[0012] Preferably, in the present invention, in order to obtain a duplex titanium alloy having a tensile strength greater than 1350 MPa and a plasticity of not less than 10%: step 3) the holding time of the solution treatment is t2 = 1h to 2h, and air cooling to room temperature, and in step 4) the aging temperature T1 is 450°C to 550°C, and the holding time t3 is 2h to 3h.

[0013] Preferably, in the present invention, in order to obtain a duplex titanium alloy having a yield strength greater than 1300 MPa and a plasticity of not less than 10%: step 3) the holding time of the solution treatment is t2 = 1h to 2h, and air cooling to room temperature, and in step 4) the aging temperature T1 = 550°C to 650°C, and the holding time t3 = 4h to 5h.

[0014] Preferably, in the present invention, in order to obtain a duplex titanium alloy having a tensile strength greater than 1400 MPa and a plasticity of not less than 10%: step 3) the holding time of the solution treatment is t2 = 1h to 2h, and air cooling to room temperature, and in step 4) the aging temperature T1 is 450°C to 550°C, and the holding time t3 is 4h to 5h.

[0015] Preferably, in the present invention, in order to obtain a duplex titanium alloy having a tensile strength greater than 1500 MPa and a plasticity of not less than 8%: step 3) the holding time of the solution treatment is t2 = 1h to 2h, and water cooled to room temperature, and in step 4) the aging temperature is T1 = 450°C to 550°C, and the holding time is t3 = 4h to 5h.

[0016] Preferably, in the present invention, in order to obtain a duplex titanium alloy having a yield strength greater than 1300 MPa and a plasticity not less than 15%: step 3) the holding time of the solution treatment is t2 = 1h to 2h, and water cooled to room temperature, and in step 4) the aging temperature is T1 = 550°C to 650°C, and the holding time is t3 = 4h to 5h.

[0017] Beneficial effects:

[0018] (1) In the present invention, the heat treatment process for the new dual-phase titanium alloy is simple, low-cost and high-efficiency, and can be used as an effective means to improve the strength and plasticity of the dual-phase titanium alloy.

[0019] (2) By selecting the aging temperature, time and cooling method after solution treatment, the microstructure of the alloy can be effectively controlled, including the morphology, volume fraction and number of α / β interfaces of the secondary α, thereby significantly improving the tensile strength and yield strength of the titanium alloy while maintaining a mild plastic loss.

[0020] (3) Through the heat treatment process of the present invention, a high-strength and high-plasticity titanium alloy with a yield strength of 1312MPa, a tensile strength of 1345MPa, and an elongation after fracture of 15.07% is obtained; an ultra-high-strength titanium alloy with a yield strength of 1390MPa, a tensile strength of 1517MPa, and an elongation after fracture of 8.57% is obtained; and a high-strength dual-phase titanium alloy with a yield strength of 1321MPa, a tensile strength of 1444MPa, and an elongation after fracture of 10.9% is obtained. Compared with traditional dual-phase titanium alloys, the mechanical properties have obvious advantages. Other advantages, objectives and features of the present invention will be explained to some extent in the subsequent description, and to some extent, will be obvious to those skilled in the art based on the following investigation and research, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be achieved and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is the SEM microstructure diagram of Example 1;

[0022] Figure 2 This is the SEM microstructure diagram of Example 2;

[0023] Figure 3 This is the SEM microstructure diagram of Example 3;

[0024] Figure 4 This is the SEM microstructure diagram of Example 4;

[0025] Figure 5 This is the SEM microstructure diagram of Example 5;

[0026] Figure 6This is the SEM microstructure diagram of Comparative Example 1;

[0027] Figure 7 This is the SEM microstructure diagram of Comparative Example 2;

[0028] Figure 8 This is the SEM microstructure diagram of Comparative Example 3;

[0029] Fig. 9 The static tensile data of each embodiment and comparative example are shown in FIG. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1:

[0032] The main components and mass ratios of the novel dual-phase titanium alloy designed by the present invention are: 6% Al, 6% Mo, 1% Cr, 1% Fe, and the balance is Ti and other inevitable impurity elements. The ingot is prepared by a vacuum induction melting furnace, comprising the following steps:

[0033] 1) Melting: Use sponge titanium with a purity of 99.92%, titanium-iron alloy with a mass fraction of 66.84% Ti and 32.89% Fe, pure Al particles with a purity of 99.84%, titanium-32 molybdenum with a mass fraction of 68.56% Ti and 31.12% Mo, and pure Cr particles with a purity of 99.28% as raw materials, mix the ingredients according to the mass percentage, and melt them in a vacuum arc melting furnace. After the melting furnace is evacuated, high-purity argon gas with a purity of 99.9% is introduced as a protective atmosphere. The alloy ingot is reversed and melted 10 times, each time for 3 minutes, and electromagnetic stirring is turned on for stirring. After the melting is completed, it is cooled to room temperature and sampled to obtain an alloy ingot. The melting current is 400-600A, and the melting vacuum is 10 -4 Pa.

[0034] 2) Rolling: the ingot obtained in step 1) is kept at 880° C. for 30 minutes and then rolled, with a single-pass pressing amount of 1 mm and a total deformation amount of 80%, and air-cooled after rolling.

[0035] 3) Solution treatment: the sample rolled in step 2) is kept at 880°C for 1 h and then air-cooled to room temperature.

[0036] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 500°C for 2h and then air-cooled to room temperature.

[0037] The solution-aged sample obtained in Example 1 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that its yield strength was 1234 MPa, tensile strength was 1356 MPa, and elongation after fracture was 11.3%. Fig. 9 The microstructure after heat treatment is shown in Figure 1 As shown, the results show that the obtained structure is a dual-state structure, β contains a large amount of lamellar secondary α with small size, small lamellar spacing, and a large volume fraction of secondary α.

[0038] Embodiment 2:

[0039] The steps 1) smelting, 2) rolling and 2) solution treatment in Example 2 are the same as those in Example 1.

[0040] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 600°C for 4 hours and then air-cooled to room temperature.

[0041] The solution-aged sample obtained in Example 2 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that its yield strength was 1313 MPa, tensile strength was 1348 MPa, and elongation after fracture was 11.6%. Fig. 9 The microstructure after heat treatment is shown in Figure 2 As shown, the results show that the obtained structure is a dual-state structure, β contains abundant lamellar secondary α, which is slightly coarse in size, and the lamellar spacing is relatively large. The volume fraction of secondary α is smaller than that of Example 1.

[0042] Embodiment 3:

[0043] The steps 1) smelting, 2) rolling and 2) solution treatment in Example 3 are the same as those in Example 1.

[0044] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 500°C for 4 hours and then air-cooled to room temperature.

[0045] The solution-aged sample obtained in Example 3 was subjected to quasi-static room temperature mechanical property testing and SEM microstructure characterization. The experiment showed that its yield strength was 1321 MPa, with an excellent tensile strength of 1444 MPa, and an acceptable elongation after break of 10.9%, which showed a certain strength-plasticity match. Fig. 9 The microstructure after heat treatment is shown in Figure 3 As shown, the results show that the obtained structure is a dual-state structure, and β contains a large number of disordered and fine nano-scale lamellar secondary α, the size and lamellar spacing are smaller than those in Example 1, and accordingly, the volume fraction of secondary α is larger than that in Example 1.

[0046] Embodiment 4:

[0047] The step 1) smelting and the step 2) rolling in Example 4 are the same as those in the previous embodiment.

[0048] 3) Solution treatment: the sample rolled in step 2) is kept at 880°C for 1 hour and then cooled to room temperature with water.

[0049] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 500°C for 4 hours and then air-cooled to room temperature.

[0050] The solution-aged sample obtained in Example 4 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that it had a high yield strength of 1390 MPa, an ultra-high tensile strength of 1517 MPa, and an elongation of 8.57%. Fig. 9 The microstructure after heat treatment is shown in Figure 4 As shown, the results show that the obtained structure is a dual-state structure, β contains fine lamellar secondary α, and is mixed with a large number of disordered and fine nanoscale secondary α. The size and lamellar spacing are smaller than those in Example 1. Correspondingly, the volume fraction of secondary α is larger than that in Example 1.

[0051] Embodiment 5:

[0052] The step 1) smelting and the step 2) rolling in Example 5 are the same as those in Example 1.

[0053] 3) Solution treatment: the sample rolled in step 2) is kept at 880°C for 1 h and then water-cooled to room temperature.

[0054] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 600°C for 4 hours and then air-cooled to room temperature.

[0055] The solution-aged sample obtained in Example 5 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that its yield strength was 1312MPa, tensile strength was 1345MPa, and it had a high elongation after fracture of 15.07%. Fig. 9 The microstructure after heat treatment is shown in Figure 4 As shown, the results show that the obtained tissue is a dual-state tissue, β contains abundant lamellar secondary α, which is slightly coarse in size, and the lamellar spacing is relatively large. The volume fraction of secondary α is larger than that of Example 1.

[0056] Comparative Example 1:

[0057] The steps 1) smelting, 2) rolling and 2) solution treatment in Comparative Example 1 are the same as those in Example 1.

[0058] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 400°C for 2h and then air-cooled to room temperature.

[0059] The solution-aged sample obtained in Comparative Example 1 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that its yield strength was 1121 MPa, tensile strength was 1236 MPa, and elongation after fracture was 10.2%. Fig. 9 The microstructure after heat treatment is shown in Figure 6 As shown, the results show that the obtained structure is a completely equiaxed structure, no secondary α is found in β, and the lack of secondary α and Hall-Petch strengthening at the α / β interface are the main reasons for its low strength.

[0060] Comparative Example 2:

[0061] The steps 1) smelting, 2) rolling and 2) solution treatment in Comparative Example 2 are the same as those in Example 1.

[0062] 4) Aging treatment: the sample after solution treatment in step 3) is kept at 700°C for 2h and then air-cooled to room temperature.

[0063] The solution-aged sample obtained in Comparative Example 2 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that its yield strength was 1015MPa, tensile strength was 1068MPa, and elongation after fracture was 17.3%. Fig. 9 The microstructure after heat treatment is shown in Figure 7 As shown, the results show that the obtained tissue is a completely equiaxed tissue, and no secondary α is found in β.

[0064] Comparative Example 3:

[0065] The steps 1) smelting and 2) rolling in Comparative Example 3 are the same as those in Example 1.

[0066] 3) Double annealing: the sample rolled in step 2) is kept at 880°C for 1 hour and then cooled to 750°C in the furnace. It is kept at this temperature for another 2 hours and then cooled to room temperature in the furnace.

[0067] The double annealed sample obtained in comparative example 3 was subjected to quasi-static room temperature mechanical property test and SEM microstructure characterization. The experiment showed that its yield strength was 1061MPa, tensile strength was 1117MPa, and it had a relatively good elongation after break of 18.18%. Figure 7 As shown, the results show that the obtained structure is a completely equiaxed structure, and the size of the primary α is larger than that of other embodiments and comparative examples, which is one of the reasons why it has good plasticity.

Claims

1. A novel high performance dual phase titanium alloy heat treatment method, characterized in that: The first step is to melt the new dual-phase titanium alloy Ti-Al-Mo-Cr-Fe in a vacuum consumable arc furnace. The second step is to roll the smelted ingot after keeping it at 40℃~60℃ below the phase transformation point for t1 time. The third step is to carry out solid solution treatment on the rolled sample at 40℃~60℃ below the phase transformation point for t2 time, and cool it to room temperature at a certain rate. The fourth step is to carry out aging heat treatment on the sample after solid solution, keep it at T1 temperature for t3 time, and then air cool it to room temperature.

2. A novel high performance dual phase titanium alloy heat treatment method according to claim 1, characterized in that: The novel dual-phase titanium alloy of the present invention has the following components in mass percentage: Al: 5%-8%, Mo: 4%-8%, Cr: 1%-3%, Fe: 0.5%-2%, and the remainder is commercial pure Ti and inevitable impurities.

3. A novel high performance dual phase titanium alloy heat treatment method according to claim 1, characterized in that: The second step is heat preservation time t1 = 0.5h-1h, the single pass pressing amount of rolling is 1mm, the total deformation amount is 80%, and air cooling is performed after rolling.

4. A novel high performance dual phase titanium alloy heat treatment method according to claim 1, characterized in that: In the third step, the solution temperature is 40℃~60℃ below the phase transition point, the holding time t2=1h~2h, and the steel is cooled to room temperature at a certain rate. In the fourth step, the aging temperature T1 is 450℃~650℃, and the holding time t3=2h~5h.

5. A novel high performance dual phase titanium alloy heat treatment method according to claim 4, characterized in that: In the third step, the solution temperature is 40℃~60℃ below the phase transition point, the holding time t2=1h~2h, and air cooling to room temperature. In the fourth step, the aging temperature T1 is 450℃~550℃, and the holding time t3=2h~3h.

6. A novel high performance dual phase titanium alloy heat treatment method according to claim 4, characterized in that: In the third step, the solution temperature is 40℃~60℃ below the phase transition point, the holding time t2=1h~2h, and air cooling to room temperature. In the fourth step, the aging temperature T1 is 550℃~650℃, and the holding time t3=4h~5h.

7. A novel high performance dual phase titanium alloy heat treatment method according to claim 4, characterized in that: In the third step, the solution temperature is 40℃~60℃ below the phase transition point, the holding time t2=1h~2h, and air cooling to room temperature. In the fourth step, the aging temperature T1 is 450℃~550℃, and the holding time t3=4h~5h.

8. A novel high performance dual phase titanium alloy heat treatment method according to claim 4, characterized in that: In the third step, the solution temperature is 40℃~60℃ below the phase transition point, the holding time t2=1h~2h, and then water-cooled to room temperature. In the fourth step, the aging temperature T1 is 450℃~550℃, and the holding time t3=4h~5h.

9. A novel high performance dual phase titanium alloy heat treatment method according to claim 4, characterized in that: In the third step, the solution temperature is 40℃~60℃ below the phase transition point, the holding time t2=1h~2h, and water cooling to room temperature. In the fourth step, the aging temperature T1 is 550℃~650℃, and the holding time t3=4h~5h.

Citation Information

Patent Citations

  • Method for thermally processing a titanium alloy, and resulting part

    CN102317484A

  • Titanium alloy with high strength, high plasticity and good fracture toughness and preparing technology of titanium alloy

    CN107217173A

  • High-strength near-beta titanium alloy and smelting method thereof

    CN114045413A

  • High-strength plastic titanium alloy suitable for cold deformation processing and preparation method thereof

    CN114657417A

  • Near-beta titanium alloy heat treated casting

    US20070102073A1

Cited By

  • Low-density superelastic functional titanium alloy and preparation method thereof

    CN120400616A

  • A low-density super-elastic functional titanium alloy and a preparation method thereof

    CN120400616B

  • Heat treatment method for synergistically enhancing strength and plasticity of TB8 titanium alloy

    CN122382493A